Hot-melt acrylate-PUR pressure-sensitive adhesive and preparation method thereof

Through the combination of polymerization reaction and polyol and resin, a hot melt acrylate-PUR pressure-sensitive adhesive without solvent residue was prepared, which solved the problem of solvent residue, achieved efficient and environmentally friendly pressure-sensitive adhesive production, and had excellent adhesion properties and widely used.

CN118931454APending Publication Date: 2024-11-12WUXI BOJIN POLYMER RES & DEV CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410824631.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-25
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing hot melt acrylate-PUR pressure-sensitive adhesives have solvent residue problems during the production process, which is difficult to meet the market demand for environmentally friendly and efficient production.

Method used

The polymerization reaction is carried out using HD-29 plasticizer, methyl methacrylate, butyl methacrylate, functional monomer hydroxyethyl methacrylate and azobisisobutyronitrile to form a pressure-sensitive adhesive intermediate, and through The reaction of polyether polyol, crystalline polyester resin and isocyanate was prepared to prepare a hot melt acrylate-PUR pressure-sensitive adhesive without solvent residue.

Benefits of technology

The preparation of hot melt acrylate-PUR pressure-sensitive adhesive without solvent residue is achieved, with excellent adhesion properties, weather resistance and environmental protection, and is suitable for a variety of application scenarios, especially in the manufacturing of electronic equipment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004910112760000051
    Figure BDA0004910112760000051
  • Figure BDA0004910112760000061
    Figure BDA0004910112760000061
Patent Text Reader

Abstract

The invention relates to the technical field of hot-melt acrylate-PUR pressure-sensitive adhesives, in particular to a hot-melt acrylate-PUR pressure-sensitive adhesive which comprises a mixture of a pressure-sensitive adhesive intermediate, crystalline polyester resin, polyether polyol and isocyanate, and the hot-melt acrylate-PUR pressure-sensitive adhesive comprises the following raw material components in parts by weight: 1-5 parts of a curing agent, 1-5 parts of a curing agent and 1-5 parts of a curing agent. The pressure-sensitive adhesive is prepared from the following components in parts by weight: 20 to 90 parts of pressure-sensitive adhesive intermediate, 5 to 45 parts of crystalline polyester resin, 20 to 50 parts of polyether polyol, 5 to 25 parts of petroleum resin, 1 to 10 parts of isocyanate (MDI-100) and 0.1 to 1 part of I rganox1076 antioxidant. The pressure-sensitive adhesive intermediate is used as a main raw material, and the reactive hot-melt pressure-sensitive adhesive is synthesized together with crystalline polyester resin, polyether polyol and isocyanate. The synthesized pressure-sensitive adhesive can be directly used without any solvent residue.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of hot-melt acrylate-PUR pressure-sensitive adhesives, and in particular relates to a hot-melt acrylate-PUR pressure-sensitive adhesive and a preparation method thereof. Background Art

[0002] Acrylic pressure-sensitive adhesive is a soft polymer material that has long-lasting adhesion at room temperature. It can adhere to the surface of the adherend through non-covalent bonds under light pressure and leaves no residue after being peeled off.

[0003] There are many types of acrylic pressure-sensitive adhesives, including solvent-based, emulsion-based, hot-melt-based and radiation-curable types. Among them, solvent-based acrylic pressure-sensitive adhesives are widely used in pressure-sensitive labels and various forms of tapes due to their advantages such as low average relative molecular weight, good wettability, fast drying, high initial adhesion and good water resistance.

[0004] PUR pressure-sensitive adhesive has excellent adhesion, weather resistance, chemical resistance and high temperature resistance. Compared with acrylic pressure-sensitive adhesive, PUR pressure-sensitive adhesive has excellent performance in adhesion, weather resistance and chemical resistance, so it is widely used in some special fields such as automobile, electronics, aviation and other industries.

[0005] Combining the technologies of acrylic pressure-sensitive adhesive and PUR pressure-sensitive adhesive can form acrylate-PUR pressure-sensitive adhesive. This new type of pressure-sensitive adhesive not only retains the softness and easy processing characteristics of acrylic pressure-sensitive adhesive, but also enhances the adhesion and weather resistance of PUR pressure-sensitive adhesive. Therefore, acrylate-PUR pressure-sensitive adhesive shows broad application prospects in many fields.

[0006] With the continuous advancement of science and technology and the increasing demand for environmentally friendly, efficient and high-performance pressure-sensitive adhesives, the technology of acrylate-PUR pressure-sensitive adhesives is also constantly developing and improving. In the future, acrylate-PUR pressure-sensitive adhesives may pay more attention to research on environmental protection, energy saving and efficient production to meet the ever-changing market and demand. Therefore, a hot-melt acrylate-PUR pressure-sensitive adhesive and its preparation method are needed to solve the above problems. Summary of the invention

[0007] In order to solve the above technical problems, the present invention provides a hot melt acrylate-PUR pressure sensitive adhesive and a preparation method thereof. The purpose of the present invention is to provide a technology and process for hot melt acrylate-PUR pressure sensitive adhesive. First, HD-29 plasticizer is used as a polymerization carrier, methyl methacrylate, butyl methacrylate, and functional monomer hydroxyethyl methacrylate are used as polymerization monomers, and azobisisobutyronitrile is used as an initiator. The above monomer mixture is added dropwise to a polymerization reactor at 100 degrees Celsius within 4 hours to complete the polymerization reaction. This pressure sensitive adhesive intermediate contains a hydroxyl functional group. The hot melt acrylate-PUR pressure sensitive adhesive is synthesized by reacting this pressure sensitive adhesive intermediate with polyether polyol, crystalline polyester polyol, petroleum resin or rosin resin, and isocyanate. The synthesized pressure sensitive adhesive of the present invention can be used directly without any solvent residue to solve the problems in the existing market raised in the above background technology.

[0008] To achieve the above object, the technical solution of the present invention is as follows:

[0009] A hot-melt acrylate-PUR pressure-sensitive adhesive, comprising:

[0010] The hot melt acrylate-PUR pressure sensitive adhesive comprises a mixture of a pressure sensitive adhesive intermediate, a crystalline polyester resin, a polyether polyol, and an isocyanate, and comprises the following raw material components in parts by weight, wherein:

[0011] 20-90 parts of pressure-sensitive adhesive intermediate, 5-45 parts of crystalline polyester resin, 20-50 parts of polyether polyol, 5-25 parts of petroleum resin, 1-10 parts of isocyanate (MDI-100), and 0.1-1 part of Irganox1076 antioxidant.

[0012] As a preferred embodiment of the present invention, the raw materials include the following components by weight: 50 parts of pressure-sensitive adhesive intermediate, 24 parts of polyether polyol (PPG2000), 20 parts of petroleum resin (TH100), 5.7 parts of isocyanate (MDI-100), and 0.3 parts of antioxidant (Irganox 1076).

[0013] As a preferred embodiment of the present invention, the raw materials include the following components by weight: 70 parts of pressure-sensitive adhesive intermediate, 25.7 parts of crystalline polyester resin (Dynacoll 7360), 4 parts of isocyanate (MDI-100), and 0.3 parts of antioxidant (Irganox 1076).

[0014] As a preferred embodiment of the present invention, the raw materials include the following components by weight: 80 parts of pressure-sensitive adhesive intermediate, 10 parts of crystalline polyester resin (Dynacoll 7360), 8 parts of petroleum resin (TH100), 1.7 parts of isocyanate (MDI-100), and 0.3 parts of antioxidant (Irganox 1076).

[0015] As a preferred embodiment of the present invention, the raw materials include the following components by weight: 30 parts of pressure-sensitive adhesive intermediate, 41 parts of polyether polyol (PPG4000), 20 parts of petroleum resin (TH100), 8.7 parts of isocyanate (MDI-100), and 0.3 parts of antioxidant (Irganox 1076).

[0016] As a preferred embodiment of the present invention, the raw materials include the following components by weight: 40 parts of pressure-sensitive adhesive intermediate, 41 parts of crystalline polyester resin (Dynacoll 7361), 12 parts of petroleum resin (TH100), 6.7 parts of isocyanate (MDI-100), and 0.3 parts of antioxidant (Irganox 1076).

[0017] As a preferred embodiment of the present invention, the pressure-sensitive adhesive intermediate comprises a mixture of a polymer carrier, a polymer monomer and an initiator.

[0018] A method for preparing a hot-melt acrylate-PUR pressure-sensitive adhesive comprises the following steps:

[0019] s1. Add pressure-sensitive adhesive intermediate, polyether polyol, crystalline polyester resin, petroleum resin and TH100 antioxidant into a reaction container;

[0020] s2. Add nitrogen into the reaction vessel and heat to 120 degrees Celsius for mixing and stirring;

[0021] s3, vacuum drying the mixture in step s2 for 30 minutes;

[0022] s4, adding isocyanate MDI-100 into the reaction container in step s3;

[0023] s5. The reaction vessel in step s4 is heated to 120 degrees Celsius for reaction for 2 hours, and then vacuum degassing is performed again.

[0024] Compared with the prior art, the present invention has the following beneficial effects:

[0025] Acrylic-PUR pressure-sensitive adhesive (Polyurethane Reinforced Acrylic Pressure Sensitive Adhesive) has demonstrated its unique advantages in many aspects.

[0026] Excellent adhesion performance: Acrylate-PUR pressure-sensitive adhesive exhibits strong adhesion to a variety of substrates, which is mainly due to the increase in PUR components. After special treatment, the pressure-sensitive adhesive can form a strong viscosity, allowing it to form a good connection between the items to be attached.

[0027] Good weather resistance and durability: Acrylate-PUR pressure-sensitive adhesive has excellent water resistance, moisture resistance, high temperature resistance and low temperature resistance. This pressure-sensitive adhesive can still maintain stable performance in harsh environments such as high temperature and high humidity, and is not easy to age or deteriorate.

[0028] Adjustable performance: The performance of acrylate-PUR pressure-sensitive adhesive can be appropriately adjusted according to user needs. This allows it to perform optimally in different application scenarios and meet the actual needs of different users.

[0029] Environmental protection: The emulsion type acrylic ester-PUR pressure sensitive adhesive has a high solid content and low viscosity, which reduces the amount of glue used to a certain extent. Compared with traditional glue, this pressure sensitive adhesive has extremely low volatile organic compound emissions and is more in line with environmental protection requirements.

[0030] Strong coating adaptability: Acrylate-PUR pressure-sensitive adhesive shows good adaptability during the coating process and can be easily coated on various substrates.

[0031] Wide range of applications: Acrylate-PUR pressure-sensitive adhesive can be used to make various pressure-sensitive tapes, labels, etc., and is widely used in packaging, protection, insulation, warning, marking and other fields.

[0032] With the development of 5G consumer electronics, it is also playing an increasingly important role in the manufacturing of electronic equipment.

[0033] In summary, acrylate-PUR pressure-sensitive adhesive has become an important product in the pressure-sensitive adhesive market due to its excellent adhesion performance, weather resistance and durability, adjustable performance, environmental protection, strong coating adaptability and wide application fields. DETAILED DESCRIPTION

[0034] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0035] The present invention provides the following embodiments:

[0036] The first step is to prepare acrylic pressure-sensitive adhesive intermediates

[0037] 49.2 parts by weight of HD-29 plasticizer was added to the reactor, and the temperature was raised to 100 degrees Celsius under a nitrogen atmosphere. 21.43 parts by weight of methyl methacrylate, 28.07 parts by weight of butyl methacrylate, 0.6 parts by weight of hydroxyethyl methacrylate and 0.5 parts by weight of azobisisobutyronitrile were added to the monomer mixing kettle, mixed evenly and then added dropwise to the above reactor. The addition time was 4 hours. After the addition was completed, the temperature was kept at 120 degrees Celsius for 1 hour, and then 0.3 parts by weight of antioxidant irganox 1076 was added. In the later stage of the reaction, an initiator was appropriately added to obtain a transparent viscous semi-solid pressure-sensitive adhesive with a residual monomer content of less than 0.2%.

[0038] Step 2: Preparation of acrylate-PUR pressure-sensitive adhesive

[0039] Embodiment 1:

[0040] Add 50 parts by weight of the intermediate, 24 parts by weight of polyether polyol PPG2000, 12 parts by weight of petroleum resin TH100, and 0.3 parts by weight of antioxidant Irganox1076 into a reaction container, mix under nitrogen protection, heat to 120 degrees Celsius, and vacuum dry for 30 minutes. Then, add 5.7 parts by weight of isocyanate MDI-100 into the reaction container at one time, react at 120 degrees Celsius for 2 hours, and vacuum degas again for standby use.

[0041] Embodiment 2:

[0042] 70 parts by weight of the intermediate, 25.7 parts by weight of the crystalline polyester resin Dynacoll7360, and 0.3 parts by weight of the antioxidant Irganox1076 were added to the reaction container, mixed under nitrogen protection and heated to 120 degrees Celsius. After vacuum drying for 30 minutes, 4.0 parts by weight of isocyanate MDI-100 were added to the reaction container at one time, reacted at 120 degrees Celsius for 2 hours, and vacuum degassed again for standby use.

[0043] Embodiment 3:

[0044] Add 80 parts by weight of the intermediate, 10 parts by weight of crystalline polyester resin Dynacoll7360, 8 parts by weight of petroleum resin TH100, and 0.3 parts by weight of antioxidant Irganox1076 into a reaction container, mix and heat to 120 degrees Celsius under nitrogen protection, vacuum dry for 30 minutes, then add 1.7 parts by weight of isocyanate MDI-100 into the reaction container at one time, react at 120 degrees Celsius for 2 hours, and vacuum degas again for standby use.

[0045] Embodiment 4:

[0046] Add 30 parts by weight of the intermediate, 41 parts by weight of polyether polyol PPG2000, 20 parts by weight of petroleum resin TH100, and 0.3 parts by weight of antioxidant Irganox1076 into a reaction container, mix under nitrogen protection, heat to 120 degrees Celsius, and vacuum dry for 30 minutes. Then, add 8.7 parts by weight of isocyanate MDI-100 into the reaction container at one time, react at 120 degrees Celsius for 2 hours, and vacuum degas again for standby use.

[0047] Embodiment 5:

[0048] 40 parts of pressure-sensitive adhesive intermediate, 41 parts of crystalline polyester resin (Dynacoll 7361), 12 parts of petroleum resin (TH100), 6.7 parts of isocyanate (MDI-100), and 0.3 parts of antioxidant (Irganox 1076).

[0049] Add 40 parts by weight of the intermediate, 41 parts by weight of the crystalline polyester resin Dynacoll7361, 12 parts by weight of the petroleum resin TH100, and 0.3 parts by weight of the antioxidant Irganox1076 into a reaction container, mix under nitrogen protection, heat to 120 degrees Celsius, and vacuum dry for 30 minutes. Then, add 6.7 parts by weight of isocyanate MDI-100 into the reaction container at one time, react at 120 degrees Celsius for 2 hours, and vacuum degas again for standby use.

[0050] The performance indicators of the above embodiment are shown in Table 1

[0051]

[0052] The glass bonding performance test data of the above embodiment is shown in Table 2

[0053] Table 2 Performance test results (test sample width 25.4mm, tensile speed 50mm / min, glass adhesion)

[0054]

[0055] The above data show that the pressure-sensitive adhesive of the present invention has good bonding performance to glass between -20 degrees Celsius and 35 degrees Celsius.

[0056] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A hot melt acrylate-PUR pressure sensitive adhesive, characterized in that ,include: The hot melt acrylate-PUR pressure sensitive adhesive comprises a mixture of a pressure sensitive adhesive intermediate, a crystalline polyester resin, a polyether polyol, and an isocyanate, and comprises the following raw material components in parts by weight, wherein: 20-90 parts of pressure-sensitive adhesive intermediate, 5-45 parts of crystalline polyester resin, 20-50 parts of polyether polyol, 5-25 parts of petroleum resin, 1-10 parts of isocyanate (MDI-100), and 0.1-1 part of Irganox1076 antioxidant.

2. The hot melt acrylate-PUR pressure sensitive adhesive according to claim 1, characterized in that: The raw materials include the following components by weight: 50 parts of pressure-sensitive adhesive intermediate, 24 parts of polyether polyol (PPG2000), 20 parts of petroleum resin (TH100), 5.7 parts of isocyanate (MDI-100), and 0.3 parts of antioxidant (Irganox 1076).

3. The hot melt acrylate-PUR pressure sensitive adhesive according to claim 1, characterized in that: The raw materials include the following components by weight: 70 parts of pressure-sensitive adhesive intermediate, 25.7 parts of crystalline polyester resin (Dynacoll 7360), 4 parts of isocyanate (MDI-100), and 0.3 parts of antioxidant (Irganox1076).

4. The hot melt acrylate-PUR pressure sensitive adhesive according to claim 1, characterized in that: The raw materials include the following components by weight: 80 parts of pressure-sensitive adhesive intermediate, 10 parts of crystalline polyester resin (Dynacol l 7360), 8 parts of petroleum resin (TH100), 1.7 parts of isocyanate (MDI-100), and 0.3 parts of antioxidant (Irganox 1076).

5. The hot melt acrylate-PUR pressure sensitive adhesive according to claim 1, characterized in that: The raw materials include the following components by weight: 30 parts of pressure-sensitive adhesive intermediate, 41 parts of polyether polyol (PPG4000), 20 parts of petroleum resin (TH100), 8.7 parts of isocyanate (MDI-100), and 0.3 parts of antioxidant (Irganox 1076).

6. The hot melt acrylate-PUR pressure sensitive adhesive according to claim 1, characterized in that: The raw materials include the following components by weight: 40 parts of pressure-sensitive adhesive intermediate, 41 parts of crystalline polyester resin (Dynacol l 7361), 12 parts of petroleum resin (TH100), 6.7 parts of isocyanate (MDI-100), and 0.3 parts of antioxidant (Irganox 1076).

7. The hot melt acrylate-PUR pressure sensitive adhesive according to claim 1, characterized in that: The pressure-sensitive adhesive intermediate comprises a mixture of a polymer carrier, a polymer monomer and an initiator.

8. A method for preparing a hot melt acrylate-PUR pressure sensitive adhesive, according to the hot melt acrylate-PUR pressure sensitive adhesive according to claims 1-7, characterized in that: The steps include: s1. Adding a pressure-sensitive adhesive intermediate, polyether polyol, crystalline polyester resin, petroleum resin and antioxidant into a reaction container; s2. Add nitrogen into the reaction vessel and heat to 120 degrees Celsius for mixing and stirring; s3, vacuum drying the mixture in step s2 for 30 minutes; s4, adding isocyanate MDI-100 into the reaction container in step s3; s5. The reaction vessel in step s4 is heated to 120 degrees Celsius for reaction for 2 hours, and then vacuum degassing is performed again.