Binder containing interpenetrating network, binder containing interpenetrating network and conductive network, and preparation and application thereof

By using interpenetrating network adhesives that build multiple hydrogen bonds and metal coordination bonds in lithium-ion batteries and introducing conductive additives, the poor conductivity and expansion problems of silicon-based anode materials are solved, and the cycle stability of lithium batteries is improved. Electrochemical properties.

CN118931431AActive Publication Date: 2024-11-12EAST CHINA UNIV OF SCI & TECH
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410999511.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-12
Estimated Expiration
2044-07-24

AI Technical Summary

Technical Problem

The silicon-based anode material has poor conductivity and is prone to expand in lithium-ion batteries, resulting in a decrease in battery capacity and service life. The existing adhesives cannot effectively suppress volume expansion and improve conductivity.

Method used

By constructing a multi-dynamic hydrogen bond interpenetrating network structure in the binder and introducing metal coordination bonds, conductive additives such as silver nanoparticles and silver nanowires are combined to form a conductive network, enhancing the mechanical properties and conductivity of the binder.

Benefits of technology

It significantly improves the cycle stability, rate performance and Coulomb efficiency of lithium batteries, reduces the expansion stress of active substances, forms a dense SEI layer, and improves electrochemical performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118931431A_ABST
    Figure CN118931431A_ABST
Patent Text Reader

Abstract

The invention relates to a binder containing an interpenetrating network, a binder containing an interpenetrating network and a conductive network as well as preparation and application. The binder comprises polyvinyl alcohol, waterborne polyurethane and water which are obtained by physical mixing, or polyvinyl alcohol, waterborne polyurethane, an additive and water which are obtained by physical mixing, wherein the additive is a conductive additive or a metal coordination agent, and the conductive additive is selected from at least one of silver nanoparticles or silver nanowires; the metal coordination agent is selected from Al < 3 + >. Compared with the prior art, by compounding the polyvinyl alcohol and the waterborne polyurethane in different proportions, mutual embedding between molecular chains is achieved, the interpenetrating network binder with multiple hydrogen-bond interaction is formed, the binder can generate strong Van der Waals force interaction with the surface of a silicon-carbon material, and the surface of the silicon-carbon material can be bonded with the surface of the silicon-carbon material. The adhesion effect between the current collector and the active substance is enhanced, the volume expansion phenomenon of silicon in the active substance is effectively inhibited, and the integrity of the electrode structure is ensured, so that the electrochemical stability in the cycle process is maintained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of lithium batteries, and relates to a binder containing an interpenetrating network, a binder containing an interpenetrating network and a conductive network, and the preparation and application of the binder in a silicon-carbon negative electrode lithium battery. Background Art

[0002] Silicon is considered to be one of the most promising negative electrode materials for lithium-ion batteries due to its high theoretical specific capacity, low voltage platform and abundant reserves. However, silicon materials have poor electrical conductivity and are prone to volume expansion during the charge and discharge process, resulting in pulverization of their own structure, which seriously reduces the battery capacity and service life, hindering its commercialization process. Binders, as additives to silicon-based negative electrodes, can effectively inhibit the volume expansion of silicon materials and improve the conductivity of the electrode. The theoretical specific capacity of silicon-carbon materials depends on the addition ratio of silicon to carbon materials. The higher the addition ratio, the higher the theoretical specific capacity of the composite negative electrode, but the worse its cycle stability. Therefore, studying how to increase the addition ratio of silicon in silicon-carbon materials while ensuring long-cycle stability and the process of application in high-power electrical appliances has broad research value.

[0003] At present, most common commercial binders are PVDF binders. PVDF binders have good electrochemical stability, but their conductivity is poor, and they lack flexible structures and polar groups that can anchor to the surface of silicon materials. Therefore, they are not suitable for silicon-based negative electrodes that are prone to volume expansion and have poor conductivity. Although linear binders such as CMC, PAA, and PVA can produce hydrogen bonds with the hydroxyl groups on the surface of silicon particles through the polar groups contained in the structure, the van der Waals force is weak. After a long period of charge and discharge cycles, silicon-based negative electrodes will still face the problem of breakage and pulverization. Therefore, it is crucial to modify the basic binder and construct a three-dimensional network structure. The interpenetrating network is conducive to giving the silicon-based negative electrode sufficient mechanical strength to withstand greater expansion stress. The conductive network binder helps to achieve high-performance electrodes because it can achieve the mechanical and electronic integrity of the electrode.

[0004] Interpenetrating networks provide strong chemical interactions between binder chains. For example, highly calcium-crosslinked alginate hydrogels and some hybrid networks prepared by diffusion methods have been proposed as novel binders for Si-based and Si-based anodes. Other strategies for preparing self-healing polymers through supramolecular interactions have also been adopted for Si binders. These interpenetrating network designs have significantly improved the electrochemical performance of Si. Wang et al. proposed an interpenetrating PAA-PVA highly absorbent gel binder for Si anode, which can effectively alleviate the huge volume expansion during cycling due to the strong adhesion of the convertible network. Despite the significant improvement in electrochemical performance, the conductivity of the gel polymer binder is still limited by the insulating polymer chains, which may greatly hinder the transport of electrons. Summary of the invention

[0005] The purpose of the present invention is to provide a method for preparing a binder containing an interpenetrating and conductive network and its application in a silicon-carbon negative electrode lithium battery, so as to improve the cycle stability, rate performance and / or coulombic efficiency of the lithium battery.

[0006] The purpose of the present invention can be achieved by the following technical solutions:

[0007] Currently, PEDOT:PSS is used as a conductive binder, which significantly inhibits the dissolution of the material and enhances the conductivity through non-covalent electrostatic interactions with the S atoms in DTT. However, due to the structural diversity of organic materials, the applicability of PEDOT:PSS to other organic electrodes is unclear. Therefore, the combination of conductive additives with new binders demonstrates a feasible method to achieve both high conductivity and strong binding interactions, which helps to improve the achievable capacity and cycle stability of the electrode.

[0008] The present invention constructs an interpenetrating network structure binder with multiple dynamic hydrogen bonds through PVA and waterborne polyurethane (WPU), and introduces metal coordination bonds (metal ions) to strengthen the interpenetrating network effect, significantly enhances the mechanical properties (peeling properties) of the binder system, and improves the adhesion between the current collector and the active material, effectively inhibits the volume expansion phenomenon of silicon in the active material, ensures the integrity of the electrode structure, and improves the utilization rate and first effect of the active material. And by introducing conductive additives (silver nanoparticles and silver nanowires) into the binder system, a conductive network is constructed to improve the long cycle performance and first coulomb efficiency of the silicon-carbon negative electrode, thereby improving the overall electrochemical performance of the battery.

[0009] The first aspect of the present invention provides an interpenetrating network-containing adhesive, comprising physically mixed polyvinyl alcohol, waterborne polyurethane and water, wherein the mass ratio of the polyvinyl alcohol to the waterborne polyurethane is (1-9):1.

[0010] The total content of the polyvinyl alcohol and waterborne polyurethane in the binder is 15-25wt%.

[0011] The second aspect of the present invention provides a method for preparing an interpenetrating network-containing adhesive, comprising: stirring and mixing polyvinyl alcohol, waterborne polyurethane and water.

[0012] The third aspect of the present invention provides an adhesive containing an interpenetrating network and a conductive network, comprising physically mixed polyvinyl alcohol, waterborne polyurethane, additives and water,

[0013] The mass ratio of polyvinyl alcohol to waterborne polyurethane is (1-9):1;

[0014] The additive is a conductive additive or a metal ligand, the conductive additive is selected from at least one of silver nanoparticles or silver nanowires, and the metal ligand is selected from Al 3+ .

[0015] Furthermore, the amount of the silver nanoparticles is 1-2 mg / 5 g polyvinyl alcohol + aqueous polyurethane, and the amount of the silver nanowires is 1-2.5 mg / 5 g polyvinyl alcohol + aqueous polyurethane;

[0016] The metal coordination agent is selected from Al 3+ The dosage is 1-2mmol / 1.5g water-based polyurethane.

[0017] The fourth aspect of the present invention provides a method for preparing an adhesive containing an interpenetrating network and a conductive network, comprising: stirring and mixing polyvinyl alcohol, waterborne polyurethane and water, and then adding additives to prepare the adhesive.

[0018] Furthermore, the preparation method of the waterborne polyurethane comprises:

[0019] Polyethylene glycol, dimethylol propionic acid, isophorone diisocyanate and dibutyltin dilaurate are mixed and reacted, and then 2-hydroxyethyl methacrylate is added and stirred to react to obtain a polyurethane prepolymer;

[0020] Add triethylamine to carry out neutralization reaction;

[0021] Add water to emulsify the reaction;

[0022] Ethylene diamine is added to carry out emulsion polymerization to obtain waterborne polyurethane.

[0023] Furthermore, the feed ratio of polyethylene glycol, dimethylol propionic acid, isophorone diisocyanate, dibutyltin dilaurate, and 2-hydroxyethyl methacrylate is (20-30) g: (2-3) g: (9-13.5) g: (42-63) μL: (1-3) mL;

[0024] The mixed reaction comprises: firstly reacting polyethylene glycol and dimethylol propionic acid at 85-90° C. for 1-1.5 hours; then adding isophorone diisocyanate and dibutyltin dilaurate and reacting at 80-85° C. for 2-2.5 hours;

[0025] In the stirring reaction, the reaction temperature is 80-85° C. and the reaction time is 1-1.5 h.

[0026] Furthermore, in the neutralization reaction, the amount of triethylamine added is (2-3) mL / mL 2-hydroxyethyl methacrylate; the reaction temperature is 40-45° C., and the reaction time is 0.5-1 h.

[0027] Furthermore, the amount of water added is (65-70) mL / mL 2-hydroxyethyl methacrylate; the reaction temperature is 85-90° C., and the reaction time is 0.25-0.3 h.

[0028] Furthermore, in the emulsion polymerization reaction, the amount of ethylenediamine added is 8-9 μL / μL dibutyltin dilaurate; the reaction temperature is 85-90° C., and the reaction time is 3-4 hours.

[0029] The fifth aspect of the present invention provides an application of a binder, including using the above binder for preparing a lithium battery; more specifically, using the above binder for preparing a negative electrode material, and then for preparing a lithium battery.

[0030] Furthermore, the negative electrode material is a silicon-carbon negative electrode material.

[0031] Furthermore, the positive electrode material of the lithium battery is lithium iron phosphate.

[0032] The present invention realizes mutual interlocking between molecular chains by compounding polyvinyl alcohol (PVA) and waterborne polyurethane (WPU) in different proportions to form an interpenetrating network binder (PVA-WPU) with multiple hydrogen bonds. The binder can generate strong van der Waals forces with the surface of silicon-carbon materials, enhance the adhesion between the current collector and the active material, effectively inhibit the volume expansion of silicon in the active material, ensure the integrity of the electrode structure, and thus maintain the electrochemical stability during the cycle. Further introduction of metal Al 3+ , PVA-Al 3+ -WPU binder, at this time the system forms a synergistic effect of multiple hydrogen bonds and metal coordination bonds, which strengthens the role of the interpenetrating network, and thus can significantly enhance the mechanical properties of the binder system, and improve the adhesion between the current collector and the active material, thereby improving the utilization rate and initial effect of the active material. However, due to the weak conductivity of silicon materials, excellent performance binders not only need to provide sufficient mechanical strength for the active material, but also should focus on improving its conductive properties. Therefore, by introducing conductive additives into the binder system, that is, introducing Ag nanoparticles and Ag nanowires, a PVA-Ag-WPU binder is prepared, which can significantly improve the Li + The silicon-carbon negative electrode made of this binder can more easily form a dense and stable SEI layer, reduce the occurrence of side reactions, and thus improve the overall electrochemical performance of the battery.

[0033] Compared with the prior art, the present invention has the following characteristics:

[0034] 1) The present invention forms an interpenetrating network binder (PVA-WPU) with multiple hydrogen bonds by physically blending WPU and PVA in different proportions. PVA-WPU enhances the interaction between the binder and the surface of the silicon-carbon material, while enhancing the adhesion between the current collector and the active material, effectively inhibiting the volume expansion of silicon in the active material, and improving the first effect and reversible capacity of the silicon-carbon negative electrode battery.

[0035] 2) Based on the optimal ratio of PVA-WPU binder, the present invention introduces metal coordination bonds (metal aluminum ions) with strong bonding force to strengthen the role of the interpenetrating network, thereby improving the mechanical properties and bonding properties of the binder system to obtain PVA-Al 3+ -WPU binder; by introducing conductive additives (silver nanoparticles and silver nanowires) with good dispersibility, the electrochemical performance of the silicon-carbon negative electrode is improved to obtain PVA-Ag-WPU binder.

[0036] 3) PVA-Ag-WPU and PVA-Al prepared by the present invention 3+ -WPU binder, through the synergistic effect of interpenetrating network and conductive network, not only effectively reduces the expansion stress of active materials during charging and discharging, but also forms a denser and thinner SEI film, constructs a new lithium ion transmission channel, and improves the transmission speed of Li+ in the battery, thereby improving the electrochemical reaction efficiency and the utilization rate of active materials.

[0037] 4) Metal coordination bond PVA-Al prepared by the present invention 3+ -WPU binder and conductive additive PVA-Ag-WPU binder are assembled into lithium-ion half-cells, which significantly improves the capacity retention rate and the first cycle coulombic efficiency. 3+ -The capacity retention rate of WPU binder increased from 70.90% to 82.15%, and the first-cycle coulomb efficiency increased from 80.96% to 85.24%;

[0038] 5) Chinese patent application CN118006253A discloses a composite binder, a negative electrode and a secondary battery, wherein the composite binder includes carboxymethyl chitosan, an auxiliary binder and polyvinyl alcohol; the auxiliary binder includes at least one of methyl hydroxypropyl cellulose, hydroxypropyl cellulose, polyurethane, polyanionic cellulose ether, hydroxypropyl starch ether and hydroxyethyl cellulose ether. The role of carboxymethyl chitosan in the above technical scheme is to improve the dispersibility and adhesion of the slurry, solve the problem of cracking and falling off during coating, have slurry moisture retention during coating, solve the problem of low peeling strength of the pole piece and severe powder falling off at the edges after winding, and improve the flexibility of the negative pole piece. However, the PVA-WPU-73 slurry in the present invention will not have the problem of cracking and falling off during coating, and will not have the problem of powder falling off after drying. Fig.11,It can also be seen that the swelling rate of PVA-WPU-73 is low and the peel strength is high, and the addition of carboxymethyl chitosan is unnecessary;

[0039] 6) The theoretical capacity of graphite negative electrode material is 372mAh / g, but the actual specific capacity is 330-370mAh / g. During the charge and discharge process, it is easy to react with the electrolyte to form an SEI film, which makes the initial coulomb efficiency of the lithium-ion battery low; in addition, the graphite negative electrode has poor compatibility with the electrolyte and is easily co-embedded with the organic solvent in the electrolyte, which will cause the negative electrode graphite layer to expand and peel off, thereby reducing the cycle stability of the lithium-ion battery. The theoretical capacity of the silicon-carbon negative electrode selected in the present invention can reach 400-800mAh / g. The silicon-carbon negative electrode material combines the advantages of silicon and carbon materials. It has both the high theoretical specific capacity of silicon and the good conductivity and cycle stability of carbon. Compared with the graphite negative electrode, it is more meaningful to study. The improvement effect of the binder on the silicon-carbon negative electrode will be more meaningful than that of the graphite negative electrode. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] Figure 1 FTIR spectra of WPU and PVA-WPU binders prepared in Example 1; (a) WPU; (b) PVA-WPU binders with different mass ratios;

[0041] Figure 2 is a particle size distribution diagram of the WPU emulsion prepared in Example 1;

[0042] Figure 3 is the XRD pattern of SiC650;

[0043] Figure 4 SEM images of the silicon-carbon negative electrode SiC650 / PVA-WPU-73 prepared in Example 1; (a) high-resolution and (b) low-resolution original morphology characterizations; (c) Si and (d) C element distribution diagrams in the electrode piece;

[0044] Figure 5 XPS spectra of the silicon-carbon negative electrode corresponding to the PVA-WPU-73 binder prepared in Example 1 after 100 cycles; (a) C1s and (b) F1s spectrum comparison;

[0045] Figure 6 CV curve of the silicon-carbon negative electrode SiC650 / PVA-WPU-73 prepared in Example 1;

[0046] Figure 7The impedance comparison diagram of the silicon-carbon negative electrode SiC650 / PVA-WPU prepared in Example 1 after 100 cycles; (a) Impedance comparison of the silicon-carbon negative electrode corresponding to the PVA-WPU type binder after 100 cycles; (b) Schematic diagram of the high-frequency region of the impedance curve of the PVA-WPU type binder;

[0047] Figure 8 This is a comparison chart of the long cycle performance of the silicon-carbon negative electrodes SiC650 / PVA-WPU, SiC650 / PVA, and SiC650 / WPU prepared in Example 1;

[0048] Fig. 9 This is a comparison chart of the rate performance of the silicon-carbon negative electrode SiC650 / PVA-WPU prepared in Example 1;

[0049] Fig.10 This is a comparison chart of the coulombic efficiency of the silicon-carbon negative electrodes SiC650 / PVA-WPU, SiC650 / PVA, and SiC650 / WPU prepared in Example 1;

[0050] Fig.11 Comparison of (a) swelling ratio and (b) average peeling force of different adhesives in Example 1;

[0051] Fig.12 The silicon-carbon negative electrode SiC650 / PVA-Ag-WPU (a) prepared in Example 2; SiC650 / PVA-Al 3+ -SEM image of WPU (b);

[0052] Fig.13 The WPU (a) and PVA-WPU-73, PVA-Ag-WPU, and PVA-Al prepared in Example 2 3+ - FTIR spectrum of WPU binder (b);

[0053] Fig.14 The PVA-Ag-WPU and PVA-Al prepared in Example 2 3+ -XPS spectra of the silicon-carbon anode corresponding to the WPU binder after 100 cycles; (ab) C1s and (cd) F1s spectra comparison;

[0054] Fig.15 The silicon-carbon negative electrode SiC650 / PVA-Ag-WPU (a) prepared in Example 2; SiC650 / PVA-Al 3+ -CV curve of WPU (b);

[0055] Fig.16The silicon-carbon negative electrode SiC650 / PVA-WPU-73, SiC650 / PVA-Ag-WPU, SiC650 / PVA-Al prepared in Example 2 3+ - Impedance comparison chart of WPU after 100 cycles;

[0056] Fig.17 The silicon-carbon negative electrode SiC650 / PVA-WPU-73, SiC650 / PVA-Ag-WPU, SiC650 / PVA-Al prepared in Example 2 3+ -Comparison chart of long cycle capacity of WPU;

[0057] Fig.18 The silicon-carbon negative electrode SiC650 / PVA-WPU-73, SiC650 / PVA-Ag-WPU, SiC650 / PVA-Al prepared in Example 2 3+ -WPU rate performance comparison chart;

[0058] Fig.19 The silicon-carbon negative electrode SiC650 / PVA-WPU-73, SiC650 / PVA-Ag-WPU, SiC650 / PVA-Al prepared in Example 2 3+ - Comparison of Coulombic efficiency of WPU;

[0059] Fig. 20 XRD patterns of SiC650 and SiC950;

[0060] Fig.21 The silicon-carbon negative electrode SiC950 / PVA-WPU-73, SiC950 / PVA-Ag-WPU; SiC950 / PVA-Al 3+ -SEM images of WPU before and after cycling at 1C current density;

[0061] Fig. 22 The silicon-carbon negative electrode SiC950 / PVA-Al prepared in Example 3 3+ -CV curve of WPU;

[0062] Fig.23 The silicon-carbon negative electrode SiC950 / PVA-WPU-73, SiC950 / PVA-Ag-WPU; SiC950 / PVA-Al 3+ -Comparison chart of long cycle capacity of WPU;

[0063] Fig.24The silicon-carbon negative electrode SiC950 / PVA-WPU-73, SiC950 / PVA-Ag-WPU; SiC950 / PVA-Al 3+ -WPU rate performance comparison chart;

[0064] Fig.25 The silicon-carbon negative electrode SiC950 / PVA-WPU-73, SiC950 / PVA-Ag-WPU; SiC950 / PVA-Al 3+ - Coulomb efficiency comparison of WPU;

[0065] Fig.26 PVA-Al 3+ -WPU, PVA-Fe 3+ -WPU, PVA-Zn 2+ -WPU, PVA-Ni 2+ -Optical photograph of WPU binder. DETAILED DESCRIPTION

[0066] The present invention is described in detail below in conjunction with the accompanying drawings and specific embodiments. This embodiment is implemented based on the technical solution of the present invention, and provides a detailed implementation method and specific operation process, but the protection scope of the present invention is not limited to the following embodiments.

[0067] The silicon-carbon active material used in the following examples is SiC650 (theoretical specific capacity is 650 mAh·g -1 ) and SiC950 (theoretical specific capacity is 950mAh g -1 ). The required drugs are: polyethylene glycol 2000 (PEG 2000), dimethylolpropionic acid (DMPA), N,N-dimethylformamide (DMF), isophorone diisocyanate (IPDI), dibutyltin dilaurate (DBTDL), 2-hydroxyethyl methacrylate (HEMA), triethylamine (TEA), dimethyl sulfoxide, ethylenediamine, polyvinyl alcohol (PVA), nanosilver (nanoparticles and / or nanosilver wires) solution, aluminum chloride, lithium hexafluorophosphate, ethylene carbonate (EC), diethyl carbonate (DEC), dimethyl carbonate (DMC), fluoroethylene carbonate (FEC), lithium iron phosphate (LiFePO4), Super P, polyvinylidene fluoride (PVDF), N-methylpyrrolidone (NMP), and ultrapure water.

[0068]

[0069] 1. Synthesis of waterborne polyurethane WPU:

[0070] Take PEG 2000 and add it to a three-necked flask, maintain a vacuum environment, and stir for a certain period of time under oil bath heating conditions. Subsequently, the chain extender DMPA is dissolved in DMF and reacted for several hours. Under a nitrogen-protected atmosphere, IPDI and DBTDL are added to the flask, and the reaction is continued for a period of time. Continue to add HEMA to obtain a transparent polyurethane prepolymer. Add TEA to the flask for neutralization reaction. Add ultrapure water to the flask for rapid emulsification reaction. After the reaction is completed, add ethylenediamine solution to the mixed emulsion, and perform emulsion polymerization for several hours to obtain the final product WPU emulsion. During the process, all drugs are added dropwise into the flask using a syringe to reduce the impact of moisture and oxygen in the air on the reaction atmosphere.

[0071] 2. Preparation of interpenetrating network adhesive PVA-WPU:

[0072] Take a certain amount of PVA gel and WPU emulsion, mix them, add ultrapure water as solvent, stir at a constant speed for a certain time at room temperature to obtain a uniform PVA-WPU adhesive solution. By changing the added mass of PVA gel and WPU emulsion, interpenetrating network adhesives with composite mass ratios of PVA and WPU of 5:5, 6:4, 7:3, 8:2, and 9:1 were obtained.

[0073] 3. Preparation of conductive network adhesive:

[0074] Preparation of PVA-Ag-WPU adhesive: Take a certain amount of PVA gel and WPU emulsion, mix the two, add ultrapure water as a solvent, stir at a constant speed for a certain time at room temperature to obtain a uniform and stable milky white adhesive solution, continue to add nanosilver solution (silver nanoparticles and silver nanowires), stir at a constant speed for a certain time at room temperature to ensure that the Ag nanoparticles are evenly dispersed, and obtain a uniform PVA-Ag-WPU adhesive.

[0075] PVA-Al 3+ -WPU binder: The preparation method is basically the same as the above-mentioned PVA-Ag-WPU binder. After obtaining a uniform milky white binder solution, continue to add AlCl3 solution and stir at a constant speed for a certain period of time at room temperature to obtain a uniform PVA-Al 3 + -WPU binder.

[0076] 3. Preparation of silicon-carbon negative electrode:

[0077] SiC650, Super P, and PVA-WPU were mixed and ground in a mass ratio of 80:10:10, and then the mixture was dispersed in NMP and stirred overnight. After the slurry was coated on aluminum foil, the obtained pole piece was dried to remove the solvent.

[0078] 4. Preparation of lithium iron phosphate (LiFePO4) positive electrode:

[0079] LiFePO4, Super P, and PVDF were mixed and ground in a mass ratio of 80:10:10. The mixture was then dispersed in NMP and stirred overnight. After the slurry was coated on aluminum foil, the prepared pole piece was dried to remove the solvent.

[0080] 5. Performance testing and battery assembly

[0081] The structures of WPU, PVA and composite binder were analyzed using Fourier transform infrared spectrometer (FTIR).

[0082] The particle size of WPU was analyzed using a dynamic light scattering (DLS) particle size analyzer.

[0083] X-ray diffraction analysis (XRD) was used to characterize the crystal form and purity of SiC650 and SiC950.

[0084] Scanning electron microscopy (SEM) was used to characterize the microstructure of SiC650 and SiC950, as well as the microstructure and elemental analysis of silicon-carbon negative electrode sheets made with different binders.

[0085] X-ray photoelectron spectroscopy (XPS) was used to compare the compound content of electrodes with different adhesives after cycling.

[0086] Cyclic voltammetry (CV) was used to perform multiple scans at different electrode potential speeds in the voltage range of 0.01-3 V at a rate of 0.1 mV·s -1 At a slow scanning speed, CV tests were performed on half-cells made with different binders to analyze the changes in the redox reactions corresponding to different batteries.

[0087] The test frequency range is 10 -2 -10 5 A disturbance voltage of 5 mV was applied in the scanning interval, and EIS tests were performed on half-cells made with different binders before and after cycling to analyze the changes in battery impedance caused by long cycling.

[0088] The cycling performance of the binder was studied by constant current charge and discharge tests. The voltage test range of the half-cell was 0.01-2V, and the long cycle test was performed at a current density of 1C; the voltage test range of the full cell was 2.5-3.9V, and the long cycle test was performed at a current density of 0.5C.

[0089] The charge and discharge tests were used to study the rate performance, cycle life, discharge capacity and coulombic efficiency of the binder. The voltage test range of the half-cell was 0.01-2V, and the voltage test range of the full-cell was 2.5-3.9V.

[0090] The mechanical properties of the adhesive were determined by characterizing the swelling performance and performing a 180° peel test on the pole pieces corresponding to different adhesives.

[0091] Swelling performance test:

[0092]

[0093] The initial mass of the adhesive film is recorded as m1. After being immersed in the electrolyte for 48 hours, it is taken out and the surface solvent is wiped off and weighed again. The mass is recorded as m2. The corresponding swelling rate can be calculated according to the above formula;

[0094] 180° peel test: Use a universal material tester to test the peeling performance. The adhesive material is cut into 2.5cm×15cm samples. Then, the sample is peeled off from the flexible or rigid substrate at an angle of 180°, and the peeling speed is 300mm / min.

[0095] Example 1

[0096] Preparation of WPU: Take 20g PEG 2000 and add it to a three-necked flask, maintain a vacuum environment, and stir for 2h under oil bath heating conditions at 110℃. Subsequently, 2g of chain extender DMPA was dissolved in DMF and added to the flask, and reacted at 85℃ for 1h. Under a nitrogen-protected atmosphere, 9g IPDI and 42μL DBTDL were added to the flask, and the reaction was continued at 80℃ for 2h. Continue to add 1mL HEMA and stir for 1h to obtain a transparent polyurethane prepolymer. Add 2mL TEA to the flask and neutralize it at 40℃ for 0.5h. Add 65mL ultrapure water to the flask and perform a rapid emulsification reaction at 85℃ for 15min. After the reaction is completed, add 350μL ethylenediamine to the mixed emulsion, and perform an emulsion polymerization reaction at 85℃ for 3h to obtain the final product WPU emulsion. During the process, all drugs are added drop by drop into the flask using a syringe to reduce the impact of moisture and oxygen in the air on the reaction atmosphere.

[0097] Preparation of PVA-WPU binder: Taking PVA-WPU-7:3 binder as an example (7:3 is the mass ratio of PVA to WPU), take 3.5g PVA gel and WPU emulsion (containing 1.5g WPU), mix the two, add 2mL ultrapure water as solvent, stir at a constant speed for 12h at room temperature to obtain a uniform PVA-WPU-7:3 binder solution. The binder formulas of the other four mass ratios (9:1, 8:2, 6:4, 5:5, the total mass of PVA+WPU is 5g) only need to change the added mass of PVA gel and WPU emulsion. At the same time, set pure PVA and pure WPU as control groups.

[0098] Preparation of silicon-carbon negative electrode: SiC650, Super P, and PVA-WPU were mixed and ground in a mass ratio of 80:10:10. The mixture was then dispersed in NMP and stirred overnight. The slurry was coated on aluminum foil and dried to remove the solvent to obtain a silicon-carbon negative electrode.

[0099] Preparation of lithium iron phosphate (LiFePO4) positive electrode: LiFePO4, Super P, and PVDF are mixed and ground in a mass ratio of 80:10:10. The mixture is then dispersed in NMP and stirred overnight. The slurry is coated on aluminum foil and dried to remove the solvent to obtain a lithium iron phosphate positive electrode sheet.

[0100] Performance testing and battery assembly:

[0101] A 2025 button cell shell was selected for battery assembly, and the entire process was carried out in a glove box (H2O, O2 < 0.01 ppm).

[0102] The silicon-carbon anode with a radius of 9 mm is used as the positive electrode in the half-cell, Celgaed 2400 polypropylene is used as the diaphragm, and the pure lithium sheet with a radius of 11 mm is used as the negative electrode. The electrolyte preparation process selected is that LiPF6 with a final concentration of 1.0M is dissolved in a mixed solution of EC, DEC, and DMC with a volume ratio of 1:1:1, and 5wt% FEC is added as an electrolyte additive. The assembly process is carried out in the order of positive electrode shell, silicon-carbon anode, diaphragm, electrolyte, lithium sheet, gasket, spring sheet, and negative electrode shell, and ensure that the components between the positive electrode shell and the negative electrode shell are placed in the center.

[0103] Figure 1 The FTIR spectra of PVA-WPU binders with different ratios are shown in Figure 2. In the FTIR spectra of PVA binders, at 3360 cm -1 The stretching vibration peak corresponding to the hydroxyl group appears at 1725cm, and in the PVA-WPU composite binder, the absorption peak shifts to the right. -1The intensity of the characteristic peak of carboxylic acid formate at 650-800cm is significantly weakened, which indicates that hydrogen bonding is formed between the hydroxyl groups in PVA and the carboxylic acid formate and carboxyl groups in WPU, thus changing the absorption peak position and intensity. -1 The corresponding primary amino characteristic peak shows a sign of obvious weakening, which is also due to the formation of hydrogen bonds between the hydroxyl groups in PVA and the amino groups in WPU. The test fully proves the successful synthesis of WPU and the formation of hydrogen bonds between PVA and WPU, which gives the binder better mechanical properties and can generate strong forces with the surface of the silicon-carbon negative electrode.

[0104] Figure 2 This is the particle size distribution diagram in the WPU emulsion, which reflects that the particle size distribution uniformity between the particles in the emulsion is good, which is conducive to the subsequent uniform distribution in the composite adhesive.

[0105] Figure 3 This is the XRD spectrum of SiC650. No other impurity peaks were found, indicating that the material has a high purity and is not prone to side reactions during the charge and discharge process, thereby improving the electrochemical stability of the silicon-carbon negative electrode.

[0106] Figure 4 SEM images of SiC650 / PVA-WPU-73, (a) high resolution, (b) low resolution original morphology characterization; (c) Si, (d) C element distribution diagram in the electrode. Figures a and b show that the surface of the electrode is relatively flat. At low resolution (20 μm), there are some pores on the surface of the electrode, which is conducive to the electrode being fully infiltrated by the electrolyte and promotes Li during the charge and discharge process. + Transmission; Figures c and d show that the Si and C elements in the electrode are evenly distributed without agglomeration.

[0107] Figure 5 This is the XPS spectrum of the silicon-carbon negative electrode corresponding to the PVA-WPU binder after 100 cycles, indicating that the higher the LiF component content, the tighter the SEI layer structure formed and the more stable the properties.

[0108] Figure 6 This is the CV curve of SiC650 / PVA-WPU-73. There are no mixed peaks, indicating that the redox reaction inside the electrode is highly reversible, without interference from side reactions, and has excellent electrochemical stability during the charge and discharge process.

[0109] Figure 7 The impedance comparison of the silicon-carbon negative electrode corresponding to the PVA-WPU type binder after 100 cycles shows that the Li + The diffusion speed is better than other silicon-carbon negative electrodes, which is conducive to the formation of a denser and thinner SEI layer and improves the electrochemical performance.

[0110] Figure 8 The long cycle performance of silicon-carbon negative electrode corresponding to different binders is compared. The capacity retention rate of the corresponding silicon-carbon negative electrode varies greatly with the different WPU introduction ratios. After 500 cycles, the corresponding capacity retention rates are 43.75%, 57.21%, 70.90%, 60.28% and 61.35%. Among them, SiC650 / PVA-WPU-73 has the highest capacity retention rate, and the highest specific capacity after activation is 503.8mAh·g -1 The discharge capacity corresponding to 500 cycles is 357.2 mAh g -1 .

[0111] Fig. 9 The performance comparison of silicon-carbon anode corresponding to PVA-WPU type binder is shown in Figure 2. At the rates of 0.1C, 0.2C, 0.3C, 0.5C, 1C, and 3C, the discharge specific capacities of lithium batteries assembled with different binder ratios at a current density of 0.1C are 536.1 mAh g -1 、563.4mAh·g -1 、613.9mAh·g -1 、579.7mAh·g -1 and 541.2mAh·g -1 As the current density gradually increases, the discharge specific capacity gradually decreases, but in this process, the discharge specific capacity of the silicon-carbon negative electrode corresponding to the PVA-WPU-73 binder is always greater than that of other silicon-carbon negative electrodes.

[0112] Fig.10 The coulombic efficiency of silicon-carbon negative electrode corresponding to different binders is compared. After 5 cycles of activation, the CE of the silicon-carbon negative electrode corresponding to the composite binder remains above 98%. The uniform and dense SEI film formed after activation effectively reduces the irreversible loss of capacity during the charge and discharge process and improves the capacity retention rate. In particular, SiC650 / PVA-WPU-73 performs best with an ICE of 80.96%.

[0113] Fig.11Comparison of swelling rate and average peeling force of different binders. PVA-WPU-73 binder has the lowest swelling rate, which can not only ensure the interaction with the electrolyte, but also effectively avoid affecting the properties of its own binder, thereby maintaining sufficient electrical contact between the active material and the current collector, and maintaining the cycle stability of the silicon-carbon negative electrode. Compared with the composite PVA-WPU binder, the average peeling force of the pole pieces prepared by pure PVA binder and pure PVA binder is smaller (1.217N, 1.366N), and the two alone cannot bring out the unique advantages of the material. The average peeling force of the pole pieces corresponding to PVA-WPU-55, PVA-WPU-64, PVA-WPU-73, PVA-WPU-82 and PVA-WPU-91 binders are 2.725N, 2.849N, 3.013N, 2.786N and 2.691N, respectively. The average peeling force corresponding to PVA-WPU-73 binder is the highest. The optimal mixing concentration of PVA and WPU is 7:3. At this time, the utilization rate of hydrogen bonding sites inside the adhesive structure is the highest, allowing the WPU molecular chains to entangle with each other, improving the overall mechanical strength of the adhesive and thus exerting the best bonding performance.

[0114] Example 2

[0115] The preparation of WPU is the same as in Example 1;

[0116] The preparation of PVA-WPU binder was the same as in Example 1, wherein the mass ratio of PVA to WPU was 7:3;

[0117] Preparation of PVA-Ag-WPU adhesive: Take 3.5g PVA gel and WPU emulsion (containing 1.5g WPU), mix the two, add ultrapure water as solvent, stir at room temperature for 12h to obtain a uniform and stable milky white adhesive solution, then add 1mL 1mg / mL silver nanoparticle solution (average particle size 12nm), stir at room temperature for 6h to ensure that the Ag nanoparticles are evenly dispersed to obtain a uniform PVA-Ag-WPU adhesive.

[0118] PVA-Al 3+ Preparation of PVA-Ag-WPU binder: The preparation method is basically the same as that of the above-mentioned PVA-Ag-WPU binder, except that after obtaining a uniform milky white binder solution, 1 mL of 1 mol / L AlCl3 solution is added and stirred at a constant speed for 6 h at room temperature to obtain a uniform PVA-Al 3+ -WPU binder.

[0119] Preparation of PVA-M-WPU binder: The preparation method of PVA-Ag-WPU binder is basically the same as that of the above-mentioned method, except that: after obtaining a uniform milky white binder solution (20 wt%), 1 mL of AlCl3 solution (1 mol·L -1 ), stirred at room temperature for 6 h to ensure that Al 3+ Dispersed evenly in the system to obtain uniform PVA-Al 3+ -WPU binder. Under the same operating conditions, AlCl3 was replaced by FeCl3, ZnCl2, and NiCl2 to obtain PVA-Fe 3+ -WPU, PVA-Zn 2+ -WPU, PVA-Ni 2+ -WPU binder. Fig.26 As shown, PVA-Al 3+ -WPU binder is evenly dispersed, but PVA-Fe 3+ -WPU, PVA-Zn 2+ -WPU, PVA-Ni 2+ -WPU three kinds of binders showed obvious flocculation phenomenon, and it can be seen that Fe 3+ 、Zn 2+ 、Ni 2+ These three metal ions are not suitable for the PVA-WPU binder system. 3+ -WPU adhesive expansion.

[0120] The preparation of the silicon-carbon negative electrode is the same as in Example 1;

[0121] The preparation of lithium iron phosphate (LiFePO4) positive electrode is the same as in Example 1;

[0122] Fig.12 It is (a) SiC650 / PVA-Ag-WPU; (b) SiC650 / PVA-Al 3+ -SEM images of WPU, Figures a and b show the distribution of Si, C, Ag, and Al in the two silicon-carbon negative electrodes. The various elements in the electrode are evenly distributed, and there is no element agglomeration. Among them, the uniform distribution of Ag and Al is conducive to the construction of the conductive network in the electrode, promoting Li + The rapid transmission of electrochemical reactions can improve the rate of electrochemical reactions, promote the effective utilization of active substances during the cycle, and thus promote the capacity stability during the charge and discharge process.

[0123] Fig.13 For WPU and PVA-WPU, PVA-Ag-WPU, PVA-Al 3+-Comparison of FTIR spectra of WPU binder, the test fully proves the successful synthesis of WPU, at 3370cm -1 The peak range becomes significantly wider and tends to move to the lower peak position, proving that the introduction of metal coordination bonds and conductive additives reacts with carbamate groups and hydroxyl groups to form a conductive composite cross-linked network.

[0124] Fig.14 PVA-Ag-WPU, PVA-Al 3+ -XPS spectrum of the silicon-carbon negative electrode corresponding to the WPU binder after 100 cycles. The silicon-carbon negative electrode made with the binder modified by conductive properties is easier to form a dense and stable SEI film, and is not easy to cause side reactions during the charge and discharge process, thereby improving the cycle stability.

[0125] Fig.15 It is (a) SiC650 / PVA-Ag-WPU; (b) SiC650 / PVA-Al 3+ -WPU CV curve, there is no stray peak, indicating that the redox reaction inside the electrode is highly reversible, there is no interference from side reactions, and it has excellent electrochemical stability during the charge and discharge process. 3+ -WPU corresponding to the current value is higher than that of SiC650 / PVA-Ag-WPU, indicating that the introduction of metal coordination bonds is more effective in improving the electrochemical performance and can better stimulate the activity of electrochemical reactions.

[0126] Fig.16 The impedance comparison of silicon-carbon anodes with different binders after 100 cycles, SiC650 / PVA-Al 3+ -WPU, SiC650 / PVA-Ag-WPU have obvious linear slopes in the low-frequency region, indicating that Li + The diffusion rate is significantly improved, which is beneficial to increase the electrochemical reaction rate and the effective capacity conversion rate of active substances, thereby improving the overall electrochemical performance.

[0127] Fig.17 Comparison of the long cycle capacity of silicon-carbon anodes corresponding to different binders, SiC650 / PVA-WPU, SiC650 / PVA-Ag-WPU and SiC650 / PVA-Al 3+ -WPU has a capacity retention rate of 70.90%, 72.67% and 82.15% after 500 cycles.

[0128] Fig.18The performance comparison of silicon-carbon anode rate corresponding to different binders is shown in Figure 1. At the rates of 0.1C, 0.2C, 0.3C, 0.5C, 1C, and 3C, the discharge specific capacities of lithium batteries assembled with different binder ratios at a current density of 0.1C are 613.9 mAh g -1 、619.3mAh·g -1 and 640.5mAh·g -1 , among which SiC650 / PVA-Al 3+ -WPU is almost close to the standard specific capacity of 650mAh g -1 At the same time, as the current density gradually increases, the discharge specific capacity of this silicon-carbon negative electrode is always greater than that of other silicon-carbon negative electrodes.

[0129] Fig.19 Comparison of the coulombic efficiency of silicon-carbon anodes corresponding to different binders, SiC650 / PVA-WPU, SiC650 / PVA-Ag-WPU and SiC650 / PVA-Al 3+ -The ICE of WPU is 80.96%, 83.20% and 85.24% respectively. The introduction of conductive additives and metal coordination bonds improves the conductivity of the binder. After 5 cycles of activation, the CE of the silicon-carbon negative electrode corresponding to the three binders remained above 98%, which shows that a stable SEI layer has been formed on the surface of the silicon-carbon negative electrode, maintaining the stability of the electrochemical reaction and having good electrochemical reversibility.

[0130] Example 3

[0131] The preparation of WPU is the same as in Example 1;

[0132] The preparation of PVA-WPU binder was the same as in Example 1, wherein the mass ratio of PVA to WPU was 7:3;

[0133] Preparation of PVA-Ag-WPU adhesive: Take 3.5g of PVA gel and WPU emulsion (containing 1.5g of WPU), mix the two, add ultrapure water as a solvent, and stir at room temperature for 12 hours to obtain a uniform and stable milky white adhesive solution. Continue to add 0.2mL of 5mg / mL silver nanowire solution (diameter: 70nm, length: 45μm, purity: >99.5%), and stir at room temperature for 6 hours to obtain a uniform PVA-Ag-WPU adhesive.

[0134] PVA-Al 3+ - The preparation of WPU binder is the same as in Example 2;

[0135] Preparation of silicon-carbon negative electrode: SiC950, Super P, and PVA-WPU were mixed and ground in a mass ratio of 80:10:10. The mixture was then dispersed in NMP and stirred overnight. The slurry was coated on aluminum foil and dried to remove the solvent to obtain a silicon-carbon negative electrode.

[0136] The preparation of lithium iron phosphate (LiFePO4) positive electrode is the same as that in Example 1.

[0137] Fig. 20 The XRD spectra of SiC650 and SiC950 show no obvious impurity peaks, indicating that the purity of the two materials is high, which can effectively avoid the probability of side reactions caused by impurities during charging and discharging, thereby improving the active material and Li + utilization rate.

[0138] Fig.21 The SEM images of the silicon-carbon negative electrode before and after cycling at a current density of 1C show that there is no significant difference between the three types of electrodes before cycling, and the surface is uniform without agglomeration. After cycling, the electrode has different degrees of electrode damage due to the expansion of silicon materials. The cracks on the surface of SiC950 / PVA-WPU are long and deep, followed by SiC950 / PVA-Ag-WPU, and SiC950 / PVA-Al 3+ -WPU surface cracks are the narrowest and have a small propagation range. Therefore, after the binder is modified with conductive properties, the charge transfer resistance is reduced, which greatly improves the Li + conductivity, promoting the formation of a denser SEI film and reducing electrode damage.

[0139] Fig. 22 SiC950 / PVA-Al 3+ -WPU CV curve, the overlap of the three test curves is high, indicating that the redox reaction inside the battery is highly reversible. The reduction peak at 0.15V corresponds to the lithium insertion reaction; at the same time, the oxidation peak at 0.53V corresponds to the formation of SEI film. There are no other impurity peaks, which indicates that there are few side reactions inside the battery and the electrochemical stability is high.

[0140] Fig.23 Comparison of the long cycle capacity of silicon-carbon anodes corresponding to different binders, SiC650 / PVA-WPU, SiC650 / PVA-Ag-WPU and SiC650 / PVA-Al 3+ -WPU has a capacity retention rate of 72.69%, 79.43% and 82.28% after 300 cycles.

[0141] Fig.24Comparison of the rate performance of silicon-carbon anodes corresponding to different binders. At the rates of 0.1C, 0.2C, 0.3C, 0.5C, 1C, and 3C, SiC950 / PVA-WPU, SiC950 / PVA-Ag-WPU, and SiC950 / PVA-Al 3+ -WPU has a discharge capacity of 810.5 mAh g at a current density of 0.1C. -1 、892.0mAh·g -1 and 930.9mAh·g -1 , among which SiC950 / PVA-Al 3+ -The discharge specific capacity of WPU reaches 97.99% of the theoretical specific capacity. At the same time, as the current density gradually increases, the discharge specific capacity of this silicon-carbon negative electrode is always greater than that of other silicon-carbon negative electrodes.

[0142] Fig.25 Comparison of the coulombic efficiency of silicon-carbon anodes corresponding to different binders, SiC950 / PVA-WPU, SiC950 / PVA-Ag-WPU and SiC950 / PVA-Al 3+ -WPU's ICE is 78.46%, 80.75% and 81.91% respectively. After 5 cycles of activation, the CE of the silicon-carbon negative electrode made of the three binders remained above 98%, which shows that although the addition ratio of silicon in the active material is increased and the volume effect is increased, each electrode still forms a stable SEI layer with good electrochemical activity and stability.

[0143] The above description of the embodiments is to facilitate the understanding and use of the invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the above embodiments, and improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention should be within the scope of protection of the present invention.

Claims

1. A binder containing an interpenetrating network, It is characterized in that The invention comprises polyvinyl alcohol, waterborne polyurethane and water obtained by physical mixing, wherein the mass ratio of the polyvinyl alcohol to the waterborne polyurethane is (1-9):

1.

2. A method for preparing an interpenetrating network-containing adhesive as claimed in claim 1, It is characterized in that include: The polyvinyl alcohol, water-based polyurethane and water are stirred and mixed to obtain the product.

3. An adhesive containing an interpenetrating network and a conductive network, It is characterized in that It includes polyvinyl alcohol, water-based polyurethane, additives and water obtained by physical mixing. The mass ratio of polyvinyl alcohol to waterborne polyurethane is (1-9):1; The additive is a conductive additive or a metal ligand, wherein the conductive additive is selected from at least one of silver nanoparticles or silver nanowires; the metal ligand is selected from Al 3+ .

4. A method for preparing an adhesive comprising an interpenetrating network and a conductive network as claimed in claim 3, It is characterized in that include: The polyvinyl alcohol, water-based polyurethane and water are stirred and mixed, and then additives are added to make it.

5. A method for preparing the adhesive according to claim 2 or 4, It is characterized in that The preparation method of the waterborne polyurethane comprises: Polyethylene glycol, dimethylol propionic acid, isophorone diisocyanate and dibutyltin dilaurate are mixed and reacted, and then 2-hydroxyethyl methacrylate is added and stirred to react to obtain a polyurethane prepolymer; Add triethylamine to carry out neutralization reaction; Add water to emulsify the reaction; Ethylene diamine is added to carry out emulsion polymerization to obtain waterborne polyurethane.

6. The method for preparing the binder according to claim 5, It is characterized in that The feeding ratio of the polyethylene glycol, dimethylol propionic acid, isophorone diisocyanate, dibutyltin dilaurate, and 2-hydroxyethyl methacrylate is (20-30) g: (2-3) g: (9-13.5) g: (42-63) μL: (1-3) mL; The mixed reaction comprises: firstly reacting polyethylene glycol and dimethylol propionic acid at 85-90° C. for 1-1.5 hours; then adding isophorone diisocyanate and dibutyltin dilaurate and reacting at 80-85° C. for 2-2.5 hours; In the stirring reaction, the reaction temperature is 80-85° C. and the reaction time is 1-1.5 h.

7. The method for preparing the binder according to claim 5, It is characterized in that In the neutralization reaction, the amount of triethylamine added is (2-3) mL / mL 2-hydroxyethyl methacrylate; the reaction temperature is 40-45° C., and the reaction time is 0.5-1 h.

8. The method for preparing the adhesive according to claim 5, It is characterized in that In the emulsification reaction, the amount of water added is (65-70) mL / mL 2-hydroxyethyl methacrylate; the reaction temperature is 85-90° C., and the reaction time is 0.25-0.3 h.

9. The method for preparing the binder according to claim 5, It is characterized in that In the emulsion polymerization reaction, the amount of ethylenediamine added is 8-9 μL / μL dibutyltin dilaurate; the reaction temperature is 85-90° C., and the reaction time is 3-4 hours.

10. Use of the adhesive according to claim 1 or 3, It is characterized in that Binders are used in the preparation of lithium batteries.

Citation Information

Patent Citations

  • Polyving alcohol composite hydrogel and preparation method thereof

    CN103665685A

  • Conductive slurry and transparent conductive coating

    CN106205774A

  • Polyvinyl alcohol / allyl copolymer interpenetrating network silicon-carbon negative electrode water-based adhesive as well as preparation method and application of polyvinyl alcohol / allyl copolymer interpenetrating network silicon-carbon negative electrode water-based adhesive

    CN114242990A

  • Polyurethane / conductive carbon black composite foam flexible sensor and preparation method thereof

    CN117801352A

  • Anisotropic conductive network fiber and preparation method and application thereof