Epoxy adhesive and preparation method thereof
By using core-shell toughening agent and ether-containing bond curing agent prepared by octamethylcyclotetrasiloxane and acrylate in epoxy adhesives, traditional epoxy adhesives are easily brittle in flexible screen applications. , the problem of easy breaking has significantly improved its flexibility and impact resistance.
Patent Information
- Application Number
- CN202411005743.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-11-12
AI Technical Summary
Traditional epoxy adhesives are prone to brittleness and breakage in flexible screen frame sealing applications, resulting in a decrease in sealing and stability, affecting the durability and reliability of the equipment.
The core-shell toughening agent prepared by emulsion polymerization using octamethylcyclotetrasiloxane and acrylate as monomers is used to form a stable and uniform core-shell structure to improve the viscosity. The shear strength and impact resistance of the mixture.
It significantly improves the flexibility and impact resistance of epoxy adhesives, prevents cracks from spreading, extends the service life of the equipment and improves reliability.
Smart Images

Figure BDA0004962966990000051 
Figure BDA0004962966990000061 
Figure BDA0004962966990000081
Abstract
Description
Technical Field
[0001] The present invention relates to the field of epoxy adhesives, and more specifically, to an epoxy adhesive and a preparation method thereof. Background Art
[0002] With the rapid development of science and technology, flexible display technology has become one of the important development directions of the modern electronics industry, especially in the fields of smart phones, tablet computers, wearable devices, etc., showing broad application prospects. Flexible screens, with their thinness, bendability, impact resistance and other characteristics, bring users a new visual and usage experience. However, flexible screens still face a series of technical challenges in practical applications, among which the performance of epoxy adhesives used for frame sealing is one of the key issues.
[0003] Traditional epoxy adhesives are widely used in the packaging and bonding of electronic products due to their excellent bonding strength, heat resistance and chemical stability. However, in the specific application of flexible screen frame sealing, epoxy adhesives show defects such as brittleness and fracture. This is because the flexible screen will produce certain deformation and stress when bent or twisted, and traditional epoxy adhesives cannot effectively adapt to such deformation and stress due to their hard and brittle characteristics. Therefore, during long-term use, epoxy adhesives will gradually crack and break, resulting in reduced sealing and stability of the flexible screen. This defect not only affects the durability and reliability of the flexible screen, but may also cause performance degradation or even failure of the device during use.
[0004] Therefore, it is an urgent problem to prepare an epoxy adhesive with good flexibility and not easy to break. Summary of the invention
[0005] In order to improve the flexibility of epoxy adhesive, the present application provides an epoxy adhesive and a preparation method thereof.
[0006] In a first aspect, the present application provides an epoxy adhesive, which adopts the following technical solution: An epoxy adhesive comprises the following raw materials in parts by weight: 90-100 parts of epoxy resin, 12-16 parts of curing agent, 0.5-5 parts of accelerator, 5-10 parts of diluent, and 6-12 parts of toughening agent, wherein the toughening agent is a core-shell toughening agent prepared by emulsion polymerization using octamethylcyclotetrasiloxane and acrylate as monomers.
[0007] By adopting the above technical scheme, there are a large number of epoxy groups in the epoxy resin, and the chemical crosslinking density of the structure after the adhesive is cured is high, the flexibility of the molecular chain is low, and the internal stress is large, which leads to greater brittleness in the epoxy group and poor impact resistance. In practical applications, it causes the bonding point to crack easily and affect the use. The toughening agent is added to improve the impact resistance of the adhesive. At the same time, the silicone in the toughening agent acts as a stress concentrator, which can induce silver streaks and shear bands to absorb energy and terminate silver streaks, which helps to prevent the rapid expansion of cracks. At the same time, the core-shell polymer is subjected to external forces, which will cause the interface between the core-shell polymer particles and the matrix to rupture and produce holes. On the one hand, it can relieve the accumulated three-dimensional stress near the crack, and on the other hand, it increases the stress concentration of silicone, so that the cavitation effect occurs further, induces local shear yield, and prevents the passivation of the crack tip, thereby further reducing the stress concentration in the epoxy resin and preventing the fracture from occurring, thereby improving the toughness and impact resistance of the epoxy adhesive.
[0008] Optionally, the preparation of the core-shell toughening agent comprises the following steps: (1) adding deionized water, dodecylbenzenesulfonic acid, and octamethylcyclotetrasiloxane, stirring and emulsifying for 20-30 minutes, heating to 60-80° C. for reaction for 2-4 hours, and dropping a crosslinking agent and a silane coupling agent having a vinyl terminal group, stirring and reacting to obtain a vinyl-modified silicone emulsion; (2) Adding acrylate and potassium persulfate to the above vinyl modified silicone emulsion, stirring and reacting for 2-3 hours, cooling to room temperature, obtaining a core-shell toughening agent emulsion, and then demulsifying, filtering, washing and drying to obtain a powdered core-shell toughening agent.
[0009] By adopting the above technical scheme, octamethylcyclotetrasiloxane undergoes polymerization reaction under the catalysis and emulsification of dodecylbenzenesulfonic acid to form an organosilicon core. Subsequently, by dripping a crosslinking agent and a silane coupling agent with a vinyl terminal group, vinyl functional groups are introduced on the surface of the organosilicon core to form a vinyl-modified organosilicon emulsion. Under the further action of an initiator, acrylate monomers undergo polymerization reaction on the surface of the vinyl-modified organosilicon emulsion to form a polyacrylate shell layer. The acrylate monomers undergo copolymerization reaction with the vinyl functional groups to form a stable core-shell structure. When added to an epoxy adhesive system, the shear strength and impact strength of the adhesive are greatly improved.
[0010] Optionally, the weight ratio of octamethylcyclotetrasiloxane, silane coupling agent, crosslinking agent and acrylate in the core-shell toughening agent is 10-12:1:1-3:8-10.
[0011] By adopting the above technical scheme, by controlling the addition amount of core layer monomer and shell layer monomer, it is conducive to forming a stable and uniform core-shell structure. Octamethylcyclotetrasiloxane is used as a soft core that provides toughness. It is combined with a shell structure of appropriate proportion to prepare a toughening agent with good toughening effect. When subjected to stress, the core-shell structure can effectively absorb and disperse energy, prevent the rapid expansion of cracks, and improve the shear strength of the adhesive.
[0012] Optionally, the crosslinking agent is 1,4-butanediol diacrylate.
[0013] By adopting the above technical solution, the molecular structure of 1,4-butanediol diacrylate contains two unsaturated bonds. During the preparation of the core layer latex, the double bonds remaining from the incomplete reaction can be used as grafting points, thereby improving the grafting efficiency during the grafting process.
[0014] Optionally, the acrylate is any one of methyl methacrylate, methyl acrylate or ethyl acrylate.
[0015] By adopting the above technical scheme, any one of methyl methacrylate, methyl acrylate or ethyl acrylate is selected as the acrylate monomer to be polymerized to form a shell layer, which has better compatibility with the epoxy resin and can ensure that the toughening agent is uniformly dispersed in the epoxy resin matrix, so that it can better absorb the energy changes caused by external forces, improve the toughness of the epoxy adhesive, and effectively improve the flexibility and impact resistance of the epoxy adhesive.
[0016] Optionally, the curing agent is obtained by mixing an aromatic amine curing agent and a polyether amine curing agent in a ratio of 1:0.8-1.2.
[0017] By adopting the above technical solution, the polyetheramine molecule contains more ether bonds and has good flexibility. Adding it to the epoxy adhesive can reduce the crosslinking density and improve the flexibility of the molecular chain. After the epoxy adhesive is cured, the flexible chain segment of the curing agent is naturally bonded to the three-dimensional crosslinking network of the adhesive system. On the one hand, it improves the flexibility of the molecule and causes the structure of the adhesive to produce plastic deformation. On the other hand, the flexible chain segment will also produce a microscopic phase separation structure in the resin system, which cooperates with the core-shell toughening agent to alleviate the stress concentration phenomenon in the epoxy resin and further improve the toughness of the epoxy adhesive. The use of a polyetheramine curing agent with a flexible ether bond and a relatively stable aromatic amine curing agent as a curing agent for the adhesive fully utilizes the advantages of the two types of curing agents to give the prepared adhesive better toughness and impact strength.
[0018] Optionally, the accelerator is any one of cobalt cyclohexaneate or cobalt stearate.
[0019] By adopting the above technical scheme, cobalt cyclopentaneate and cobalt stearate show a good promoting effect in the aromatic amine curing agent, catalyze the curing reaction, increase the curing speed, and ensure that the curing process is efficient and stable, thereby obtaining an epoxy adhesive with stable performance and good toughness.
[0020] In a second aspect, the present application provides a method for preparing an epoxy adhesive, using the following technical solution: A method for preparing an epoxy adhesive comprises the following steps: A certain amount of epoxy resin, toughening agent and polyurethane are weighed and stirred evenly, ultrasonically mixed, cooled to room temperature, and then a curing agent, an accelerator and a diluent are added and mixed evenly to obtain the epoxy adhesive.
[0021] By adopting the above technical solution, an epoxy adhesive with good toughness is obtained.
[0022] In summary, this application has the following beneficial effects: 1. Since the core-shell toughener prepared by using octamethylcyclotetrasiloxane and acrylate as monomers is used in the present application, different material components are enriched inside and outside the core-shell structure, showing a special double-layer structure. After being impacted, this structure can effectively resist stress damage and prevent the expansion of cracks, so that the adhesive has better toughness and impact strength. At the same time, the shell acrylate polymer of the toughener can form an interpenetrating network with the epoxy resin to further reduce the internal stress of the epoxy resin, so that the impact resistance of the adhesive system is further improved.
[0023] 2. The present application optimizes the raw material ratio, and by controlling the amount of octamethylcyclotetrasiloxane, silane coupling agent, crosslinking agent and acrylate added in the core-shell toughening agent, a stable and uniform core-shell structure can be formed. When the weight ratio of octamethylcyclotetrasiloxane, silane coupling agent, crosslinking agent and acrylate added is 10-12:1:1-3:8-10, the resulting toughening agent has the best toughening effect.
[0024] 3. In this application, it is preferred to use a curing agent containing an ether bond as the curing agent, in which the macromolecules containing flexible segments are bonded to the three-dimensional cross-linked network of the adhesive system, which helps to alleviate stress concentration, improve the brittleness and easy breakage problems of the epoxy adhesive, and greatly improve the toughness of the adhesive. DETAILED DESCRIPTION
[0025] The present application is further described in detail below with reference to the embodiments.
[0026] If the specific conditions are not specified in the examples, the experiments were carried out under conventional conditions or conditions recommended by the manufacturer. If the manufacturers of the reagents or instruments are not specified, they are all conventional products that can be purchased commercially.
[0027] As one of the important development directions of the modern electronic industry, the market demand for flexible display technology continues to grow. However, flexible screens still face a series of technical challenges in practical applications, among which the performance of epoxy adhesives for frame sealing is one of the key issues. Although traditional epoxy adhesives have excellent performance, they show defects such as brittleness and easy fracture in the application of flexible screen frame sealing, which limits the further development of flexible display technology. In order to improve the flexibility of epoxy adhesives, the present application proposes a new epoxy adhesive and a preparation method thereof. The epoxy adhesive adopts a specific raw material ratio and preparation process, and has excellent flexibility and impact resistance. By controlling the addition amount of octamethylcyclotetrasiloxane, silane coupling agent, crosslinking agent and acrylate in the core-shell toughening agent, a stable and uniform core-shell structure is formed. Experiments show that when the added weight ratio of octamethylcyclotetrasiloxane, silane coupling agent, crosslinking agent and acrylate is 10-12:1:1-3:6-8, the toughening agent obtained has the best toughening effect. The selection of curing agent also has an important influence on the performance of epoxy adhesive. This application selects aromatic amine curing agent containing ether bonds as the curing agent of epoxy adhesive. This curing agent can reduce the crosslinking density and improve the flexibility of the molecular chain. After the epoxy adhesive is cured, the flexible segment of the curing agent will naturally bond to the three-dimensional crosslinking network of the adhesive system, thereby improving the flexibility of the molecule and causing the structure of the adhesive to produce plastic deformation. In addition, the flexible segment will also produce a microscopic phase separation structure in the resin system, and cooperate with the core-shell toughening agent to alleviate the stress concentration phenomenon in the epoxy resin, further improving the toughness of the epoxy adhesive. The selection of acrylate monomers also has an important influence on the performance of the core-shell toughening agent. This application selects any one of methyl methacrylate, methyl acrylate or ethyl acrylate as an acrylate monomer to form the shell structure of the toughening agent. These monomers have better compatibility with epoxy resin and can ensure that the toughening agent is uniformly dispersed in the epoxy resin matrix. When subjected to external forces, the toughening agent can effectively absorb and disperse energy to prevent the rapid expansion of cracks.
[0028] Source of raw materials Octamethylcyclotetrasiloxane was purchased from Jiangsu Runfeng Synthetic Technology Co., Ltd., CAS No. 556-67-2; Bisphenol F epoxy resin was purchased from Shandong Poly Chemical Co., Ltd., model DER351, viscosity 4500-6500 mPas; polyetheramine curing agent was purchased from Shandong Huaye Trading Co., Ltd., CAS No. 9046-10-0.
[0029] Preparation example of toughening agent Preparation Example 1 A core-shell toughening agent, the preparation of which comprises the following steps: (1) adding 30 g of deionized water, 0.5 g of dodecylbenzenesulfonic acid, and 20 g of octamethylcyclotetrasiloxane, stirring and emulsifying for 20 min, heating to 70° C. for reaction for 4 h, and dropping 2 g of a crosslinking agent and 2 g of a silane coupling agent having a vinyl terminal group, stirring and reacting to obtain a vinyl-modified silicone emulsion; (2) Add 18g of methyl acrylate and 0.15g of potassium persulfate to the above vinyl modified silicone emulsion, stir and react for 2.5h, cool to room temperature to obtain a core-shell toughening agent, add 10% CaCl2 aqueous solution to stir and demulsify, filter, wash and dry to finally obtain a powdered core-shell toughening agent. The crosslinking agent is 1,4-butanediol diacrylate, and the silane coupling agent is vinyl triethoxysilane.
[0030] Preparation Example 2 A core-shell toughening agent, the preparation of which comprises the following steps: (1) adding 30 g of deionized water, 0.5 g of dodecylbenzenesulfonic acid, and 24 g of octamethylcyclotetrasiloxane, stirring and emulsifying for 30 min, heating to 60° C. for reaction for 4 h, and dropping 6 g of a crosslinking agent and 2 g of a silane coupling agent having a vinyl terminal group, stirring and reacting to obtain a vinyl-modified silicone emulsion; (2) Add 20g of ethyl acrylate and 0.15g of potassium persulfate to the above vinyl modified silicone emulsion, stir and react for 2h, cool to room temperature to obtain a core-shell toughening agent, add 10% CaCl2 aqueous solution and stir to break the emulsion, filter, wash and dry to finally obtain a powdered core-shell toughening agent. The crosslinking agent is 1,4-butanediol diacrylate, and the silane coupling agent is vinyl triethoxysilane.
[0031] Preparation Example 3 A core-shell toughening agent, the preparation of which comprises the following steps: (1) adding 30 g of deionized water, 0.5 g of dodecylbenzenesulfonic acid, and 22 g of octamethylcyclotetrasiloxane, stirring and emulsifying for 25 min, heating to 80° C. for reaction for 4 h, and dropping 4 g of a crosslinking agent and 2 g of a silane coupling agent having a vinyl terminal group, stirring and reacting to obtain a vinyl-modified silicone emulsion; (2) Add 16g of methyl methacrylate and 0.15g of potassium persulfate to the above vinyl modified silicone emulsion, stir and react for 3h, cool to room temperature to obtain a core-shell toughening agent, add 10% CaCl2 aqueous solution and stir to break the emulsion, filter, wash and dry to finally obtain a powdered core-shell toughening agent. The crosslinking agent is 1,4-butanediol diacrylate, and the silane coupling agent is vinyl triethoxysilane.
[0032] Preparation Example 4 A core-shell toughening agent, which is different from Example 1 in that the crosslinking agent added in this preparation example is divinylbenzene.
[0033] Preparation Example 5 A core-shell toughening agent, which is different from Example 1 in that the acrylate added in this preparation example is butyl acrylate.
[0034] Table 1 Raw materials and their weights in Preparation Examples 1-3 (g) Preparation example of curing agent Preparation Example 6 A curing agent, the preparation of which comprises the following steps: Take 20g of 4,4'-diaminodiphenylmethane (aromatic amine curing agent) and heat it to 85°C to melt it into liquid state, then add it to 30g of toluene solution and stir it. At the same time, add 16g of polyetheramine curing agent and stir and mix it evenly at a speed of 500r / min to obtain the curing agent.
[0035] Preparation Example 7 A curing agent, the preparation of which comprises the following steps: Take 20g of 4,4'-diaminodiphenylmethane (aromatic amine curing agent) and heat it to 85°C to melt it into liquid state, then add it to 30g of toluene solution and stir it. At the same time, add 24g of polyetheramine curing agent and stir and mix it evenly at a speed of 500r / min to obtain the curing agent. Example
[0036] Example 1 An epoxy adhesive, the preparation of which comprises the following steps: Weigh 90g of epoxy resin and 6g of toughening agent, stir and mix at 800r / min for 10min, ultrasonically mix, cool to room temperature, add 14g of curing agent, 3g of cobalt cyclopentaneate (accelerator) and 7.5g of dibutyl phthalate (diluent), mix evenly to obtain the epoxy adhesive; the toughening agent is the toughening agent prepared in Preparation Example 1, the epoxy resin is bisphenol F epoxy resin, model DER351, and the curing agent is the curing agent prepared in Preparation Example 6.
[0037] Example 2 An epoxy adhesive, the preparation of which comprises the following steps: Weigh 95g of epoxy resin and 12g of toughening agent, stir and mix at 800r / min for 10min, ultrasonically mix, cool to room temperature, add 12g of polyetheramine curing agent (curing agent), 0.5g of cobalt cyclopentaneate (accelerator) and 5g of dibutyl phthalate (diluent), mix evenly to obtain the epoxy adhesive; the toughening agent is the toughening agent prepared in Preparation Example 1, the epoxy resin is bisphenol F epoxy resin, model DER351, and the curing agent is the curing agent prepared in Preparation Example 7.
[0038] Example 3 An epoxy adhesive, the preparation of which comprises the following steps: Weigh 100g of epoxy resin and 9g of toughening agent, stir and mix at 800r / min for 10min, ultrasonically mix, cool to room temperature, add 16g of polyetheramine curing agent (curing agent), 5g of cobalt cyclopentaneate (accelerator) and 10g of dibutyl phthalate (diluent), mix evenly to obtain the epoxy adhesive; the toughening agent is the toughening agent prepared in Preparation Example 1, the epoxy resin is bisphenol F epoxy resin, model DER351, and the curing agent is the curing agent prepared in Preparation Example 6.
[0039] Table 2 Raw materials and their weights in Examples 1-3 (g) Example 1 Example 2 Example 3 Epoxy resin 90 95 100 Toughening agent 6 12 9 Curing agent 14 12 16 Accelerator 3 0.5 5 Thinner 7.5 5 10 Example 4 An epoxy adhesive, which is different from Example 1 in that the toughening agent used in this example is prepared in Preparation Example 2.
[0040] Example 5 An epoxy adhesive, which is different from Example 1 in that the toughening agent used in this example is prepared in Preparation Example 3.
[0041] Example 6 An epoxy adhesive, which is different from Example 1 in that the toughening agent used in this example is prepared in Preparation Example 4.
[0042] Example 7 An epoxy adhesive, which is different from Example 1 in that the toughening agent used in this example is prepared in Preparation Example 5.
[0043] Example 8 An epoxy adhesive, which is different from Example 1 in that the curing agent used in this example is 2-ethyl-4-methylimidazole.
[0044] Example 9 An epoxy adhesive, which is different from Example 1 in that the curing agent used in this example is 4,4'-diaminodiphenylmethane.
[0045] Example 10 An epoxy adhesive, which is different from Example 1 in that the curing agent used in this example is a polyetheramine curing agent.
[0046] Embodiment 11 An epoxy adhesive, which is different from Example 1 in that the accelerator used in this example is cobalt stearate.
[0047] Example 12 An epoxy adhesive, which is different from Example 1 in that the accelerator used in this example is sodium acetate.
[0048] Comparative Example Comparative Example 1 An epoxy adhesive, which is different from Example 1 in that the toughening agent added in this comparative example is a polymer polyol, model PL1850G.
[0049] Comparative Example 2 An epoxy adhesive, which is different from Example 1 in that no toughening agent is added in this comparative example, and the preparation comprises the following steps: 90 g of epoxy resin was weighed and stirred at 800 r / min for 10 min, ultrasonicated, and cooled to room temperature. Then, 14 g of amino-terminated polybisphenol A ether benzophenone (curing agent), 3 g of cobalt cyclohexaneate (accelerator) and 7.5 g of dibutyl phthalate (diluent) were added and mixed evenly to obtain the epoxy adhesive; the toughening agent was the toughening agent prepared in Preparation Example 1, and the epoxy resin was bisphenol F epoxy resin, model DER351.
[0050] Comparative Example 3 An epoxy adhesive, which is different from Example 1 in that no toughening agent is added in this comparative example, and octamethylcyclotetrasiloxane and methyl acrylate are added respectively, and the preparation comprises the following steps: 90 g of epoxy resin, 3.75 g of octamethylcyclotetrasiloxane and 2.25 g of methyl acrylate were weighed and stirred at a speed of 800 r / min for 10 min, and ultrasonic mixing was continued. After cooling to room temperature, 14 g of amino-terminated polybisphenol A ether benzophenone (curing agent), 3 g of cobalt cyclohexaneate (accelerator) and 7.5 g of dibutyl phthalate (diluent) were added and mixed evenly to obtain the epoxy adhesive; the epoxy resin was bisphenol F epoxy resin, model DER351.
[0051] Performance testing Detection method / test method Shear strength test: Test according to the test method shown in GB / T 7124-2008 "Determination of tensile shear strength of adhesives"; Impact strength: Tested according to the method shown in GB / T 2567-2008 "Resin Casting" 5.4 Simply supported beam impact toughness test (sample size 80mm×10mm×4mm, 5 parallel tests to take the average value).
[0052] Table 3 Test results Combining Examples 1-3 and Comparative Example 1 and Table 3, it can be seen that all the data of Example 1 are better than those of Comparative Example 1, indicating that when the toughening agent prepared by the present application is added to the epoxy adhesive system, its core-shell structure can be fully utilized, and a complete "sea-island" phase separation structure is formed after curing to prevent further diffusion of cracks. At the same time, the flexible chain segments inside it can act as stress concentrators to further improve the toughness and impact resistance of the adhesive, and its toughening effect is better than that of ordinary toughening agents.
[0053] It can be seen from the combination of Examples 1-3 and Comparative Examples 2-3 and Table 3 that the various data of Example 1 are better than those of Comparative Examples 2-3, indicating that the adhesive prepared in the present application has good impact resistance. The unique core-shell structure of the toughening agent added thereto has a shell structure with good compatibility with the adhesive on the one hand, and a core structure with long flexible segments on the other hand, which work together to improve the toughness and impact strength of the adhesive.
[0054] Combining Examples 1-6 and Table 3, it can be seen that the various data of Examples 1-5 are better than those of Example 6, indicating that the addition of the cross-linking agent affects the performance of the toughening agent obtained, thereby affecting the performance of the epoxy adhesive. 1,4-Butanediol diacrylate is selected as the cross-linking agent. Its molecular structure contains two unsaturated bonds, which effectively cross-link the core-shell polymer molecular chains and quickly form a cross-linked structure, thereby obtaining an adhesive with good toughness and high impact strength.
[0055] Combining Example 1 with Example 7 and Table 3, it can be seen that the various test data of Example 1 are better than those of Example 7, indicating that selecting an acrylate with better compatibility with the epoxy resin to form a shell structure can promote the uniform dispersion of the toughening agent in the epoxy resin, thereby better absorbing external forces and improving the toughness of the adhesive.
[0056] Combining Example 1 with Examples 8-10 and Table 3, it can be seen that the various test data of Example 1 are better than those of Examples 8-10, indicating that selecting aromatic amine curing agent and polyether amine curing agent in a certain proportion and adding them to the epoxy adhesive as curing agent can further improve the flexibility of the epoxy molecular chain and improve the toughness of the epoxy adhesive. At the same time, it can cooperate with the core-shell toughening agent to further alleviate the stress concentration in the epoxy resin and prevent brittle fracture.
[0057] Combining Example 1 with Examples 11-12 and Table 3, it can be seen that the test data of Example 1 and Example 11 are better than those of Example 12, indicating that selecting a suitable accelerator can promote the reaction between the curing agent and the epoxy resin, making the generated polymer network more stable, thereby improving the impact resistance of the adhesive network.
[0058] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed. However, as long as it is within the scope of the claims of the present application, it shall be protected by the patent law.
Claims
1. An epoxy adhesive, characterized in that: The composition comprises the following raw materials in parts by weight: 90-100 parts of epoxy resin, 12-16 parts of curing agent, 0.5-5 parts of accelerator, 5-10 parts of diluent, and 6-12 parts of toughening agent, wherein the toughening agent is a core-shell toughening agent prepared by emulsion polymerization using octamethylcyclotetrasiloxane and acrylate as monomers.
2. The epoxy adhesive according to claim 1, characterized in that: The preparation of the core-shell toughening agent comprises the following steps: (1) After adding deionized water, dodecylbenzenesulfonic acid and octamethylcyclotetrasiloxane and stirring and emulsifying for 20-30 minutes, the temperature is raised to 60-80°C and reacted for 2-4 hours, and a crosslinking agent and a silane coupling agent with a vinyl terminal group are added dropwise and stirred to react to obtain a vinyl-modified silicone emulsion; (2) Add acrylate and potassium persulfate to the above vinyl modified silicone emulsion, stir and react for 2-3 hours, cool to room temperature to obtain a core-shell toughening agent emulsion, and then demulsify, filter, wash and dry to obtain a powdered core-shell toughening agent.
3. The epoxy adhesive according to claim 2, characterized in that: The weight ratio of octamethylcyclotetrasiloxane, silane coupling agent, crosslinking agent and acrylate in the core-shell toughening agent is 10-12:1:1-3:8-10.
4. The epoxy adhesive according to claim 1, characterized in that: The crosslinking agent is 1,4-butanediol diacrylate.
5. The epoxy adhesive according to claim 1, characterized in that: The acrylic acid ester is any one of methyl methacrylate, methyl acrylate or ethyl acrylate.
6. The epoxy adhesive according to claim 1, characterized in that: The curing agent is obtained by mixing an aromatic amine curing agent and a polyether amine curing agent in a ratio of 1:0.8-1.
2.
7. The epoxy adhesive according to claim 1, characterized in that: The accelerator is any one of cobalt naphthenate or cobalt stearate.
8. A method for preparing the epoxy adhesive according to any one of claims 1 to 7, characterized in that: The method comprises the following preparation steps: A certain amount of epoxy resin and toughening agent are weighed, stirred evenly, and ultrasonically mixed. After cooling to room temperature, a curing agent, an accelerator, and a diluent are added and mixed evenly to obtain the epoxy adhesive.