Preparation method of sprayable polyurethane adhesive

The sprayable polyurethane adhesive, prepared through specific components and processes, solves the problems of aging under ultraviolet light and poor high-temperature resistance of polyurethane adhesives, achieving strong weather resistance, good high-temperature resistance, and strong stability.

CN118931459AInactive Publication Date: 2024-11-12SHANGHAI JINGTAN CHEM CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411150431.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing polyurethane adhesives are prone to aging and discoloration under strong ultraviolet radiation, have poor high-temperature resistance, short shelf life, and are inconvenient to use.

Method used

A prepolymer was synthesized under nitrogen protection using a specific ratio of diisocyanate, polyester polyol, catalyst, emulsifier, coupling agent, modifier, solvent, nano silica, plasticizer and flame retardant. After emulsification reaction, catalytic reaction, viscosity test and homogenization treatment, a sprayable polyurethane adhesive was prepared.

Benefits of technology

It improves the weather resistance, high temperature resistance, stability and ease of use of polyurethane adhesives, enhances the solubility and dispersibility of adhesives, and optimizes the construction effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118931459A_ABST
    Figure CN118931459A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a sprayable polyurethane adhesive, and relates to the technical field of high-temperature-resistant adhesives. Comprising the following components in parts by weight: 80-120 parts of diisocyanate, 50-120 parts of polyester polyol, 5-12 parts of a terminator, 5-13 parts of a catalyst, 5-10 parts of an emulsifier, 5-10 parts of a coupling agent, 6-12 parts of a modifier, 40-80 parts of a solvent and 65-125 parts of nano silicon dioxide, the preparation method comprises the following steps: synthesizing a prepolymer under the protection of nitrogen, modifying the prepolymer through the coupling agent and the modifier, adding the emulsifier for emulsification to prepare a pre-adhesive, adding the catalyst for catalysis, adding the terminator for polymerization termination, and finally homogenizing to uniformly mix the adhesive. The polyurethane adhesive has the advantages of strong weather resistance, good high temperature resistance, strong stability, long storage time and the like, can be sprayed for use after being modified by a modifier, and is more convenient and quicker.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of high temperature resistant adhesives, and in particular to a method for preparing a sprayable polyurethane adhesive. Background Art

[0002] With the progress of the times and the development of society, our demand for high-performance adhesives is also increasing. Therefore, the polyurethane adhesive market is also gradually expanding.

[0003] As the application of polyurethane adhesives becomes more and more extensive, our requirements for this adhesive are also getting higher and higher. The adhesives used need to meet the requirements of good weather resistance, strong high temperature resistance, stability, long shelf life, and easy use.

[0004] Although existing polyurethane adhesives have good performance at room temperature, their weather resistance is relatively limited. Especially in an environment with strong ultraviolet radiation, polyurethane adhesives are prone to aging, discoloration and performance degradation. At the same time, existing polyurethane adhesives have poor high temperature resistance and cannot be used in high temperature working environments. They have problems such as short shelf life and inconvenient use.

[0005] In view of the above technical defects, a solution is now proposed. Summary of the invention

[0006] The purpose of the present invention is to provide a method for preparing a sprayable polyurethane adhesive to solve the problems raised in the above background technology.

[0007] In order to achieve the above object, the present invention adopts the following technical scheme: a method for preparing a sprayable polyurethane adhesive, characterized in that, in parts by weight, the polyurethane adhesive comprises the following components: 80 to 120 parts by weight of diisocyanate, 50 to 120 parts by weight of polyester polyol, 5 to 12 parts by weight of terminator, 5 to 13 parts by weight of catalyst, 5 to 10 parts by weight of emulsifier, 5 to 11 parts by weight of inhibitor, 5 to 10 parts by weight of coupling agent, 6 to 12 parts by weight of modifier, 40 to 80 parts by weight of solvent, 65 to 125 parts by weight of nano silicon dioxide, 7 to 12 parts by weight of plasticizer and 7 to 12 parts by weight of flame retardant;

[0008] The diisocyanate is one or a mixture of two or more of 1,5-naphthalene diisocyanate, 1,4-cyclohexane diisocyanate, p-phenylene diisocyanate, and toluene diisocyanate;

[0009] The solvent is one or a mixture of two or more of N,N-dimethylformamide, toluene and butanone;

[0010] The preparation method of the polyurethane adhesive comprises:

[0011] Step 1, synthesizing prepolymer 1: adding p-phenylene diisocyanate, toluene diisocyanate, polyester polyol and nano-silicon dioxide in a reaction kettle according to a certain proportion, introducing nitrogen into the reaction kettle, and stirring the reaction materials while heating to prepare prepolymer 1;

[0012] Step 2, synthesizing prepolymer 2: observing prepolymer 1 in the reactor, when the prepolymer starts to produce water, stopping the introduction of nitrogen, and keeping the temperature for a period of time, then cooling the reactor, adding 1,5-naphthalene diisocyanate, 1,4-cyclohexane diisocyanate, and nano-silicon dioxide into the reactor in proportion while stirring, and keeping the temperature for a period of time to obtain prepolymer 2;

[0013] Step 3, modification and emulsification reaction: add prepolymer 2, coupling agent and modifier into a high-speed mixer in proportion, react fully, then add emulsifier into the high-speed mixer in proportion, mix and react fully to obtain pre-adhesive 1, and keep warm for a period of time;

[0014] Step 4, catalytic reaction: adding pre-adhesive agent 1 and catalyst into a reaction container in proportion, evacuating the reaction container, heating the reaction container, and keeping the temperature for a period of time to obtain pre-adhesive agent 2;

[0015] Step 5, test viscosity: preset the target viscosity, use a capillary viscometer to test the viscosity of the pre-adhesive, when the viscosity of the main agent reaches the target viscosity, add the terminator and stir thoroughly to obtain the pre-adhesive three;

[0016] Step 6, adding solvent: nitrogen is introduced into the reaction container, N, N-dimethylformamide, toluene and butanone are added in proportion while stirring, and the mixture is fully stirred and mixed to obtain pre-adhesive agent 4, and the introduction of nitrogen is stopped after keeping the mixture warm for a period of time;

[0017] Step 7, homogenization treatment: add plasticizer, flame retardant and polymerization inhibitor in proportion, keep them warm for a period of time, stir and mix them thoroughly to obtain pre-adhesive five, keep them warm for a period of time, pour the pre-adhesive five into a high-pressure homogenizer, perform homogenization treatment, obtain pre-adhesive six, filter and remove impurities from the pre-adhesive six, and obtain the desired adhesive.

[0018] Furthermore, in the step 1, the mass ratio of p-phenylene diisocyanate, toluene diisocyanate, polyester polyol and nano-silicon dioxide is 20-30:20-30:50-120:65-125, the reaction temperature for synthesizing prepolymer 1 is 50-60° C., and the pressure is 0.1-1.5 MPa.

[0019] Furthermore, in the step 2, the temperature in the reactor is raised to 220° C. to 300° C., the nitrogen is stopped, and the temperature is kept for 2 to 5 hours, and then the temperature of the reactor is lowered to 70 to 100° C., and then kept for 1 to 4 hours;

[0020] In the step 2, the mass ratio of 1,5-naphthalene diisocyanate, 1,4-cyclohexane diisocyanate and nano-silicon dioxide added is 100:1 to 100:0.5 to 50:0.1.

[0021] Furthermore, in the step 3, the mass ratio of the prepolymer 2, the coupling agent and the modifier is 100:1-20:0.1-20:0.1, the temperature of the modification reaction is 20-80°C, the reaction time is 2-10h, and the reaction pressure is 0.1-0.5MPa;

[0022] The emulsification reaction temperature is 20-60°C, the emulsification reaction time is 2-3h, and the emulsification reaction pressure is 0.1-0.15MPa;

[0023] In the step three, the modifier is aminosulfonic acid sodium salt, the coupling agent is 3-epoxypropyltriethoxysilane, and the emulsifier is polysorbate and polyoxyethylene.

[0024] Furthermore, in the step 4, the mass ratio of the pre-binder 1 to the catalyst is 100:0-10:0.5, the reaction container is heated to 200-260° C., the reaction pressure is 0.01-0.1 MPa, and the reaction time is 0.5-1 h.

[0025] Furthermore, the preset target viscosity in step 5 is 3000±500 centipoise, the temperature during the viscosity test in step 5 is 20-25°C, the test pressure is 0.1-1.5MPa, and the humidity during the test is maintained at 40-60%;

[0026] In the step 5, the terminator is triphenyl phosphate.

[0027] Furthermore, in step six, the mass ratio of N,N-dimethylformamide, toluene and butanone is 50:0.5-50:0.5-50:0.1, the reaction temperature is 55-70°C, and the insulation time is 1-3h.

[0028] Furthermore, in step seven, the mass ratio of the plasticizer, the flame retardant and the polymerization inhibitor is 10:0.1 to 10:0.1 to 11:0.2;

[0029] The plasticizer is polyethylene glycol, the reaction temperature of adding the plasticizer is 70-85°C, and the insulation time is 1-3h;

[0030] The flame retardant is melamine phosphate, the reaction temperature of adding the flame retardant is 80-95°C, and the heat preservation time is 0.5-2.5h;

[0031] The polymerization inhibitors are butylated hydroxytoluene and butylated hydroxyethylbenzene, the reaction temperature for adding the polymerization inhibitors is 100-125° C., and the heat preservation time is 1-1.5 hours.

[0032] Furthermore, in step seven, the speed of the homogenization reaction is 3000-3500 rpm, the pressure of the homogenization reaction is 1.5-5 MPa, the temperature of the homogenization reaction is 70-85° C., and the time of the homogenization reaction is 1-3.5 h.

[0033] In summary, due to the adoption of the above technical solution, the beneficial effects of the present invention are:

[0034] 1. The present invention synthesizes the prepolymer under nitrogen protection, which can isolate moisture and oxygen in the air, prevent moisture in the air from reacting with the active NCO group in the isocyanate molecule, hinder the polymerization reaction, and lead to unstable reaction process, local overheating, implosion and other phenomena, affecting production safety;

[0035] 2. The present invention uses a coupling agent and a modifier to modify the adhesive into a water-based adhesive, which can improve the adhesive's viscosity, water resistance, weather resistance and other properties, and can be directly sprayed for use, which is more convenient and quick;

[0036] 3. The present invention can make the polyurethane adhesive uniformly dispersed in water or other solvents through emulsification reaction, thereby improving the solubility, dispersibility and stability of the adhesive;

[0037] 4. The present invention can control the progress of the reaction by adding a terminator, thereby preventing the reaction from getting out of control due to excessive polymerization, and generating products with too large or too small molecular weight, which affects the performance of the polyurethane adhesive;

[0038] 5. The present invention can make the components in the adhesive evenly dispersed through homogenization reaction, thereby enhancing the stability of the adhesive itself, improving the curing quality, and optimizing the use effect, making the construction more convenient. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] Figure 1 The preparation flow chart of the present invention is shown. DETAILED DESCRIPTION

[0040] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0041] The invention discloses a preparation method of a sprayable polyurethane adhesive. The polyurethane adhesive comprises the following components: 80-120 parts by weight of diisocyanate, 50-120 parts by weight of polyester polyol, 5-12 parts by weight of terminator, 5-13 parts by weight of catalyst, 5-10 parts by weight of emulsifier, 5-11 parts by weight of polymerization inhibitor, 5-10 parts by weight of coupling agent, 6-12 parts by weight of modifier, 40-80 parts by weight of solvent, 65-125 parts by weight of nano silicon dioxide, 7-12 parts by weight of plasticizer and 7-12 parts by weight of flame retardant. The diisocyanate is one or a mixture of two or more of 1,5-naphthalene diisocyanate, 1,4-cyclohexane diisocyanate, p-phenylene diisocyanate and toluene diisocyanate, and the solvent is one or a mixture of two or more of N,N-dimethylformamide, toluene and butanone.

[0042] The preparation method of the polyurethane adhesive comprises:

[0043] Step 1, synthesizing prepolymer 1: adding p-phenylene diisocyanate, toluene diisocyanate, polyester polyol and nano-silicon dioxide in a reaction kettle according to a proportion, introducing nitrogen into the reaction kettle, stirring the reaction materials while heating, to prepare prepolymer 1, wherein the reaction temperature for synthesizing prepolymer 1 is 50-60° C. and the pressure is 0.1-1.5 MPa;

[0044] Step 2, synthesizing prepolymer 2: observe prepolymer 1 in the reactor, when the prepolymer starts to discharge water, heat the reactor to 220°C to 300°C, stop introducing nitrogen, and keep warm for 2 to 5 hours, then cool the reactor to 70 to 100°C, and keep warm for 1 to 4 hours, add 1,5-naphthalene diisocyanate, 1,4-cyclohexane diisocyanate, and nano-silicon dioxide into the reactor in proportion while stirring, and keep warm for a period of time to obtain prepolymer 2;

[0045] Step 3, modification and emulsification reaction: add prepolymer 2, coupling agent and modifier into a high-speed mixer in proportion, react for 2 to 10 hours under environmental conditions of temperature of 20 to 80° C. and pressure of 0.1 to 0.5 MPa, then add emulsifier into the high-speed mixer in proportion, react for 2 to 3 hours under environmental conditions of temperature of 20 to 60° C. and pressure of 0.1 to 0.15 MPa, to obtain pre-adhesive 1;

[0046] The modifier is sodium aminosulfonic acid, the coupling agent is 3-epoxypropyltriethoxysilane, and the emulsifier is polysorbate and polyoxyethylene;

[0047] Step 4, catalytic reaction: adding pre-adhesive agent 1 and catalyst into a reaction container in proportion, evacuating the reaction container, and heating the reaction container to 200-260° C., and keeping the temperature at a pressure of 0.01-0.1 MPa for 0.5-1 h to obtain pre-adhesive agent 2;

[0048] Step 5, testing viscosity: under the environmental conditions of temperature of 20-25°C, pressure of 0.1-1.5 MPa and relative humidity of 40-60%, use a capillary viscometer to test the viscosity of the pre-adhesive. When the viscosity of the main agent reaches 3000±500 centipoise, add the terminator and stir thoroughly to obtain the pre-adhesive three;

[0049] Wherein: the terminator is triphenyl phosphate;

[0050] Step 6, adding solvent: nitrogen is introduced into the reaction container, and N,N-dimethylformamide, toluene and butanone are added in proportion under a temperature environment of 55-70° C. while stirring, and the pre-adhesive agent 4 is prepared by stirring and mixing, and the introduction of nitrogen is stopped after keeping the temperature for 1-3 hours;

[0051] Step 7, homogenization treatment: add plasticizer, flame retardant and polymerization inhibitor in proportion, adjust the temperature to 70-85°C after adding plasticizer, keep warm for 1-3h, adjust the temperature to 80-95°C after adding flame retardant, keep warm for 0.5-2.5h, adjust the temperature to 100-125°C after adding polymerization inhibitor, keep warm for 1-1.5h, stir and mix thoroughly to obtain pre-adhesive 5;

[0052] Pour the pre-adhesive agent five into a high-pressure homogenizer for homogenization. The homogenization reaction speed is 3000-3500rpm, the homogenization reaction pressure is 1.5-5MPa, the homogenization reaction temperature is 70-85°C, and the homogenization reaction time is 1-3.5h to obtain the pre-adhesive agent six. Filter the pre-adhesive agent six to remove impurities and obtain the desired high temperature resistant adhesive.

[0053] Embodiment 1:

[0054] The invention provides a method for preparing a sprayable polyurethane adhesive. The components of the polyurethane adhesive in parts by weight of various raw materials are: 80 parts by weight of diisocyanate, 55 parts by weight of polyester polyol, 6 parts by weight of terminator, 7 parts by weight of catalyst, 6 parts by weight of emulsifier, 6 parts by weight of polymerization inhibitor, 7 parts by weight of coupling agent, 8 parts by weight of modifier, 60 parts by weight of solvent, 85 parts by weight of nano silicon dioxide, 9 parts by weight of plasticizer, and 9 parts by weight of flame retardant. The method for preparing the polyurethane adhesive comprises: firstly, synthesizing a prepolymer: under the environmental conditions of a temperature of 55° C. and a pressure of 0.15 MPa, adding p-phenylene diisocyanate, toluene diisocyanate, polyester polyol and nano silicon dioxide into a reaction kettle in proportion, and introducing into the reaction kettle; Nitrogen, heating and stirring the reaction raw materials to prepare prepolymer 1, observing the prepolymer 1 in the reactor, when the prepolymer starts to discharge water, raising the temperature in the reactor to 250°C, stopping the introduction of nitrogen, and keeping warm for 2.5 hours, then cooling the reactor to 75°C, and keeping warm for 2 hours, while stirring, adding 1,5-naphthalene diisocyanate, 1,4-cyclohexane diisocyanate, and nano-silica to the reactor in proportion, keeping warm for a period of time to prepare prepolymer 2, adding prepolymer 2, coupling agent and modifier in proportion to a high-speed mixer, reacting for 5 hours under the environmental conditions of temperature of 45°C and pressure of 0.1MPa, then adding emulsifier in proportion to the high-speed mixer, and under the environmental conditions of temperature of 30°C and pressure of 0.12MPa. The reaction was carried out under the following conditions for 2.2 hours to obtain pre-adhesive agent 1. Pre-adhesive agent 1 and catalyst were added to the reaction container in proportion, the reaction container was evacuated, and the reaction container was heated to 250°C. Under the environmental condition of 0.1 MPa, the temperature was kept for 0.5 hours to obtain pre-adhesive agent 2. The viscosity was tested: under the environmental condition of 23°C, 1 MPa and relative humidity of 55%, the viscosity of the pre-adhesive agent was tested using a capillary viscometer. When the viscosity of the main agent reached 3000±500 centipoise, a terminator was added and the mixture was stirred thoroughly to obtain pre-adhesive agent 3. Nitrogen was introduced into the reaction container. Under the temperature of 60°C, N,N-dimethylformamide, toluene and butanone were added in proportion while stirring, and the mixture was stirred thoroughly to obtain pre-adhesive agent 3. Pre-adhesive agent No. 4 is obtained. After keeping the mixture warm for 1.5 hours, the nitrogen gas is stopped from being introduced. Plasticizer, flame retardant and polymerization inhibitor are added in proportion. After adding the plasticizer, the temperature is adjusted to 75°C and the heat preservation time is 2 hours. After adding the flame retardant, the temperature is adjusted to 85°C and the heat preservation time is 1.5 hours. After adding the polymerization inhibitor, the temperature is adjusted to 110°C and the heat preservation time is 1.3 hours. The mixture is fully stirred to obtain pre-adhesive agent No. 5. The pre-adhesive agent No. 5 is poured into a high-pressure homogenizer for homogenization. The homogenization reaction speed is 3500 rpm, the homogenization reaction pressure is 1.9 MPa, the homogenization reaction temperature is 80°C, and the homogenization reaction time is 2 hours to obtain pre-adhesive agent No. 6. The pre-adhesive agent No. 6 is filtered to remove impurities to obtain the desired high temperature resistant adhesive.

[0055] Embodiment 2:

[0056] The invention provides a method for preparing a sprayable polyurethane adhesive. The components of the polyurethane adhesive in parts by weight of various raw materials are: 100 parts by weight of diisocyanate, 80 parts by weight of polyester polyol, 6 parts by weight of terminator, 7 parts by weight of catalyst, 6 parts by weight of emulsifier, 6 parts by weight of polymerization inhibitor, 7 parts by weight of coupling agent, 8 parts by weight of modifier, 60 parts by weight of solvent, 85 parts by weight of nano silicon dioxide, 9 parts by weight of plasticizer, and 9 parts by weight of flame retardant. The method for preparing the polyurethane adhesive comprises: firstly, synthesizing a prepolymer: under the environmental conditions of a temperature of 55° C. and a pressure of 0.15 MPa, adding p-phenylene diisocyanate, toluene diisocyanate, polyester polyol and nano silicon dioxide into a reaction kettle in proportion, and introducing into the reaction kettle; Nitrogen, heating and stirring the reaction raw materials to prepare prepolymer 1, observing the prepolymer 1 in the reactor, when the prepolymer starts to discharge water, raising the temperature in the reactor to 250°C, stopping the introduction of nitrogen, and keeping warm for 2.5 hours, then cooling the reactor to 75°C, and keeping warm for 2 hours, while stirring, adding 1,5-naphthalene diisocyanate, 1,4-cyclohexane diisocyanate, and nano-silica to the reactor in proportion, keeping warm for a period of time to prepare prepolymer 2, adding prepolymer 2, coupling agent and modifier in proportion to a high-speed mixer, reacting for 5 hours under the environmental conditions of temperature of 45°C and pressure of 0.1MPa, then adding emulsifier in proportion to the high-speed mixer, and under the environmental conditions of temperature of 30°C and pressure of 0.12MPa. The reaction was carried out under the following conditions for 2.2 hours to obtain pre-adhesive agent 1. Pre-adhesive agent 1 and catalyst were added to the reaction container in proportion, the reaction container was evacuated, and the reaction container was heated to 250°C. Under the environmental condition of 0.1 MPa, the temperature was kept for 0.5 hours to obtain pre-adhesive agent 2. The viscosity was tested: under the environmental condition of 23°C, 1 MPa and relative humidity of 55%, the viscosity of the pre-adhesive agent was tested using a capillary viscometer. When the viscosity of the main agent reached 3000±500 centipoise, a terminator was added and the mixture was stirred thoroughly to obtain pre-adhesive agent 3. Nitrogen was introduced into the reaction container. Under the temperature of 60°C, N,N-dimethylformamide, toluene and butanone were added in proportion while stirring, and the mixture was stirred thoroughly to obtain pre-adhesive agent 3. Pre-adhesive agent No. 4 is obtained. After keeping the mixture warm for 1.5 hours, the nitrogen gas is stopped from being introduced. Plasticizer, flame retardant and polymerization inhibitor are added in proportion. After adding the plasticizer, the temperature is adjusted to 75°C and the heat preservation time is 2 hours. After adding the flame retardant, the temperature is adjusted to 85°C and the heat preservation time is 1.5 hours. After adding the polymerization inhibitor, the temperature is adjusted to 110°C and the heat preservation time is 1.3 hours. The mixture is fully stirred to obtain pre-adhesive agent No. 5. The pre-adhesive agent No. 5 is poured into a high-pressure homogenizer for homogenization. The homogenization reaction speed is 3500 rpm, the homogenization reaction pressure is 1.9 MPa, the homogenization reaction temperature is 80°C, and the homogenization reaction time is 2 hours to obtain pre-adhesive agent No. 6. The pre-adhesive agent No. 6 is filtered to remove impurities to obtain the desired high temperature resistant adhesive.

[0057] Embodiment 3:

[0058] The invention provides a method for preparing a sprayable polyurethane adhesive. The components of the polyurethane adhesive in parts by weight of various raw materials are: 120 parts by weight of diisocyanate, 110 parts by weight of polyester polyol, 6 parts by weight of terminator, 7 parts by weight of catalyst, 6 parts by weight of emulsifier, 6 parts by weight of polymerization inhibitor, 7 parts by weight of coupling agent, 8 parts by weight of modifier, 60 parts by weight of solvent, 85 parts by weight of nano silicon dioxide, 9 parts by weight of plasticizer, and 9 parts by weight of flame retardant. The method for preparing the polyurethane adhesive comprises: firstly, synthesizing a prepolymer: under the environmental conditions of a temperature of 55°C and a pressure of 0.15MPa, adding p-phenylene diisocyanate, toluene diisocyanate, polyester polyol and nano silicon dioxide into a reaction kettle in proportion, and passing a stream of the mixture into the reaction kettle; Nitrogen was introduced, and the reaction raw materials were stirred while heating to prepare prepolymer 1. The prepolymer 1 in the reactor was observed. When the prepolymer began to discharge water, the temperature in the reactor was raised to 250°C, the nitrogen was stopped, and the temperature was kept for 2.5 hours. The reactor was then cooled to 75°C and kept for 2 hours. 1,5-naphthalene diisocyanate, 1,4-cyclohexane diisocyanate and nano-silica were added to the reactor in proportion while stirring. The prepolymer 2 was prepared by keeping the temperature for a period of time. Prepolymer 2, coupling agent and modifier were added to the high-speed mixer in proportion. The reaction was carried out under the environmental conditions of temperature of 45°C and pressure of 0.1MPa for 5 hours. The emulsifier was then added to the high-speed mixer in proportion. The temperature was kept at 30°C and pressure of 0.12MPa. Conditions: react for 2.2 hours to obtain pre-adhesive agent 1, add pre-adhesive agent 1 and catalyst into the reaction container in proportion, evacuate the reaction container, and heat the reaction container to 250°C at the same time. Keep it warm for 0.5 hours under the environmental condition of 0.1MPa pressure to obtain pre-adhesive agent 2. Test viscosity: use a capillary viscometer to test the viscosity of the pre-adhesive agent under the environmental condition of 23°C, 1MPa pressure and 55% relative humidity. When the viscosity of the main agent reaches 3000±500 centipoise, add the terminator and stir well to obtain pre-adhesive agent 3. Pass nitrogen into the reaction container, add N,N-dimethylformamide, toluene and butanone in proportion under the temperature of 60°C while stirring, and stir well to mix. Pre-adhesive agent No. 4 is prepared, and after keeping warm for 1.5 hours, the nitrogen is stopped from being introduced, and plasticizer, flame retardant and polymerization inhibitor are added in proportion in sequence. After adding the plasticizer, the temperature is adjusted to 75°C and the insulation time is 2 hours. After adding the flame retardant, the temperature is adjusted to 85°C and the insulation time is 1.5 hours. After adding the polymerization inhibitor, the temperature is adjusted to 110°C and the insulation time is 1.3 hours. The pre-adhesive agent No. 5 is fully stirred and mixed to prepare the pre-adhesive agent No. 5. The pre-adhesive agent No. 5 is poured into a high-pressure homogenizer for homogenization treatment. The homogenization reaction speed is 3500rpm, the homogenization reaction pressure is 1.9MPa, the homogenization reaction temperature is 80°C, and the homogenization reaction time is 2 hours to prepare the pre-adhesive agent No. 6. The pre-adhesive agent No. 6 is filtered and impurities are removed to prepare the desired high temperature resistant adhesive.

[0059] Comparative Example 1

[0060] The invention provides a method for preparing a sprayable polyurethane adhesive. The components of the polyurethane adhesive in parts by weight of various raw materials are: 100 parts by weight of diisocyanate, 80 parts by weight of polyester polyol, 6 parts by weight of terminator, 7 parts by weight of catalyst, 6 parts by weight of emulsifier, 6 parts by weight of inhibitor, 7 parts by weight of coupling agent, 8 parts by weight of modifier, 60 parts by weight of solvent, 85 parts by weight of nano silicon dioxide, 9 parts by weight of plasticizer and 9 parts by weight of flame retardant. The method for preparing the polyurethane adhesive comprises: firstly, synthesizing a prepolymer: under the environmental conditions of a temperature of 55°C and a pressure of 0.15MPa, adding p-phenylene diisocyanate, toluene diisocyanate, polyester polyol and nano silicon dioxide in proportion; Add silicon to the reactor, stir the reaction materials while heating to prepare prepolymer 1, observe the prepolymer 1 in the reactor, when the prepolymer starts to discharge water, cool the reactor to 75°C and keep it warm for 2 hours, add 1,5-naphthalene diisocyanate, 1,4-cyclohexane diisocyanate and nano-silica to the reactor in proportion while stirring, keep it warm for a period of time to prepare prepolymer 2, add prepolymer 2, coupling agent and modifier to the high-speed mixer in proportion, react for 5 hours under the environmental conditions of temperature of 45°C and pressure of 0.1MPa, then add emulsifier to the high-speed mixer in proportion, react for 2.2 hours under the environmental conditions of temperature of 30°C and pressure of 0.12MPa, and prepare Pre-adhesive agent 1 is obtained, and pre-adhesive agent 1 and catalyst are added to a reaction container in proportion, and the reaction container is evacuated, and the temperature of the reaction container is raised to 250° C., and the temperature is kept at 0.1 MPa for 0.5 h to obtain pre-adhesive agent 2. Viscosity test: under the environmental conditions of temperature of 23° C., pressure of 1 MPa and relative humidity of 55%, the viscosity of the pre-adhesive agent is tested using a capillary viscometer. When the viscosity of the main agent reaches 3000±500 centipoise, a terminator is added and the mixture is stirred thoroughly to obtain pre-adhesive agent 3. Under the temperature environment of 60° C., N,N-dimethylformamide, toluene and butanone are added in proportion while stirring, and the mixture is stirred thoroughly to obtain pre-adhesive agent 4. Keep warm for 1.5 hours, add plasticizer, flame retardant and polymerization inhibitor in proportion, adjust the temperature to 75°C after adding plasticizer, and keep warm for 2 hours, adjust the temperature to 85°C after adding flame retardant, and keep warm for 1.5 hours, adjust the temperature to 110°C after adding polymerization inhibitor, and keep warm for 1.3 hours, stir and mix thoroughly to obtain pre-adhesive five, pour pre-adhesive five into high-pressure homogenizer, carry out homogenization treatment, the homogenization reaction speed is 3500rpm, the homogenization reaction pressure is 1.9MPa, the homogenization reaction temperature is 80°C, the homogenization reaction time is 2 hours, obtain pre-adhesive six, filter and remove impurities from pre-adhesive six to obtain the required high temperature resistant adhesive.

[0061] Comparative Example 2

[0062] The invention provides a method for preparing a sprayable polyurethane adhesive. The components of the polyurethane adhesive in parts by weight of various raw materials are: 100 parts by weight of diisocyanate, 80 parts by weight of polyester polyol, 6 parts by weight of terminator, 7 parts by weight of catalyst, 6 parts by weight of emulsifier, 6 parts by weight of polymerization inhibitor, 7 parts by weight of coupling agent, 8 parts by weight of modifier, 60 parts by weight of solvent, 85 parts by weight of nano silicon dioxide, 9 parts by weight of plasticizer and 9 parts by weight of flame retardant. The method for preparing the polyurethane adhesive comprises: firstly, synthesizing a prepolymer: under the environmental conditions of a temperature of 55°C and a pressure of 0.15MPa, adding p-phenylene diisocyanate, toluene diisocyanate, polyester polyol and nano silicon dioxide in proportion; to a reactor, introduce nitrogen into the reactor, stir the reaction materials while heating to prepare prepolymer 1, observe the prepolymer 1 in the reactor, when the prepolymer starts to discharge water, heat the reactor to 250°C, stop introducing nitrogen, and keep warm for 2.5 hours, then cool the reactor to 75°C, and keep warm for 2 hours, add 1,5-naphthalene diisocyanate, 1,4-cyclohexane diisocyanate, and nano-silica into the reactor in proportion while stirring, and keep warm for a period of time to prepare prepolymer 2, add prepolymer 2, coupling agent and modifier into a high-speed stirrer in proportion, and keep warm for 5 hours under the environmental conditions of temperature of 45°C and pressure of 0.1MPa to prepare pre-adhesive 1, add pre-adhesive 1 in proportion Mixture 1 and catalyst into a reaction container, evacuate the reaction container, raise the temperature of the reaction container to 250°C, and keep it warm for 0.5h under a pressure of 0.1MPa to obtain pre-adhesive 2. Test viscosity: use a capillary viscometer to test the viscosity of the pre-adhesive under a temperature of 23°C, a pressure of 1MPa and a relative humidity of 55%. When the viscosity of the main agent reaches 3000±500 centipoise, add a terminator and stir well to obtain pre-adhesive 3. Pass nitrogen into the reaction container, and add N,N-dimethylformamide, toluene and butanone in proportion under a temperature of 60°C while stirring, stir well to obtain pre-adhesive 4. Keep it warm for 1.5 After 1 h, stop introducing nitrogen, add plasticizer, flame retardant and polymerization inhibitor in proportion, adjust the temperature to 75°C after adding plasticizer, and keep warm for 2 h, adjust the temperature to 85°C after adding flame retardant, and keep warm for 1.5 h, adjust the temperature to 110°C after adding polymerization inhibitor, and keep warm for 1.3 h, stir and mix thoroughly to obtain pre-adhesive five, pour pre-adhesive five into high-pressure homogenizer for homogenization, the homogenization reaction speed is 3500 rpm, the homogenization reaction pressure is 1.9 MPa, the homogenization reaction temperature is 80°C, and the homogenization reaction time is 2 h to obtain pre-adhesive six, filter and remove impurities from pre-adhesive six to obtain the required high temperature resistant adhesive.

[0063] Comparative Example 3

[0064] The invention provides a method for preparing a sprayable polyurethane adhesive. The components of the polyurethane adhesive in parts by weight of various raw materials are: 100 parts by weight of diisocyanate, 80 parts by weight of polyester polyol, 7 parts by weight of catalyst, 6 parts by weight of emulsifier, 6 parts by weight of polymerization inhibitor, 7 parts by weight of coupling agent, 8 parts by weight of modifier, 60 parts by weight of solvent, 85 parts by weight of nano silicon dioxide, 9 parts by weight of plasticizer and 9 parts by weight of flame retardant. The method for preparing the polyurethane adhesive comprises: firstly, synthesizing a prepolymer: under the environmental conditions of a temperature of 55°C and a pressure of 0.15MPa, adding p-phenylene diisocyanate, toluene diisocyanate, polyester polyol and nano-isocyanate in proportion; Add nano-silica to the reactor, introduce nitrogen into the reactor, stir the reaction materials while heating to prepare prepolymer 1, observe the prepolymer 1 in the reactor, when the prepolymer starts to produce water, raise the temperature in the reactor to 250°C, stop introducing nitrogen, and keep it warm for 2.5 hours, then cool the reactor to 75°C, and keep it warm for 2 hours, add 1,5-naphthalene diisocyanate, 1,4-cyclohexane diisocyanate and nano-silica to the reactor in proportion while stirring, and keep it warm for a period of time to prepare prepolymer 2, add prepolymer 2, coupling agent and modifier into a high-speed mixer in proportion, and react at a temperature of 45°C and a pressure of 0.1MPa. 5h, then add the emulsifier in proportion to the high-speed mixer, react for 2.2h under the environmental conditions of temperature of 30℃ and pressure of 0.12MPa to obtain pre-adhesive one, add pre-adhesive one and catalyst in proportion to the reaction container, evacuate the reaction container, and heat the reaction container to 250℃, keep it warm for 0.5h under the environmental conditions of pressure of 0.1MPa to obtain pre-adhesive two, pass nitrogen into the reaction container, and under the temperature of 60℃, add N,N-dimethylformamide, toluene and butanone in proportion while stirring, mix thoroughly to obtain pre-adhesive three, keep warm for 1.5h and stop passing nitrogen, and keep it warm in proportion according to the conditions of 1.5h. Add plasticizer, flame retardant and polymerization inhibitor for the first time, adjust the temperature to 75°C after adding the plasticizer, and keep it warm for 2 hours, adjust the temperature to 85°C after adding the flame retardant, and keep it warm for 1.5 hours, adjust the temperature to 110°C after adding the polymerization inhibitor, and keep it warm for 1.3 hours, stir and mix thoroughly to obtain pre-adhesive four, pour the pre-adhesive four into a high-pressure homogenizer for homogenization, the homogenization reaction speed is 3500rpm, the homogenization reaction pressure is 1.9MPa, the homogenization reaction temperature is 80°C, and the homogenization reaction time is 2 hours to obtain pre-adhesive five, filter the pre-adhesive five to remove impurities, and obtain the required high temperature resistant adhesive.

[0065] The specific sources of all chemicals used in the above Examples 1 to 3 and Comparative Examples 1 to 3 are shown in Table 1:

[0066] Table 1

[0067]

[0068]

[0069]

[0070] Experimental Example 1

[0071] Peel strength and viscosity test at room temperature:

[0072] The adhesive strength is expressed by the peel strength test, which is measured according to the national standard adhesive 180° peel strength test method - flexible material to rigid material, GB / T2790-1995 standard;

[0073] Apply glue on the entire width of the bonded test piece, the glue coating length is 200mm, the glue coating thickness is controlled at about 0.25mm, and uniform pressure is applied on the entire bonding surface. Heat and cure at 60℃ for 12h, bend the unbonded end of the electrode sheet 180°, clamp the steel plate on the fixed chuck, and clamp the electrode on the other end. The separation rate of the chuck is 100mm / min, and the effective peeling distance is at least 125mm;

[0074] The sample test temperature was set to 25±0.5°C, and the viscosity of the polyurethane adhesive in the embodiment and the comparative example was tested. The viscosity test was performed using a capillary method, wherein the instrument used was a capillary viscometer. The specific test steps were as follows:

[0075] Use a pipette to accurately transfer the liquid to the capillary viscometer, and use the suction ball to suck the liquid to a certain height. Fix the viscometer vertically, keep the liquid temperature uniform, and wait for at least 30 minutes to achieve temperature equilibrium.

[0076] Open the outlet of the capillary and use a stopwatch to record the time t0 required for the liquid to drop from mark E to mark F. The time should be recorded to one fifth of a second. Perform at least three measurements and take the average value as the final flow time t.

[0077] Calculate the dynamic viscosity using the formula: (in MPa·s), where k is the constant of the capillary viscometer, ρ is the density of the liquid (in mg / mm³, which can be obtained by multiplying the relative density of the liquid by 0.9982), and t is the time the liquid flows (in seconds);

[0078] The peel strength and viscosity test results are shown in Table 2:

[0079] Table 2

[0080]

[0081] According to the data in Table 2, it can be seen that: Referring to Examples 1, 2, and 3, it can be seen that the more diisocyanate and polyester polyol components are used to prepare the adhesive, the higher the peel strength and viscosity thereof. Referring to Example 2 and Comparative Example 1, under the conditions of the same additives, the same additive mass components, and the same preparation environment, when nitrogen is not introduced to protect the reaction, the viscosity and peel strength of the polyurethane adhesive will decrease. Referring to Example 2 and Comparative Example 2, under the conditions of the same additives, the same additive mass components, and the preparation conditions, when the emulsification reaction is not performed, the viscosity and peel strength of the polyurethane adhesive will also decrease. Referring to Example 2 and Comparative Example 3, under the conditions of the same additives, the same additive mass components, and the preparation conditions, when the viscosity test is not performed and the terminator is not added, the viscosity and peel strength of the polyurethane adhesive will also decrease.

[0082] Experimental Example 2

[0083] Testing the high temperature resistance of polyurethane adhesives:

[0084] The polyurethane adhesive prepared in the above embodiment and comparative example was placed in a thermogravimetric analyzer, the test atmosphere was nitrogen, the temperature was increased in the range of 30 to 600°C, and the heating rate was 10°C / min, and the mass loss of the polyurethane was calculated respectively. The thermogravimetric analyzer analyzed the relationship between the mass loss of the polyurethane and the temperature or time, and drew a thermogravimetric curve to analyze the high temperature resistance of the polyurethane adhesive;

[0085] Testing the flame retardant properties of polyurethane adhesives:

[0086] Test the flame retardant properties of polyurethane adhesives according to GB / T2408 standard and record the results;

[0087] Testing the UV resistance of polyurethane adhesives:

[0088] In the temperature environment of 25±0.5℃, the wavelength of ultraviolet light irradiation is 280~315nm, the irradiation intensity is 200W, and the irradiation time is 24h. Measure the tensile strength and elongation at break of the bonded test piece under ultraviolet light and record them;

[0089] In the temperature environment of 25±0.5℃ and without ultraviolet radiation, measure the tensile strength and elongation at break of the bonded test piece and record them;

[0090] The specific test methods for tensile strength and elongation at break are:

[0091] According to national standards, first select the bonded test piece, install the bonded test piece on the tensile testing machine, set the test speed to 50±5mm / min, start the test, gradually increase the tensile force on the bonded test piece until it breaks, record the maximum tensile stress, and calculate the tensile strength. , where Fm is the maximum tensile force and S0 is the original cross-sectional area of ​​the specimen;

[0092] Test method for elongation at break:

[0093] Elongation at break refers to the percentage of elongation of the bonded specimen when it is stretched to break. During the test, the original gauge length is marked on the bonded specimen, and the change in gauge length is measured after breakage to calculate the elongation: ,in is the elongation, is the gauge length at fracture, L0 is the original gauge length, and the force-elongation curve is recorded. Data such as tensile strength and elongation at fracture are read from the curve.

[0094] The test results are shown in Table 3 below:

[0095] Table 3:

[0096]

[0097] According to the data in Table 3, it can be seen that, with reference to Examples 1, 2, and 3, the more diisocyanate and polyester polyol components used in preparing the adhesive, the higher the tensile strength and elongation at break. With reference to Example 2 and Comparative Example 1, under the same additives, the same additive mass components, and the same preparation environment, when nitrogen is not introduced to protect the reaction, the high temperature resistance, flame retardant grade, tensile strength, and elongation at break of the polyurethane adhesive will be reduced, and the anti-ultraviolet performance will also be reduced. With reference to Example 2 and Comparative Example 2, under the same additives, the same additive mass components, and the same preparation conditions, when the emulsification reaction is not performed, the high temperature resistance, flame retardant grade, tensile strength, and elongation at break of the polyurethane adhesive will be reduced, and the anti-ultraviolet performance will also be reduced. With reference to Example 2 and Comparative Example 3, under the same additives, the same additive mass components, and the same preparation conditions, when the viscosity test is not performed and the terminator is not added, the high temperature resistance, flame retardant grade, tensile strength, and elongation at break of the polyurethane adhesive will be reduced, and the anti-ultraviolet performance will also be reduced.

[0098] It can be seen that the polyurethane adhesive prepared by the present invention has strong weather resistance, good high temperature resistance, obvious anti-ultraviolet performance and strong stability.

[0099] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A method for preparing a sprayable polyurethane adhesive, characterized in that: The polyurethane adhesive comprises the following components in parts by weight: 80 to 120 parts by weight of diisocyanate, 50 to 120 parts by weight of polyester polyol, 5 to 12 parts by weight of terminator, 5 to 13 parts by weight of catalyst, 5 to 10 parts by weight of emulsifier, 5 to 11 parts by weight of inhibitor, 5 to 10 parts by weight of coupling agent, 6 to 12 parts by weight of modifier, 40 to 80 parts by weight of solvent, 65 to 125 parts by weight of nano-silicon dioxide, 7 to 12 parts by weight of plasticizer and 7 to 12 parts by weight of flame retardant; The diisocyanate is one or a mixture of two or more of 1,5-naphthalene diisocyanate, 1,4-cyclohexane diisocyanate, p-phenylene diisocyanate, and toluene diisocyanate; The solvent is one or a mixture of two or more of N,N-dimethylformamide, toluene and butanone; The preparation method of the polyurethane adhesive comprises: Step 1, synthesizing prepolymer 1: adding p-phenylene diisocyanate, toluene diisocyanate, polyester polyol and nano-silicon dioxide in a reaction kettle according to a certain proportion, introducing nitrogen into the reaction kettle, and stirring the reaction materials while heating to prepare prepolymer 1; Step 2, synthesizing prepolymer 2: observing prepolymer 1 in the reactor, when the prepolymer starts to produce water, stopping the introduction of nitrogen, and keeping the temperature for a period of time, then cooling the reactor, adding 1,5-naphthalene diisocyanate, 1,4-cyclohexane diisocyanate, and nano-silicon dioxide into the reactor in proportion while stirring, and keeping the temperature for a period of time to obtain prepolymer 2; Step 3, modification and emulsification reaction: add prepolymer 2, coupling agent and modifier into a high-speed mixer in proportion, react fully, then add emulsifier into the high-speed mixer in proportion, mix and react fully to obtain pre-adhesive 1, and keep warm for a period of time; Step 4, catalytic reaction: adding pre-adhesive agent 1 and catalyst into a reaction container in proportion, evacuating the reaction container, heating the reaction container, and keeping the temperature for a period of time to obtain pre-adhesive agent 2; Step 5, test viscosity: preset the target viscosity, use a capillary viscometer to test the viscosity of the pre-adhesive, when the viscosity of the main agent reaches the target viscosity, add the terminator and stir thoroughly to obtain the pre-adhesive three; Step 6, adding solvent: nitrogen is introduced into the reaction container, N, N-dimethylformamide, toluene and butanone are added in proportion while stirring, and the mixture is fully stirred and mixed to obtain pre-adhesive agent 4, and the introduction of nitrogen is stopped after keeping the mixture warm for a period of time; Step 7, homogenization treatment: add plasticizer, flame retardant and polymerization inhibitor in proportion, keep them warm for a period of time, stir and mix them thoroughly to obtain pre-adhesive five, keep them warm for a period of time, pour the pre-adhesive five into a high-pressure homogenizer, perform homogenization treatment, obtain pre-adhesive six, filter and remove impurities from the pre-adhesive six, and obtain the desired adhesive.

2. The method for preparing a sprayable polyurethane adhesive according to claim 1, characterized in that: In the step 1, the mass ratio of p-phenylene diisocyanate, toluene diisocyanate, polyester polyol and nano-silicon dioxide is 20-30:20-30:50-120:65-125, the reaction temperature for synthesizing prepolymer 1 is 50-60° C., and the pressure is 0.1-1.5 MPa.

3. The method for preparing a sprayable polyurethane adhesive according to claim 1, characterized in that: In the step 2, the temperature in the reactor is raised to 220°C to 300°C, the nitrogen is stopped, and the temperature is kept for 2 to 5 hours, and then the temperature of the reactor is lowered to 70 to 100°C, and then kept for 1 to 4 hours; In the step 2, the mass ratio of 1,5-naphthalene diisocyanate, 1,4-cyclohexane diisocyanate and nano-silicon dioxide added is 100:1 to 100:0.5 to 50:0.

1.

4. The method for preparing a sprayable polyurethane adhesive according to claim 1, characterized in that: In the step 3, the mass ratio of prepolymer 2, coupling agent and modifier is 100:1-20:0.1-20:0.1, the temperature of the modification reaction is 20-80°C, the reaction time is 2-10h, and the reaction pressure is 0.1-0.5MPa; The emulsification reaction temperature is 20-60°C, the emulsification reaction time is 2-3h, and the emulsification reaction pressure is 0.1-0.15MPa; In the step three, the modifier is aminosulfonic acid sodium salt, the coupling agent is 3-epoxypropyltriethoxysilane, and the emulsifier is polysorbate and polyoxyethylene.

5. The method for preparing a sprayable polyurethane adhesive according to claim 1, characterized in that: In the step 4, the mass ratio of the pre-binder 1 to the catalyst is 100:0-10:0.5, the reaction container is heated to 200-260° C., the reaction pressure is 0.01-0.1 MPa, and the reaction time is 0.5-1 h.

6. The method for preparing a sprayable polyurethane adhesive according to claim 1, characterized in that: The preset target viscosity in step 5 is 3000±500 centipoise, the temperature during the viscosity test in step 5 is 20-25°C, the test pressure is 0.1-1.5MPa, and the humidity during the test is maintained at 40-60%; In the step 5, the terminator is triphenyl phosphate.

7. The method for preparing a sprayable polyurethane adhesive according to claim 1, characterized in that: In the step six, the mass ratio of N,N-dimethylformamide, toluene and butanone is 50:0.5-50:0.5-50:0.1, the reaction temperature is 55-70°C, and the insulation time is 1-3h.

8. The method for preparing a sprayable polyurethane adhesive according to claim 1, characterized in that: In the step 7, the mass ratio of the plasticizer, the flame retardant and the polymerization inhibitor is 10:0.1 to 10:0.1 to 11:0.2; The plasticizer is polyethylene glycol, the reaction temperature of adding the plasticizer is 70-85°C, and the insulation time is 1-3h; The flame retardant is melamine phosphate, the reaction temperature of adding the flame retardant is 80-95°C, and the heat preservation time is 0.5-2.5h; The polymerization inhibitors are butylated hydroxytoluene and butylated hydroxyethylbenzene, the reaction temperature for adding the polymerization inhibitors is 100-125° C., and the heat preservation time is 1-1.5 hours.

9. The method for preparing a sprayable polyurethane adhesive according to claim 1, characterized in that: In the step 7, the speed of the homogenization reaction is 3000-3500 rpm, the pressure of the homogenization reaction is 1.5-5 MPa, the temperature of the homogenization reaction is 70-85° C., and the time of the homogenization reaction is 1-3.5 h.

Citation Information

Patent Citations

  • Preparation method of adhesive for shoes

    CN107698736A

  • Waterborne polyurethane adhesive for shoes and preparation method thereof

    CN107760247A

  • Polyurethane adhesive and preparation method thereof

    CN108517193A