Formaldehyde-free cold-pressing adhesive as well as preparation method and application thereof

Through the preparation of the preparative free cold pressing glue, the problems of low formaldehyde release and mechanical properties of wood adhesives are solved, and low formaldehyde release and high-strength glue are achieved. It is suitable for the preparation of artificial boards and magnesium oxychloride cement, reducing production costs and carbon emission.

CN118931423APending Publication Date: 2024-11-12GUANGDONG LIERAN CHEM GRP CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411226331.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-03
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Existing wood adhesives will release formaldehyde during production and use, resulting in excess of the formaldehyde content in indoor air, which will cause harm to human health. At the same time, the mechanical properties of formaldehyde-free adhesives are low, making it difficult to meet the needs of high-strength glue.

Method used

A dextrode-free cold pressing glue, which consists of water, cellulose, dihydrogen phosphate, retarder, additive and neutral silica sol, is prepared by specific proportioning and process steps for artificial boards and chlorine. The preparation of oxygen-magnesium cement avoids formaldehyde emission and improves the glue strength and water resistance.

Benefits of technology

It achieves low formaldehyde emission, reduces production costs, avoids the hot pressing process, improves the glue strength and water resistance, and meets the physical and mechanical properties requirements of Class II plywood in GB/T 9846-2015.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005024680340000061
    Figure BDA0005024680340000061
Patent Text Reader

Abstract

The invention relates to the technical field of adhesives, in particular to the field of IPC C09F, and more particularly relates to a formaldehyde-free cold-pressing adhesive as well as a preparation method and application thereof. The high-performance concrete is prepared from the following components in parts by weight: 1000 to 3000 parts of water, 50 to 100 parts of cellulose, 50 to 100 parts of dihydric phosphate, 10 to 50 parts of a retarder, 1000 to 3000 parts of an auxiliary agent, 50 to 100 parts of neutral silica sol and 100 to 300 parts of a modifier. According to the formaldehyde-free cold-pressing adhesive prepared by the invention, harmful substances such as formaldehyde and benzene are not added in the production process, only cold pressing is needed for producing a plate, a hot press is not needed for hot pressing, the cost is low, and the stability is good.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of adhesives, in particular to the field of IPC C09F, and more specifically to a formaldehyde-free cold-pressed adhesive and a preparation method and application thereof. Background Art

[0002] There are many types of wood adhesives, among which urea-formaldehyde resin glue, phenol-formaldehyde resin glue and melamine-formaldehyde resin glue are dominant, all of which release formaldehyde. Formaldehyde is released during the production and use of plywood; the release period of formaldehyde is as long as 3-15 years, and it is impossible to completely evaporate within 1-2 years after decoration, resulting in long-term excessive formaldehyde content in indoor air, which is harmful to human health. The characteristics of urea-formaldehyde glue determine that it can release free formaldehyde during the production process of the board, and simply reducing the formaldehyde content in the glue also reduces the bonding strength. Even if formaldehyde-free adhesives appear on the market, although there is no formaldehyde release, their mechanical properties are also limited.

[0003] CN 109575875 A discloses a biomass formaldehyde-free adhesive and its application in the preparation of formaldehyde-free aroma-releasing fiberboard. The biomass formaldehyde-free adhesive comprises the following raw materials and weight proportions: 100 parts of water, 20-30 parts of soy protein isolate, 10-30 parts of urea, 1-5 parts of sodium tripolyphosphate, 0.1-1 parts of methylcellulose, and 1-5 parts of mildew-proof agent. The invention also discloses a method for preparing the biomass formaldehyde-free adhesive. In the production of formaldehyde-free aroma-releasing fiberboard, in the process of adjusting and applying glue, the biomass formaldehyde-free adhesive, polymethylene polyphenyl isocyanate, and environmentally friendly slow-release fragrance are fully mixed and uniformly through a static mixer and then directly sprayed onto the fiber surface. The invention is used for floor substrates, which overcomes the disadvantages of ordinary fiberboards releasing formaldehyde and wood odor, but the mechanical properties are not high enough and need to be hot pressed. Summary of the invention

[0004] The first aspect of the present invention provides a formaldehyde-free cold-pressed adhesive, which comprises, by weight, 1000-3000 parts of water, 50-100 parts of cellulose, 50-100 parts of dihydrogen phosphate, 10-50 parts of retarder, 1000-3000 parts of additive, 50-100 parts of neutral silica sol, and 100-300 parts of modifier.

[0005] The dihydrogen phosphate includes at least one of ammonium dihydrogen phosphate, aluminum dihydrogen phosphate, potassium dihydrogen phosphate, and sodium dihydrogen phosphate.

[0006] The retarder includes at least one of sodium chloride and borax.

[0007] The modifier includes at least one of polyvinyl alcohol, carboxymethyl cellulose and polyacrylamide.

[0008] Preferably, the modifier comprises polyvinyl alcohol, and the average degree of polymerization (DP) of the polyvinyl alcohol is 2000-3000.

[0009] More preferably, the average degree of polymerization (DP) of the polyvinyl alcohol is 2400-2600.

[0010] The auxiliary agent includes at least one of a sodium salt aqueous solution and a magnesium salt aqueous solution.

[0011] A second aspect of the present invention provides a method for preparing a formaldehyde-free cold-pressed adhesive, comprising the following steps:

[0012] S1, add modifier and water and stir evenly;

[0013] S2, heating to 70-80°C, adding cellulose, dihydrogen phosphate and retarder to react;

[0014] S3, after cooling, add auxiliary agent and neutral silica sol to obtain.

[0015] The temperature of the reaction was 85-94°C.

[0016] Preferably, the reaction temperature is 88-94°C.

[0017] Further preferably, the reaction temperature is 88-92°C.

[0018] A third aspect of the present invention provides an application of a formaldehyde-free cold-pressed adhesive, wherein the formaldehyde-free cold-pressed adhesive is applied to the preparation of an adhesive for artificial boards or magnesium oxychloride and magnesium oxysulfate cement.

[0019] In parts by weight, the adhesive comprises 100 parts of formaldehyde-free cold-pressed adhesive, 40-60 parts of industrial mineral powder and 1-5 parts of curing agent.

[0020] Preferably, the industrial mineral powder comprises talc, dolomite and bentonite, and the weight ratio of the talc, dolomite and bentonite is 1:(0.8-1.2):(0.8-1.2).

[0021] Preferably, the industrial mineral powder comprises talc, dolomite and bentonite, and the weight ratio of the talc, dolomite and bentonite is 1:(0.8-1):(1-1.2).

[0022] The applicant has found that the industrial mineral powder includes talc, dolomite and bentonite, and the weight ratio of the talc, dolomite and bentonite is 1: (0.8-1.2): (0.8-1.2), which can reduce the amount of glue used and improve the bonding strength. It may be a specific industrial mineral powder that increases the lubrication performance between the glues, adjusts the shrinkage rate during the curing process, and reduces the difference in thermal expansion coefficient between the cold-pressed glue and the adherend, thereby improving the bonding strength. At the same time, it can also increase the viscosity of the glue, improve the thixotropy, control the fluidity of the glue, adjust the curing speed, and thus reduce the amount of industrial mineral powder added.

[0023] Preferably, the curing agent comprises phosphoric acid and silicic acid, and the weight ratio of the phosphoric acid to the silicic acid is 1:(0.8-1.2).

[0024] Preferably, the curing agent comprises phosphoric acid and silicic acid, and the weight ratio of the phosphoric acid to the silicic acid is 1:(0.8-1).

[0025] Beneficial effects:

[0026] 1. The formaldehyde-free cold-pressed adhesive prepared in this application does not add harmful solvents such as formaldehyde and benzene during the production process. It is used for bonding artificial boards, and the formaldehyde emission can be as low as 0.005 mg / m 3 .

[0027] 2. The formaldehyde-free cold-pressed adhesive prepared in the present application only needs cold pressing to produce boards, and does not require hot pressing by a hot press. It has low cost, good stability, and reduces carbon emissions and energy.

[0028] 3. The formaldehyde-free cold-pressed adhesive prepared in this application is used in artificial boards, and its physical and mechanical properties reach GB / T

[0029] Requirements for Class II plywood in 9846-2015.

[0030] 4. The reaction temperature is 85-94°C, which can improve the bonding strength (≥1MPa) and water resistance (Class I immersion peeling ≥5) of the board.

[0031] 5. The industrial mineral powder includes talc, dolomite and bentonite, and the weight ratio of the talc, dolomite and bentonite is 1:(0.8-1.2):(0.8-1.2), which can reduce the amount of glue used and improve the bonding strength.

[0032] 6. The formaldehyde-free cold-pressed adhesive is used in the preparation of artificial board adhesives or magnesium oxychloride and magnesium oxysulfate cement. DETAILED DESCRIPTION

[0033] Example 1

[0034] A formaldehyde-free cold-pressed adhesive comprises the following components, measured by weight: 1000 parts of water, 50 parts of cellulose (Jinzhou Fuqiang Fine Chemical), 50 parts of dihydrogen phosphate (ammonium dihydrogen phosphate), 10 parts of retarder (borax), 1000 parts of auxiliary agent (25wt% sodium sulfate aqueous solution), 50 parts of neutral silica sol (Guangdong Huierte Nano Technology Co., Ltd.), and 100 parts of modifier (polyvinyl alcohol, purchased from Anhui Wanwei, with an average degree of polymerization of 2400-2500).

[0035] A method for preparing formaldehyde-free cold-pressed adhesive comprises the following steps:

[0036] S1, add modifier and water and stir evenly;

[0037] S2, raise the temperature to 70°C, add cellulose, dihydrogen phosphate and retarder, and react at 90°C for 75 minutes;

[0038] S3, after cooling, add auxiliary agent and neutral silica sol to obtain.

[0039] The invention discloses an application of formaldehyde-free cold-pressed adhesive, wherein the formaldehyde-free cold-pressed adhesive is applied to the preparation of an adhesive for artificial boards. The adhesive comprises, by weight, 100 parts of formaldehyde-free cold-pressed adhesive, 50 parts of industrial mineral powder and 2.5 parts of a curing agent.

[0040] The industrial mineral powder is talcum powder, dolomite and bentonite, the weight ratio of the talcum powder, dolomite and bentonite is 1:1:1, and the particle size of the industrial mineral powder is 500 meshes.

[0041] The curing agent is phosphoric acid and silicic acid, and the weight ratio of the phosphoric acid to the silicic acid is 1:1.

[0042] Example 2

[0043] A formaldehyde-free cold-pressed adhesive comprises the following components, measured by weight: 1000 parts of water, 50 parts of cellulose (Jinzhou Fuqiang Fine Chemical), 50 parts of dihydrogen phosphate (ammonium dihydrogen phosphate), 10 parts of retarder (borax), 1000 parts of auxiliary agent (25wt% sodium sulfate aqueous solution), 50 parts of neutral silica sol (Guangdong Huierte Nano Technology Co., Ltd.), and 300 parts of modifier (polyvinyl alcohol, purchased from Anhui Wanwei, with an average degree of polymerization of 2400-2500).

[0044] A method for preparing formaldehyde-free cold-pressed adhesive comprises the following steps:

[0045] S1, add modifier and water and stir evenly;

[0046] S2, raise the temperature to 70°C, add cellulose, dihydrogen phosphate and retarder, and react at 90°C for 75 minutes;

[0047] S3, after cooling, add auxiliary agent and neutral silica sol to obtain.

[0048] The invention discloses an application of formaldehyde-free cold-pressed adhesive, wherein the formaldehyde-free cold-pressed adhesive is applied to the preparation of an adhesive for artificial boards. The adhesive comprises, by weight, 100 parts of formaldehyde-free cold-pressed adhesive, 50 parts of industrial mineral powder and 2.5 parts of a curing agent.

[0049] The industrial mineral powder is talcum powder, dolomite and bentonite, the weight ratio of the talcum powder, dolomite and bentonite is 1:1:1, and the particle size of the industrial mineral powder is 500 meshes.

[0050] The curing agent is phosphoric acid and silicic acid, and the weight ratio of the phosphoric acid to the silicic acid is 1:1.

[0051] Example 3

[0052] A formaldehyde-free cold-pressed adhesive comprises the following components, measured by weight: 2000 parts of water, 50 parts of cellulose (Jinzhou Fuqiang Fine Chemical), 50 parts of dihydrogen phosphate (ammonium dihydrogen phosphate), 10 parts of retarder (borax), 1000 parts of auxiliary agent (25wt% sodium sulfate aqueous solution), 50 parts of neutral silica sol (Guangdong Huierte Nano Technology Co., Ltd.), and 300 parts of modifier (polyvinyl alcohol, purchased from Anhui Wanwei, with an average degree of polymerization of 2400-2500).

[0053] A method for preparing formaldehyde-free cold-pressed adhesive comprises the following steps:

[0054] S1, add modifier and water and stir evenly;

[0055] S2, raise the temperature to 70°C, add cellulose, dihydrogen phosphate and retarder, and react at 90°C for 75 minutes;

[0056] S3, after cooling, add auxiliary agent and neutral silica sol to obtain.

[0057] The invention discloses an application of formaldehyde-free cold-pressed adhesive, wherein the formaldehyde-free cold-pressed adhesive is applied to the preparation of an adhesive for artificial boards. The adhesive comprises, by weight, 100 parts of formaldehyde-free cold-pressed adhesive, 50 parts of industrial mineral powder and 2.5 parts of a curing agent.

[0058] The industrial mineral powder is talcum powder, dolomite and bentonite, the weight ratio of the talcum powder, dolomite and bentonite is 1:1:1, and the particle size of the industrial mineral powder is 500 meshes.

[0059] The curing agent is phosphoric acid and silicic acid, and the weight ratio of the phosphoric acid to the silicic acid is 1:1.

[0060] Example 4

[0061] A formaldehyde-free cold-pressed adhesive comprises the following components, measured by weight: 3000 parts of water, 50 parts of cellulose (Jinzhou Fuqiang Fine Chemical), 50 parts of dihydrogen phosphate (ammonium dihydrogen phosphate), 10 parts of a retarder (borax), 1000 parts of an auxiliary agent (25wt% sodium sulfate aqueous solution), 50 parts of a neutral silica sol (Guangdong Huierte Nanotechnology Co., Ltd.), and 300 parts of a modifier (polyvinyl alcohol, purchased from Anhui Wanwei, with an average degree of polymerization of 2400-2500).

[0062] A method for preparing formaldehyde-free cold-pressed adhesive comprises the following steps:

[0063] S1, add modifier and water and stir evenly;

[0064] S2, raise the temperature to 70°C, add cellulose, dihydrogen phosphate and retarder, and react at 90°C for 75 minutes;

[0065] S3, after cooling, add auxiliary agent and neutral silica sol to obtain.

[0066] The invention discloses an application of formaldehyde-free cold-pressed adhesive, wherein the formaldehyde-free cold-pressed adhesive is applied to the preparation of an adhesive for artificial boards. The adhesive comprises, by weight, 100 parts of formaldehyde-free cold-pressed adhesive, 50 parts of industrial mineral powder and 2.5 parts of a curing agent.

[0067] The industrial mineral powder is talcum powder, dolomite and bentonite, the weight ratio of the talcum powder, dolomite and bentonite is 1:1:1, and the particle size of the industrial mineral powder is 500 meshes.

[0068] The curing agent is phosphoric acid and silicic acid, and the weight ratio of the phosphoric acid to the silicic acid is 1:1.

[0069] Comparative Example 1

[0070] A formaldehyde-free cold-pressed adhesive comprises the following components, measured by weight: 1000 parts of water, 50 parts of cellulose (Jinzhou Fuqiang Fine Chemical), 50 parts of dihydrogen phosphate (ammonium dihydrogen phosphate), 10 parts of retarder (borax), 1000 parts of auxiliary agent (25wt% sodium sulfate aqueous solution), 50 parts of neutral silica sol (Guangdong Huierte Nano Technology Co., Ltd.), and 100 parts of modifier (polyvinyl alcohol, purchased from Anhui Wanwei, with an average degree of polymerization of 2400-2500).

[0071] A method for preparing formaldehyde-free cold-pressed adhesive comprises the following steps:

[0072] S1, add modifier and water and stir evenly;

[0073] S2, raise the temperature to 65°C, add cellulose, dihydrogen phosphate and retarder, and react at 90°C for 75 minutes;

[0074] S3, after cooling, add auxiliary agent and neutral silica sol to obtain.

[0075] The invention discloses an application of formaldehyde-free cold-pressed adhesive, wherein the formaldehyde-free cold-pressed adhesive is applied to the preparation of an adhesive for artificial boards. The adhesive comprises, by weight, 100 parts of formaldehyde-free cold-pressed adhesive, 50 parts of industrial mineral powder and 2.5 parts of a curing agent.

[0076] The industrial mineral powder is talcum powder, dolomite and bentonite, the weight ratio of the talcum powder, dolomite and bentonite is 1:1:1, and the particle size of the industrial mineral powder is 500 meshes.

[0077] The curing agent is phosphoric acid and silicic acid, and the weight ratio of the phosphoric acid to the silicic acid is 1:1.

[0078] Comparative Example 2

[0079] A formaldehyde-free cold-pressed adhesive comprises the following components, measured by weight: 1000 parts of water, 50 parts of cellulose (Jinzhou Fuqiang Fine Chemical), 50 parts of dihydrogen phosphate (ammonium dihydrogen phosphate), 10 parts of retarder (borax), 1000 parts of auxiliary agent (25wt% sodium sulfate aqueous solution), 50 parts of neutral silica sol (Guangdong Huierte Nano Technology Co., Ltd.), and 100 parts of modifier (polyvinyl alcohol, purchased from Anhui Wanwei, with an average degree of polymerization of 2400-2500).

[0080] A method for preparing formaldehyde-free cold-pressed adhesive comprises the following steps:

[0081] S1, add modifier and water and stir evenly;

[0082] S2, raise the temperature to 70°C, add cellulose, dihydrogen phosphate and retarder, and react at 95°C for 75 minutes;

[0083] S3, after cooling, add auxiliary agent and neutral silica sol to obtain.

[0084] The invention discloses an application of formaldehyde-free cold-pressed adhesive, wherein the formaldehyde-free cold-pressed adhesive is applied to the preparation of an adhesive for artificial boards. The adhesive comprises, by weight, 100 parts of formaldehyde-free cold-pressed adhesive, 50 parts of industrial mineral powder and 2.5 parts of a curing agent.

[0085] The industrial mineral powder is talcum powder, dolomite and bentonite, the weight ratio of the talcum powder, dolomite and bentonite is 1:1:1, and the particle size of the industrial mineral powder is 500 meshes.

[0086] The curing agent is phosphoric acid and silicic acid, and the weight ratio of the phosphoric acid to the silicic acid is 1:1.

[0087] Performance testing methods and data

[0088] 1. GB / T 14074-2017 "Test methods for adhesives and resins for wood industry" The cold pressed adhesives of Examples 1 to 4 and Comparative Examples 1 to 2 were tested, and the quality indicators detected are shown in Table 1.

[0089] Table 1

[0090] Test items Example 1 Example 2 Example 3 Example 4 Comparative Example 1 Comparative Example 2 Solid content (%) 42.25 42.35 41.25 40.06 42.30 42.35 Viscosity(cps) 800 800 600 500 800 800 pH 5.3 5.4 5.5 5.3 5.4 5.5

[0091] 2. According to the bonding strength and formaldehyde emission determination method in GB / T 17657-2013 "Test methods for physical and chemical properties of artificial boards and veneer artificial boards" - climate chamber method, the adhesive for artificial boards in Examples 1 to 4 and Comparative Examples 1 to 2 was tested. 40×40×2mm eucalyptus veneer, five layers, layer by layer, double-sided glue 380g / m 2 After the lamination, the embryos were cold pressed in a cold press. The results are shown in Table 2.

[0092] Table 2

[0093]

Claims

1. A formaldehyde-free cold-pressed adhesive, characterized in that: Calculated by weight, the components include: 1000-3000 parts of water, 50-100 parts of cellulose, 50-100 parts of dihydrogen phosphate, 10-50 parts of retarder, 1000-3000 parts of additive, 50-100 parts of neutral silica sol, and 100-300 parts of modifier.

2. The formaldehyde-free cold-pressed adhesive according to claim 1, characterized in that: The dihydrogen phosphate includes at least one of ammonium dihydrogen phosphate, aluminum dihydrogen phosphate, potassium dihydrogen phosphate, and sodium dihydrogen phosphate.

3. The formaldehyde-free cold-pressed adhesive according to claim 2, characterized in that: The modifier includes at least one of polyvinyl alcohol, carboxymethyl cellulose and polyacrylamide.

4. The formaldehyde-free cold-pressed adhesive according to claim 3, characterized in that: The auxiliary agent includes at least one of a sodium salt aqueous solution and a magnesium salt aqueous solution.

5. A method for preparing the formaldehyde-free cold-pressed adhesive according to any one of claims 1 to 4, characterized in that: The following steps are involved: S1, add modifier and water and stir evenly; S2, heating to 70-80°C, adding cellulose, dihydrogen phosphate and retarder to react; S3, after cooling, add auxiliary agent and neutral silica sol to obtain.

6. The method for preparing the formaldehyde-free cold-pressed adhesive according to claim 5, characterized in that: The temperature of the reaction was 85-94°C.

7. An application of the formaldehyde-free cold-pressed adhesive according to any one of claims 1 to 4, characterized in that: The formaldehyde-free cold-pressed adhesive is used in the preparation of artificial board adhesive or magnesium oxychloride and magnesium oxysulfate cement.

8. The use of the formaldehyde-free cold-pressed adhesive according to claim 7, characterized in that: In parts by weight, the adhesive comprises 100 parts of formaldehyde-free cold-pressed adhesive, 40-60 parts of industrial mineral powder and 1-5 parts of curing agent.

9. The use of the formaldehyde-free cold-pressed adhesive according to claim 8, characterized in that: The industrial mineral powder comprises talc, dolomite and bentonite, and the weight ratio of the talc, dolomite and bentonite is 1: (0.8-1.2):(0.8-1.2)。 10. The use of the formaldehyde-free cold-pressed adhesive according to claim 7, characterized in that: The curing agent includes phosphoric acid and silicic acid, and the weight ratio of the phosphoric acid to the silicic acid is 1:(0.8-1.2).