Preparation method of hydrothermal carbon powder fully replaced by flour filler in urea-formaldehyde adhesive and application of hydrothermal carbon powder in plywood

Hydrothermal carbon powder prepared by hydrothermal method is used to replace flour fillers in plywood, solving the problem of insufficient viscosity and prepressing performance of flour substitute materials in the prior art, achieving efficient plywood production, and reducing edible resources and improves the performance and environmental protection of plywood.

CN118931440APending Publication Date: 2024-11-12GUANGXI NORMAL UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411196775.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

In the production of existing plywood, the alternative materials for flour fillers have problems such as low initial viscosity and poor prepressing performance, and consume a lot of edible resources, making it difficult to replace flour completely.

Method used

Hydrothermal carbon powder was prepared by hydrothermal method by hydrothermal method, and it was completely replaced as flour filler for urea-formaldehyde adhesive to prepare plywood with high initial viscosity and good prepressing properties.

Benefits of technology

Effectively utilize agricultural and forestry solid waste, reduce the use of edible resources, improve the mechanical properties of plywood and reduce formaldehyde emission, and meet the national standard Class I I plywood standards.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005016668380000091
    Figure BDA0005016668380000091
Patent Text Reader

Abstract

The invention belongs to the technical field of plywood, and particularly relates to a preparation method of hydrothermal carbon powder fully replaced by flour filler in a urea-formaldehyde adhesive and application of the hydrothermal carbon powder in the plywood. The method comprises the following steps: 1) mixing fiber-containing biomass with water, and carrying out heat treatment in a reaction kettle to obtain a hydrothermal carbon precursor; 2) treating the hydrothermal carbon precursor obtained in the step 1) into hydrothermal carbon powder; and (3) mixing and stirring the hydrothermal carbon powder obtained in the step (2), urea-formaldehyde adhesive raw glue and a curing agent, and blending into smooth paste, so as to obtain the urea-formaldehyde adhesive blended glue for preparing the plywood. The fiber-containing biomass is a new or waste agriculture and forestry biomass material. According to the invention, the fiber-containing agriculture and forestry biomass material is prepared into the hydrothermal carbon powder through a hydrothermal method, and the prepared hydrothermal carbon powder is used as a full substitute for a urea-formaldehyde adhesive flour filler in the plywood production process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of plywood, and particularly relates to a preparation method of hydrothermal carbon powder for fully replacing flour filler in urea-formaldehyde adhesive and application of the powder in plywood. Background Art

[0002] Plywood production has been developing rapidly due to its advantages such as light weight, high strength, beautiful appearance, convenient construction and cost-effectiveness. Adhesives are needed to produce plywood. Urea-formaldehyde adhesives have become the most widely used synthetic resin adhesives in the wood industry due to their rich raw material sources, low production costs and fast curing speed. The performance of urea-formaldehyde adhesives can be changed or adjusted by adding various additives. The fillers in urea-formaldehyde adhesives can increase the initial viscosity, prevent excessive penetration of the glue, improve the pre-pressing performance of the plywood, and improve the water resistance, heat resistance, aging resistance, and toughness of the plywood. It can also reduce the amount of adhesive used in plywood and reduce production costs. In the production of plywood, flour is usually used as a filler, and the amount of flour added is 20% to 30% of the weight of the urea-formaldehyde adhesive. Flour is one of the staple foods for human survival, and plywood production consumes a large amount of edible resources.

[0003] In order to reduce the use of edible flour, alternative materials for filler flour have been studied. At present, the alternative materials for flour filler in adhesives for plywood production can be divided into inorganic mineral fillers, organic fillers and carbon fillers according to their chemical composition.

[0004] Alternative materials for flour fillers in adhesives in plywood production (1) Inorganic mineral fillers, such as zeolite, sepiolite, clay, algae, coal grinding stone powder, etc. Inorganic mineral fillers added to urea-formaldehyde resin adhesives will cause the initial viscosity of the adhesive to be too low and the pre-pressing performance to be very poor. In addition, excessive addition will cause the adhesive to stratify when standing. (2) Protein powder fillers, such as soybean powder and blood powder, are very good fillers, but they are expensive. (3) Organic starch and agricultural and forestry waste biomass powder (crop waste, wood waste) fillers. Starch is also an edible resource. Using it in the adhesive industry will cause a waste of edible resources. Agricultural and forestry waste biomass powder has poor sizing and pre-pressing performance. (4) Carbon fillers such as carbon black and activated carbon. Carbon fillers have higher bonding strength and lower formaldehyde emission in plywood prepared with urea-formaldehyde resin. However, the current carbon fillers still have the disadvantages of low adhesive viscosity, poor pre-pressing performance, and cannot completely replace flour. Summary of the invention

[0005] In order to solve the deficiencies of the prior art, the present invention provides a method for preparing hydrothermal carbon powder that can completely replace flour filler in urea-formaldehyde adhesive and its application in plywood. The present invention prepares hydrothermal carbon powder from fiber-containing agricultural and forestry waste biomass materials by a hydrothermal method, and uses the prepared hydrothermal carbon powder as a complete replacement for flour filler in urea-formaldehyde adhesive in the production process of plywood.

[0006] The technical solution provided by the present invention is as follows:

[0007] A method for preparing hydrothermal carbon powder for fully replacing flour filler in urea-formaldehyde adhesive and its application in plywood, comprising the following steps:

[0008] 1) mixing the fiber-containing biomass with water and placing the mixture in a reactor for heat treatment to obtain a hydrothermal carbon precursor;

[0009] 2) processing the hydrothermal carbon precursor obtained in step 1) into hydrothermal carbon powder;

[0010] 3) The hydrothermal carbon powder, urea-formaldehyde adhesive and curing agent obtained in step 2) are mixed and stirred to form a smooth paste to obtain a urea-formaldehyde adhesive for preparing plywood.

[0011] The above technology can use fiber-containing biomass as raw material to prepare hydrothermal carbon powder filler, and this filler can completely replace flour filler to prepare urea-formaldehyde adhesive used in the plywood production process.

[0012] Specifically, in step 1), the fiber-containing biomass is new or discarded agricultural and forestry biomass material, or is industrial fiber-containing waste.

[0013] Specifically, the agricultural and forestry biomass material is selected from any one or more of bagasse, sugarcane straw, bamboo, eucalyptus or other agricultural and forestry biomass wood containing fiber.

[0014] Specifically, in step 1), the mass ratio of fiber biomass to water is 1:1 to 1:3, and can be 1:1, 1:2, 1:3 or other ratios, preferably 1:2.

[0015] The heat treatment temperature is 225 degrees Celsius or above, preferably 240 degrees Celsius;

[0016] The heat treatment time is 3 hours or more, preferably 3 hours.

[0017] Specifically, in step 2):

[0018] Step a): directly drying and crushing the hydrothermal carbon precursor obtained in step 1) to obtain hydrothermal carbon powder;

[0019] Alternatively, step b) is adopted: freeze drying is used to obtain hydrothermal carbon powder.

[0020] More specifically, in step a), the hydrothermal carbon precursor obtained in step 1) is filtered to remove water, and then heated and dried in an oven to obtain a dry hydrothermal carbon precursor, which is then crushed to obtain hydrothermal carbon powder.

[0021] More specifically, in step b), a certain amount of water is added to the hydrothermal carbon precursor obtained in step 1), and then crushed by a wall-breaking machine to obtain a mixture of crushed hydrothermal carbon and water, and then filtered to remove water, and then dried by freeze drying, and then dried in an oven, and then crushed to obtain hydrothermal carbon powder; the mass ratio of the hydrothermal carbon precursor to the newly added water is 1:1 to 1:2. It can be 1:1, or 1:1.5, 1:2 or other ratios.

[0022] Specifically, in step 3), the weight percentage usage of each component is: take 80g of urea-formaldehyde adhesive raw rubber; then add 20-30% filler by weight of the urea-formaldehyde adhesive raw rubber and 1.25% curing agent by weight of the urea-formaldehyde adhesive raw rubber and stir evenly to obtain urea-formaldehyde adhesive prepared glue.

[0023] The preparation method of hydrothermal carbon powder for completely replacing flour filler with urea-formaldehyde adhesive may specifically include the following steps:

[0024] S1. placing agricultural and forestry waste biomass and deionized water (mass ratio of 1:2) in a hydrothermal reactor;

[0025] S2. Tighten the hydrothermal reactor and place it in a muffle furnace, set the reaction temperature, and the reaction time is 3h;

[0026] S3. After the reaction is completed, cool to room temperature and take out to obtain a hydrothermal carbon precursor;

[0027] S4. Take out the hydrothermal carbon precursor and place it in an oven to dry, and then crush it to obtain hydrothermal carbon powder; or prepare hydrothermal carbon powder according to steps S5-S7;

[0028] S5. Add water to the hydrothermal carbon precursor to form a hydrothermal carbon mixture, that is, the hydrothermal carbon precursor and a certain amount of water are added, the ratio can be 1:1, or 1:1.5, 1:2 or other ratios, and then use a wall breaking machine to break and filter;

[0029] S6. Place the solid sample in a vacuum freeze dryer and freeze for 8 hours and dry for 12 hours;

[0030] S7. Use a grinder or agate mortar to grind the agricultural and forestry waste biomass to obtain hydrothermal charcoal powder.

[0031] The invention also provides hydrothermal carbon powder prepared by the method.

[0032] The present invention also provides an application of the hydrothermal carbon powder, which is used for completely replacing the flour filler of the urea-formaldehyde adhesive in the process of preparing plywood.

[0033] The hydrothermal carbon powder prepared by the present invention is used as a substitute for the flour filler of the plywood without changing the preparation process of the plywood, is easy to apply glue, has high initial viscosity, is not easy to debond and bubble, has good pre-pressing performance, and the plywood has excellent mechanical properties, and is conducive to the release of formaldehyde in the plywood.

[0034] The beneficial effects of the present invention are as follows:

[0035] Compared with other existing flour substitute fillers, the present invention can effectively utilize the product prepared from agricultural and forestry solid waste as a complete substitute for flour filler, saving edible resources;

[0036] The only additive in the hydrothermal reaction is water, which is easy to remove after the reaction; the hydrothermal carbon precursor is taken out and placed in an oven directly, and then crushed to obtain hydrothermal carbon powder. The process is simple, but the particle size is relatively coarse; after the hydrothermal reaction, a wall breaker is used to crush the hydrothermal reaction product, and after crushing, freeze-drying and heating drying are used to obtain hydrothermal carbon powder. This process has high crushing efficiency, the product after drying does not agglomerate, and it is easy to crush into powder. DETAILED DESCRIPTION

[0037] The principles and features of the present invention are described below. The examples given are only used to explain the present invention and are not used to limit the scope of the present invention.

[0038] Unless otherwise specified, the test methods used in the embodiments of the present invention are conventional methods; the materials and reagents used are reagents and materials that can be obtained from commercial channels unless otherwise specified.

[0039] Example 1

[0040] 65 g of bagasse and 130 g of deionized water (mass ratio of 1:2) were placed in a hydrothermal reactor; the hydrothermal reactor was tightened and placed in a muffle furnace, and heat treated at 240°C for 3 h; after the heat treatment was completed, it was cooled to room temperature and taken out to obtain a mixture of hydrothermal carbon and water (hydrothermal carbon precursor), and 300 g of water was added, that is, the mass ratio of the hydrothermal carbon and water mixture to the newly added water was about 1:1.5; then it was crushed with a wall breaker and filtered; the solid sample was placed in a vacuum freeze dryer for 8 h and dried for 12 h; it was crushed with a grinder or an agate mortar to obtain bagasse hydrothermal carbon powder 1.

[0041] Example 2

[0042] 65 g of bagasse and 65 g of deionized water (mass ratio of 1:1) were placed in a hydrothermal reactor; the hydrothermal reactor was tightened and placed in a muffle furnace, and heat treated at 240°C for 3 h; after the heat treatment was completed, it was cooled to room temperature and taken out to obtain a mixture of hydrothermal carbon and water (hydrothermal carbon precursor), and 130 g of water was added, that is, the mass ratio of the mixture to the newly added water was 1:1; then it was crushed with a wall breaker and filtered; the solid sample was placed in a vacuum freeze dryer and frozen for 8 h, and dried for 12 h; it was crushed to obtain bagasse hydrothermal carbon powder 2.

[0043] Example 3

[0044] 65 g of bagasse and 195 g of deionized water (mass ratio of 1:3) were placed in a hydrothermal reactor; the hydrothermal reactor was tightened and placed in a muffle furnace, and heat treated at 240°C for 5 hours; after the heat treatment, a hydrothermal carbon precursor was obtained; it was then dried in an oven at 100°C for 3 hours and then crushed to obtain bagasse hydrothermal carbon powder 3.

[0045] Example 4

[0046] 65 g of bagasse and 65 g of deionized water (mass ratio of 1:1) were placed in a hydrothermal reactor; the hydrothermal reactor was tightened and placed in a muffle furnace, and heat treated at 225°C for 5 h; after the heat treatment was completed, it was cooled to room temperature and taken out to obtain a mixture of hydrothermal charcoal and water, and 130 g of water was added, i.e., the mass ratio of the mixture to the newly added water was 1:1; then it was crushed using a wall breaker and filtered; the solid sample was placed in a vacuum freeze dryer and frozen for 8 h, and dried for 12 h; it was crushed to obtain 4% bagasse hydrothermal charcoal powder.

[0047] Example 5

[0048] 65 g of bamboo chips and 130 g of deionized water (mass ratio of 1:2) were placed in a hydrothermal reactor; the hydrothermal reactor was tightened and placed in a muffle furnace, and heat treated at 240°C for 3 h; after the heat treatment was completed, it was cooled to room temperature and taken out to obtain a mixture of hydrothermal charcoal and water, and 390 g of water was added, that is, the mass ratio of the mixture to the newly added water was about 1:2; then it was crushed using a wall breaker and filtered; the solid sample was placed in a vacuum freeze dryer and frozen for 8 h, and dried for 12 h; it was crushed to obtain bamboo chip hydrothermal charcoal powder 5.

[0049] Example 6

[0050] 65 g of eucalyptus board and 130 g of deionized water (mass ratio of 1:2) were placed in a hydrothermal reactor; the hydrothermal reactor was tightened and placed in a muffle furnace, and heat treated at 240°C for 3 h; after the heat treatment was completed, it was cooled to room temperature and taken out to obtain a mixture of hydrothermal charcoal and water, and 300 g of water was added, that is, the mass ratio of the mixture to the newly added water was about 1:1.5; then it was crushed with a wall breaker and filtered; the solid sample was placed in a vacuum freeze dryer and frozen for 8 h, and dried for 12 h; it was crushed to obtain bagasse hydrothermal charcoal powder 6.

[0051] Example 7

[0052] 65 g of sugarcane straw and 130 g of deionized water (mass ratio of 1:2) were placed in a hydrothermal reactor; the hydrothermal reactor was tightened and placed in a muffle furnace, and heat treated at 240°C for 3 h; after the heat treatment was completed, it was cooled to room temperature and taken out to obtain a mixture of hydrothermal charcoal and water, and 300 g of water was added, that is, the mass ratio of the mixture to the newly added water was about 1:1.5; then it was crushed using a wall breaker and filtered; the solid sample was placed in a vacuum freeze dryer and frozen for 8 h, and dried for 12 h; it was crushed to obtain sugarcane straw hydrothermal charcoal powder 7.

[0053] Example 8

[0054] 30 g of bagasse, 35 g of sugarcane straw and 130 g of deionized water (mass ratio of solid to water is 1:2) are placed in a hydrothermal reactor; the hydrothermal reactor is tightened and placed in a muffle furnace, and heat treated at 240°C for 3 h; after the heat treatment is completed, it is cooled to room temperature and taken out to obtain a mixture of hydrothermal charcoal and water, and 300 g of water is added, that is, the mass ratio of the mixture to the newly added water is about 1:1.5; then it is crushed with a wall breaker and filtered; the solid sample is placed in a vacuum freeze dryer and frozen for 8 h, and dried for 12 h; crushed to obtain 8 g of bagasse and sugarcane straw mixed hydrothermal charcoal powder.

[0055] Plywood properties

[0056] The hydrothermal carbon powder filler and flour filler prepared in Examples 1, 2, 3, 4, 5, 6, 7, and 8 were uniformly mixed with the original urea-formaldehyde adhesive (F:U=1.4:1) synthesized in the laboratory to prepare a modulated glue for the urea-formaldehyde adhesive for plywood. Then, the modulated glue was used as an adhesive to prepare plywood 1, plywood 2, plywood 3, plywood 4, plywood 5, plywood 6, plywood 7, plywood 8, and a plywood control (flour filler). The properties of the obtained plywoods were tested and shown in (Table 2).

[0057] The specific steps of synthesizing the original urea-formaldehyde adhesive (F:U=1.4:1) are as follows:

[0058] Add formaldehyde solution (454g) to a 1000ml four-necked flask and stir for a while, and slowly adjust the reaction temperature to 60°C. Add the first batch of urea U1 (60g) to the reaction system, and then adjust the pH of the system to 8-8.5 with an appropriate amount of NaOH solution (concentration of 40%). Slowly heat the water bath to 88°C. Adjust the pH to 5-5.4 with formic acid solution, keep warm for 20min, add the second batch of urea U2 twice (50g, 100g), and react to the target viscosity. Cool down to 60°C, add the third batch of urea U3 (30g), and keep at the reaction temperature for 20min. After that, cool the reaction temperature to 30°C to obtain a transparent urea-formaldehyde adhesive.

[0059] Preparation of urea-formaldehyde adhesive for plywood:

[0060] Weigh 80g of the synthesized urea-formaldehyde adhesive raw rubber and put it into a beaker, add 20-30% filler based on the weight of the urea-formaldehyde adhesive raw rubber and 1.25% ammonium chloride based on the weight of the urea-formaldehyde adhesive raw rubber as a curing agent, stir evenly to obtain a urea-formaldehyde adhesive modulated glue for standby use.

[0061] Determination of pre-compression properties of plywood:

[0062] Eucalyptus veneer (480mm×480mm, thickness 1.7mm) with a moisture content of 8% to 12% was selected, and double-sided glue was applied manually, with a single-sided glue amount of 166g / m 2 (Urea-formaldehyde adhesive modulated glue), press three-layer plywood, place the assembled plywood in the press, take it out after 30 minutes of pre-pressing at room temperature and 1.0MPa, and then place the board in a dry and ventilated environment for 30 minutes, observe the situation of the periphery rolling up and debonding perpendicular to the wood fiber, measure the length of the debonding side, and express the pre-pressing performance of the glue as a percentage of the total side length. This evaluation standard adopts the laboratory custom standard (Table 1) provided by reference (Li Xiaona, Shi Ruiqing, Li Jianzhang. Effect of white clay on the performance of melamine-urea-formaldehyde co-condensation resin. Journal of Forestry Engineering, 2022, 7(2): 78-83.) to judge the pre-pressing performance.

[0063] Table 1 Laboratory preloading performance custom evaluation table

[0064] Crack length Can it meet production requirements? grade The percentage of warped side length to total side length = 0% (no warping) satisfy A 0%<The percentage of warped side length to total side length≤10% Basic satisfaction B The percentage of warped side length to total side length is > 10% Cannot satisfy C

[0065] Determination of bonding strength

[0066] 1. Pressing plywood: After raising the temperature of the hot press to 115°C, place a piece of pre-pressed plywood into the hot press, set the hot press pressure to 1.2MPa, and the hot press time to 5min.

[0067] 2. Bonding strength test: Plywood is made in strict accordance with the preparation method in GB / T 9846-2015 "Ordinary Plywood", and the wet bonding strength of the sample is tested according to the test method for Class II plywood in GB / T 17657-2013 "Test methods for physical and chemical properties of wood-based panels and veneered wood-based panels".

[0068] Determination of formaldehyde emission

[0069] The formaldehyde emission of plywood was tested according to the dryer method in the national standard GB / T 17657-2013 "Test methods for physical and chemical properties of wood-based panels and veneer wood-based panels".

[0070] The test results are shown in Table 2:

[0071] Table 2 Performance indicators of plywood

[0072]

[0073] It can be seen that the urea-formaldehyde adhesive for preparing plywood provided by the present invention can effectively reduce the formaldehyde emission of plywood, improve the water-resistant bonding performance, and meet the national standard for Class II plywood.

[0074] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing hydrothermal carbon powder for completely replacing flour filler in urea-formaldehyde adhesive, characterized in that: The following steps are involved: 1) mixing the fiber-containing biomass with water and placing the mixture in a hydrothermal reactor for heat treatment to obtain a hydrothermal carbon precursor; 2) processing the hydrothermal carbon precursor obtained in step 1) into hydrothermal carbon powder; 3) The hydrothermal carbon powder, urea-formaldehyde adhesive and curing agent obtained in step 2) are mixed and stirred to form a smooth paste to obtain a urea-formaldehyde adhesive prepared for preparing plywood.

2. The method for preparing hydrothermal carbon powder for fully replacing flour filler in urea-formaldehyde adhesive according to claim 1, characterized in that: In step 1), the fiber-containing biomass is new or waste agricultural and forestry biomass material.

3. The method for preparing hydrothermal carbon powder for fully replacing flour filler in urea-formaldehyde adhesive according to claim 2, characterized in that: The agricultural and forestry biomass material is selected from any one or more of bagasse, sugarcane straw, bamboo, eucalyptus or other agricultural and forestry biomass containing fiber.

4. The method for preparing hydrothermal carbon powder for fully replacing flour filler in urea-formaldehyde adhesive according to claim 1, characterized in that: In step 1): The mass ratio of fiber biomass to water is 1:1 to 1:3; The heat treatment temperature is 225 degrees Celsius or above; The heat treatment time is 3 hours or more.

5. The method for preparing hydrothermal carbon powder for fully replacing flour filler in urea-formaldehyde adhesive according to claim 1, characterized in that: In step 2): Step a): directly drying and crushing the hydrothermal carbon precursor obtained in step 1) to obtain hydrothermal carbon powder; Alternatively, step b) is adopted: freeze drying is used to obtain hydrothermal carbon powder.

6. The method for preparing hydrothermal carbon powder for fully replacing flour filler in urea-formaldehyde adhesive according to claim 5, characterized in that: In step a), the hydrothermal carbon precursor obtained in step 1) is filtered to remove water, and then heated and dried in an oven to obtain a dry hydrothermal carbon precursor, which is then crushed to obtain hydrothermal carbon powder.

7. The method for preparing hydrothermal carbon powder for fully replacing flour filler in urea-formaldehyde adhesive according to claim 5, characterized in that: In step b): Adding a certain amount of new water to the hydrothermal carbon precursor obtained in step 1), and then crushing it with a wall-breaking machine to obtain a mixture of crushed hydrothermal carbon and water, then filtering to remove water, and then drying it with a freeze-drying method to obtain dry, and then drying it in an oven, and then crushing it to obtain hydrothermal carbon powder; The mass ratio of the hydrothermal carbon precursor to the newly added water is 1:1 to 1:

2.

8. A hydrothermal carbon powder prepared according to the preparation method according to any one of claims 1 to 7.

9. An application of the hydrothermal carbon powder according to claim 8, characterized in that: Used as a complete replacement for flour fillers in urea-formaldehyde adhesives during the preparation of plywood.