UV glue with high bonding strength and high water resistance and preparation method thereof
By adjusting the ratio of raw materials for preparation of oligomers and compounding with acrylate monomers, high bond strength and high water resistance UV glue are prepared, which solves the problem that existing UV glues are difficult to meet the requirements of high bond strength and water resistance, and achieves the High bonding ability and long-term stability of resin cured parts.
Patent Information
- Application Number
- CN202411201353.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-11-12
AI Technical Summary
Existing UV glues are difficult to meet the performance requirements of high bonding strength and high water resistance at the same time, which affects the performance and service life of smart home appliances.
By adjusting the raw material ratio of oligomers, oligomers with excellent bonding, water resistance and strength are prepared, and combined with acrylate monomers to prepare high bonding strength and high water resistance UV glue, including Formulations of oligomers, acrylate monomers, photoinitiators and polymerization inhibitors.
It significantly improves the bonding ability of resin cured parts, has high bonding strength and high water resistance, and has good long-term storage stability, meeting the high-performance demand of smart home appliances for glue.
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of UV glue, and mainly to a UV glue with high bonding strength and high water resistance and a preparation method thereof. Background Art
[0002] With the rapid development of industries such as smart home appliances such as floor scrubbers and vacuum cleaners, the variety and quantity of smart home appliances are increasing, and the demand for glue is also increasing. People also have higher and higher requirements for the quality and safety of glue. When bonding home appliance parts, quick and convenient glue is often needed. In daily use, due to the large number and intensity of home appliances, and the generally high humidity in the working environment, the glue also needs to have high bonding strength and high water resistance. With the rapid development of the home appliance industry, the market demand for adhesives with high bonding strength and high water resistance has increased significantly in the past two years. However, the current use of traditional solvent-based glue has the problems of slow effectiveness and insufficient practicality, and some of the UV glues used have not been adjusted specifically, and it is difficult to meet the performance requirements of high bonding strength and high water resistance at the same time, which affects the performance and service life of home appliances. Therefore, it is necessary to develop a UV glue with high bonding strength and high water resistance. Summary of the invention
[0003] In view of the above-mentioned deficiencies in the prior art, the purpose of the present application is to provide a UV glue with high bonding strength and high water resistance and a preparation method thereof, aiming to solve the problem that the existing UV glue is difficult to simultaneously meet the performance requirements of high bonding strength and high water resistance.
[0004] The technical solution of this application is as follows: In a first aspect, the present application provides a UV glue with high bonding strength and high water resistance, wherein, by weight, it comprises the following components: 65-80 parts of oligomer, 10-25 parts of acrylate monomer, 2-5 parts of photoinitiator, and 0.1-0.5 parts of first inhibitor; The raw materials for preparing the oligomer include isocyanate, polyol, hydroxyl-containing acrylate monomer and reactive diluent; The mass ratio of the isocyanate, the polyol and the hydroxyl-containing acrylate monomer is 2:1.3-1.7:0.6-1.5; the added amount of the reactive diluent is 30%-60% of the mass of the isocyanate.
[0005] By adjusting the proportion of raw materials for preparing the oligomer, the oligomer obtained in the present application has better adhesion, water resistance and strength, and is more compatible with the formula of the present application. The high bonding strength and high water resistance UV glue provided can significantly improve the bonding ability of the resin-cured parts, has high bonding strength, and at the same time gives it higher water resistance and good long-term storage stability.
[0006] Furthermore, the method for preparing the oligomer comprises the following steps: (1) Add the vacuum-treated polyol, active diluent, a second inhibitor accounting for 0.5‰-0.8‰ of the mass of the active diluent, and a catalyst accounting for 0.3‰-0.5‰ of the mass of the active diluent into a reaction kettle, raise the temperature to 50-55°C, and gradually add isocyanate dropwise for 1-2 hours; (2) Raise the temperature to 70-75°C and keep warm for 2-3 hours; (3) lowering the temperature to 45-50°C, adding the hydroxyl-containing acrylate monomer, keeping the temperature for 40 minutes, and then adding the catalyst in an amount of 0.3‰-0.5‰ of the mass of the hydroxyl-containing acrylate monomer, and keeping the temperature for 0.5h; (4) raising the temperature to 78-85° C. and maintaining the temperature until the NCO content is less than 0.1% to obtain the oligomer; The mass ratio of the isocyanate, the polyol and the hydroxyl-containing acrylate monomer is 2:1.5:1.
[0007] Through the preparation method of the oligomer provided, the synthesized self-made polyurethane acrylate has sufficient strength while ensuring adhesion and water resistance, has better adaptability to subsequent formulations, has good comprehensive performance, and is used as an oligomer in a UV glue formula, which is conducive to meeting the required UV glue performance.
[0008] Further, the polyol is one or more of T5652, T6002, T4672, T4692 and G3452 of Asahi Kasei PCDL of Japan; The isocyanate is one or more of 2,4-diisocyanatotoluene, 1,3,3-trimethyl-5-isocyanato-1-isocyanatomethylcyclohexane, 1,6-diisocyanatohexane and 4,4′-dicyclohexylmethane diisocyanate; The active diluent is one or more of 4-(1-oxo-2-propenyl)morpholine, tetrahydrofurfuryl acrylate, 2-methyl-2-propenoic acid 1,7,7-trimethylbicyclo[2.2.1]hept-2-ol ester, and 1,7,7-trimethylbicyclo[2.2.1]hept-2-ol-2-propenoate; The hydroxyl-containing acrylate monomer is one or more of ethylene glycol monomethacrylate, 2-hydroxyethyl methacrylate, 2-hydroxyethyl acrylate, propylene glycol monoacrylate, hydroxypropyl methacrylate, trimethylolpropane diacrylate and pentaerythritol triacrylate; The catalyst is one of dibutyltin laurate, organic bismuth, stannous octoate, triethanolamine and zinc naphthenate; The second polymerization inhibitor is one of p-hydroxyanisole, hydroquinone and 2,6-di-tert-butyl-p-cresol.
[0009] Furthermore, the polyol is T5652 or T4692.
[0010] Furthermore, the isocyanate is the 1,3,3-trimethyl-5-isocyanato-1-isocyanatomethylcyclohexane or 4,4′-dicyclohexylmethane diisocyanate.
[0011] Furthermore, the active diluent is a combination of 2-methyl-2-acrylic acid 1,7,7-trimethylbicyclo[2.2.1]hept-2-ol ester and tetrahydrofurfuryl acrylate, and the mass ratio of 2-methyl-2-acrylic acid 1,7,7-trimethylbicyclo[2.2.1]hept-2-ol ester and tetrahydrofurfuryl acrylate is 2:1.
[0012] Furthermore, the hydroxyl-containing acrylic acid ester monomer is 2-hydroxyethyl acrylate or hydroxypropyl methacrylate.
[0013] Further, the acrylic acid ester monomer is one or more of 2-methyl-2-acrylic acid dodecyl ester, 2-propionic acid-(5-ethyl-1,3-dioxane-5-yl)methyl ester, 1,7,7-trimethylbicyclo[2.2.1]hept-2-ol-2-acrylate and dicyclopentane acrylate; The photoinitiator is one or more of a benzil photoinitiator, an aromatic acylphosphine oxide benzene, an alkyl phenone photoinitiator, an acetone derivative, and an aromatic ketone photoinitiator; the acetone derivative is one of 1-hydroxycyclohexylacetophenone, 2,2-dimethyl-α-hydroxyacetophenone, or p-isopropylphenyl-2-hydroxy-2,2-dimethyl-1-propanone; the aromatic ketone photoinitiator is one of benzophenone, dimethylthioxanthone, or diethylthioxanthone; The first polymerization inhibitor is one or both of p-hydroxyanisole and 1,4-benzoquinone.
[0014] Furthermore, the photoinitiator is 1-hydroxycyclohexylacetophenone.
[0015] In a second aspect, the present application further provides a method for preparing the UV glue with high bonding strength and high water resistance as described in the first aspect, which comprises the following steps: Weigh the acrylic acid ester monomer and the oligomer in proportion, place in a container, and stir at a temperature of 60-70° C. and a speed of 200-300 r / min for 1.5 hours to obtain a mixed solution; The mixed solution is cooled to 45-55° C., the photoinitiator and the first polymerization inhibitor are added in sequence according to proportion, and the mixture is stirred at a speed of 1200-1500 r / min for 30-40 minutes to obtain the UV glue with high bonding strength and high water resistance. Beneficial effects: The present application adjusts the proportion of raw materials for preparing oligomers, so that the oligomers obtained have better adhesion, water resistance and strength, and are more compatible with the formula of UV glue. The bonding ability of resin-cured parts can be improved by compounding oligomers with acrylate monomers. The provided UV glue has high bonding strength after curing, and has good high water resistance and long-term storage stability. DETAILED DESCRIPTION
[0016] The present application provides a UV glue with high bonding strength and high water resistance and a preparation method thereof. To make the purpose, technical solution and effect of the present application clearer and more specific, the present application is further described in detail below. It should be understood that the specific embodiments described herein are only used to explain the present application and are not used to limit the present application.
[0017] The present application provides a UV glue with high bonding strength and high water resistance, which includes the following components in parts by mass: 65-80 parts of oligomer, 10-25 parts of acrylate monomer, 2-5 parts of photoinitiator, and 0.1-0.5 parts of first inhibitor.
[0018] The present application provides a high bonding strength and high water resistance UV glue by compounding oligomers with acrylate monomers, which can significantly improve the bonding ability of resin-cured parts, have high bonding strength, and at the same time give them high water resistance and good long-term storage stability.
[0019] Furthermore, the method for preparing the oligomer comprises the following steps: (1) Add the vacuum-treated polyol, active diluent, 0.5‰-0.8‰ of the second inhibitor and 0.3‰-0.5‰ of the catalyst into the reactor, raise the temperature to 50-55°C, and gradually add isocyanate dropwise for 1-2 hours; (2) Raise the temperature to 70-75°C and keep warm for 2-3 hours; (3) Lower the temperature to 45-50°C, add the hydroxyl-containing acrylate monomer, keep warm for 40 minutes, then add a catalyst accounting for 0.3‰-0.5‰ of the mass of the hydroxyl-containing acrylate monomer, and keep warm for 0.5h; (4) Raise the temperature to 78-85°C and keep warm for 3.5-4.5 hours until the NCO content is less than 0.1% to obtain an oligomer.
[0020] Furthermore, in the preparation step of the oligomer, the mass ratio of isocyanate, polyol and hydroxyl-containing acrylate monomer is 2:1.3-1.7:0.6-1.5. The amount of active diluent added is 30%-60% of the mass of isocyanate.
[0021] Furthermore, the optimal ratio of the mass ratio of isocyanate, polyol and hydroxyl-containing acrylate monomer is 2:1.5:1. Under this ratio, the synthesized polyurethane acrylate oligomer has the best comprehensive performance, while ensuring adhesion and water resistance, it also has sufficient strength, has better adaptability to subsequent formulations, and is used as an oligomer in a UV glue formula, which is conducive to meeting the required UV glue performance. Further, the polyol is selected from one or more of T5652, T6002, T4672, T4692 and G3452 of Asahi Chemical PCDL of Japan. The oligomer prepared by the selected polyol has good performance and can be specifically obtained from commercial sources.
[0022] Furthermore, the polyol is preferably T5652 or T4692. In the present application, by using the preferred polyol as the soft chain part of the self-made polyurethane acrylate, the synthesized resin can be significantly improved in terms of mechanical strength, hydrolysis resistance, thermal stability, weather resistance, etc., especially in terms of water resistance. In addition, the soft chain part can also provide a certain adhesion to the resin and improve the adhesion to the substrate.
[0023] Further, the isocyanate is selected from one or more of 2,4-diisocyanatotoluene, 1,3,3-trimethyl-5-isocyanato-1-isocyanatomethylcyclohexane, 1,6-diisocyanatohexane and 4,4′-dicyclohexylmethane diisocyanate. The oligomer is prepared by the selected isocyanate.
[0024] Furthermore, the isocyanate is preferably 1,3,3-trimethyl-5-isocyanato-1-isocyanatomethylcyclohexane or 4,4′-dicyclohexylmethane diisocyanate. In the present application, by using the preferred isocyanate, the synthesized self-made polyurethane acrylate has good yellowing resistance and is relatively friendly in terms of compatibility with other materials.
[0025] Further, the active diluent is selected from one or more of 4-(1-oxo-2-propenyl)morpholine, tetrahydrofurfuryl acrylate, 2-methyl-2-propenoic acid 1,7,7-trimethylbicyclo[2.2.1]hept-2-ol ester, and 1,7,7-trimethylbicyclo[2.2.1]hept-2-ol-2-propenoate. The selected active diluent can adjust the synthetic properties of the oligomer.
[0026] Furthermore, the active diluent is a combination of 2-methyl-2-acrylic acid 1,7,7-trimethylbicyclo[2.2.1]hept-2-ol ester and tetrahydrofurfuryl acrylate, and the mass ratio of 2-methyl-2-acrylic acid 1,7,7-trimethylbicyclo[2.2.1]hept-2-ol ester and tetrahydrofurfuryl acrylate is 2:1. In the present application, by selecting a combination of active diluents at a specific ratio and content, adding them during the synthesis process to play a certain viscosity-reducing effect, it is beneficial to the preparation of self-made polyurethane acrylate and improve the performance. The synthesized self-made polyurethane acrylate shows relatively prominent viscosity to the PC substrate, and when participating in the curing of UV glue in the later stage, the active diluent is also used as part of the formula to further improve the adhesion.
[0027] Furthermore, the hydroxyl-containing acrylate monomer is selected from one or more of ethylene glycol monomethacrylate, 2-hydroxyethyl methacrylate, 2-hydroxyethyl acrylate, propylene glycol monoacrylate, hydroxypropyl methacrylate, trimethylolpropane diacrylate and pentaerythritol triacrylate. Grafting is performed through the selected hydroxyl-containing acrylate monomer.
[0028] Furthermore, the hydroxyl-containing acrylate monomer is 2-hydroxyethyl acrylate or hydroxypropyl methacrylate. In the present application, a specific hydroxyl-containing acrylate monomer combination and ratio are selected, and the combination is grafted onto polyurethane acrylate, so that the resin can be endowed with light-curing properties, and the side methyl groups contained in its structure can improve the water resistance and compatibility of the resin, and because of the steric hindrance it produces, its reactivity is reduced, so that the shrinkage of the self-made polyurethane acrylate after curing is reduced, thereby further improving the adhesion of the resin.
[0029] Furthermore, the catalyst is selected from one of dibutyltin laurate, organic bismuth, stannous octoate, triethanolamine and zinc naphthenate.
[0030] Furthermore, the second polymerization inhibitor is selected from one of p-hydroxyanisole, hydroquinone and 2,6-di-tert-butyl-p-cresol.
[0031] Further, in the UV glue with high bonding strength and high water resistance, the acrylate monomer is one or more of 2-methyl-2-dodecyl acrylate (LMA), 2-propionic acid-(5-ethyl-1,3-dioxane-5-yl)methyl ester (CTFA), 1,7,7-trimethylbicyclo[2.2.1]hept-2-ol-2-acrylate (IBOA) and dicyclopentane acrylate (HDCPMA). In the present application, the selected acrylate monomer has strong adhesion to the substrate PC and good water resistance.
[0032] Furthermore, the photoinitiator is selected from one or more of benzil-based photoinitiators, aromatic acylphosphine oxide benzene, alkyl phenone-based photoinitiators, acetone derivatives and aromatic ketone-based photoinitiators.
[0033] Among them, the acetone derivative is one of 1-hydroxycyclohexylacetophenone, 2,2-dimethyl-α-hydroxyacetophenone or p-isopropylphenyl-2-hydroxy-2,2-dimethyl-1-propanone, and the aromatic ketone photoinitiator is one of benzophenone, dimethylthioxanthone or diethylthioxanthone.
[0034] Preferably, the photoinitiator is 1-hydroxycyclohexylacetophenone. In the present application, the preferred 1-hydroxycyclohexylacetophenone (HCPK) added to the UV glue system of the present application has good solubility and reactivity, small dosage, high initiation efficiency, fast curing speed, and as a photoinitiator, it can further improve the curing rate of the cured part and improve the aging resistance.
[0035] Further, the first inhibitor is selected from one or both of p-hydroxyanisole and 1,4-benzoquinone. In the present application, the selected p-hydroxyanisole and 1,4-benzoquinone play a positive role in the thermal stability of the UV glue formula.
[0036] The UV glue provided in the present application has both high bonding strength and high water resistance after curing, wherein the bonding ability of the resin cured part can be improved by compounding the oligomer with the acrylate monomer, and has high bonding strength, good high water resistance, and good long-term storage stability.
[0037] The present application also provides a method for preparing the UV glue with high bonding strength and high water resistance as described above, which comprises the following steps: Weigh the acrylic acid ester monomer and the oligomer in proportion, place them in a container, and stir them at 60-70° C. and 200-300 r / min for 1.5 hours to obtain a mixed solution; The mixed solution is cooled to 45-55°C, and the photoinitiator and the first inhibitor are added in proportion in sequence, and stirred at a speed of 1200-1500 r / min for 30-40 minutes to obtain a UV glue with high bonding strength and high water resistance.
[0038] Compared with traditional solvent-based glue, the UV glue with high bonding strength and high water resistance prepared in this application is time-saving, convenient, fast, and practical, and can effectively meet the performance requirements of use. After simple adjustment, it can be mass-produced to meet market demand.
[0039] The invention is further described below by means of specific examples.
[0040] The method for preparing the oligomer used in each embodiment of the present application comprises the following steps: (1) Add the vacuum-treated polyol, active diluent, 0.65‰ of the second inhibitor and 0.4‰ of the catalyst into the reactor, raise the temperature to 55°C, and gradually add isocyanate dropwise for 1-2 hours; (2) Raise the temperature to 75°C and keep warm for 2.5 hours; (3) Lower the temperature to 50°C, add the hydroxyl-containing acrylate monomer, keep the temperature for 40 minutes, then add a catalyst accounting for 0.4‰ of the mass of the hydroxyl-containing acrylate monomer, and keep the temperature for 0.5 hours; (4) The temperature was raised to 80°C and kept at this temperature for 4 hours. The NCO content was measured to be less than 0.1%, thereby obtaining a self-made polyurethane acrylate, i.e., an oligomer.
[0041] Among them, the polyol is T5652; the isocyanate is 1,3,3-trimethyl-5-isocyanato-1-isocyanatomethylcyclohexane; the active diluent is a combination of 2-methyl-2-acrylic acid 1,7,7-trimethylbicyclo[2.2.1]hept-2-ol ester and tetrahydrofurfuryl acrylate in a mass ratio of 2:1; the hydroxyl-containing acrylate monomer is 2-hydroxyethyl acrylate; the mass ratio of isocyanate, polyol and hydroxyl-containing acrylate monomer is 2:1.5:1; the amount of active diluent added is 45% of the mass of isocyanate; the catalyst is dibutyltin laurate; and the second inhibitor is p-hydroxyanisole.
[0042] Examples 1-6 The high bonding strength and high water resistance UV adhesive of Examples 1-6 of the present application, by weight, has specific proportions of the components as shown in Table 1: Table 1 Composition (portions) Example 1 Example 2 Example 3 Example 4 Example 5 Example 6 Homemade polyurethane acrylate 70 80 75 70 80 75 LMA 20 10 15 - - - CTFA - - - 20 10 15 HCPK 2 5 3 2 5 3 p-Hydroxyanisole 0.1 0.5 0.3 0.1 0.5 0.3 The high bonding strength and high water resistance UV glue raw materials of Examples 1-6 were prepared by the component proportions in Table 1, and commercially available UV glue was selected as Comparative Example 1. The high bonding strength and high water resistance UV glue of Examples 1-6 were tested for performance, and the test method included: (1) Water resistance test: Use the high bonding strength and high water resistance UV glue of each embodiment to bond the PC substrates to each other, put them under a 1000W UV lamp for curing for 2 minutes, and cool them. Soak the bonded PC boards in clean water for 500 hours, and observe whether the glue spots are white or fall off.
[0043] (2) Adhesion strength test: i.e. shear strength test. Use a digital caliper to measure the required dimensions and draw lines on the test workpiece. Refer to the standard: GB / T 7124-2008 / ISO 4587:2003. Apply a proper amount of glue to the shear part of the workpiece, flatten and wipe off the excess glue. Place the workpiece under a 1000W UV lamp to cure for 2 minutes and cool. Install the workpiece on the tensile testing machine according to the clamping distance for testing.
[0044] The performance test results of the high bonding strength and high water resistance UV glues of Examples 1-6 and the UV glue of Comparative Example 1 are shown in Table 2: Table 2 Shear strength(MPa) Water resistance Example 1 20.5 pass Example 2 19.8 pass Example 3 20.6 pass Example 4 20.3 pass Example 5 20.5 pass Example 6 20.6 pass Comparative Example 1 16.3 Degumming, whitening By comparing the test results, it can be found that the UV glue of the preferred embodiment of the present application, which selects homemade polyurethane acrylate, suitable monomers, initiators and inhibitors, can have better water resistance while ensuring high bonding strength, which is far superior to the UV glue on the market.
[0045] It should be understood that the application of the present application is not limited to the above examples. For ordinary technicians in this field, improvements or changes can be made according to the above description, and all these improvements and changes should fall within the scope of protection of the present application.
Claims
1. A UV glue with high bonding strength and high water resistance, characterized in that: The composition comprises the following components by weight: 65-80 parts of oligomer, 10-25 parts of acrylate monomer, 2-5 parts of photoinitiator, and 0.1-0.5 parts of first inhibitor; The raw materials for preparing the oligomer include isocyanate, polyol, hydroxyl-containing acrylate monomer and reactive diluent; The mass ratio of the isocyanate, the polyol and the hydroxyl-containing acrylate monomer is 2:1.3-1.7:0.6-1.5; the added amount of the reactive diluent is 30%-60% of the mass of the isocyanate.
2. The high bonding strength and high water resistance UV glue according to claim 1, characterized in that: The method for preparing the oligomer comprises the following steps: (1) Add the vacuum-treated polyol, active diluent, a second inhibitor accounting for 0.5‰-0.8‰ of the mass of the active diluent, and a catalyst accounting for 0.3‰-0.5‰ of the mass of the active diluent into a reaction kettle, raise the temperature to 50-55°C, and gradually add isocyanate dropwise for 1-2 hours; (2) Raise the temperature to 70-75°C and keep warm for 2-3 hours; (3) lowering the temperature to 45-50°C, adding the hydroxyl-containing acrylate monomer, keeping the temperature for 40 minutes, and then adding the catalyst in an amount of 0.3‰-0.5‰ of the mass of the hydroxyl-containing acrylate monomer, and keeping the temperature for 0.5h; (4) raising the temperature to 78-85° C. and maintaining the temperature until the NCO content is less than 0.1% to obtain the oligomer; The mass ratio of the isocyanate, the polyol and the hydroxyl-containing acrylate monomer is 2:1.5:
1.
3. The high bonding strength and high water resistance UV glue according to claim 2, characterized in that: The polyol is one or more of T5652, T6002, T4672, T4692 and G3452 of Asahi Kasei PCDL of Japan; The isocyanate is one or more of 2,4-diisocyanatotoluene, 1,3,3-trimethyl-5-isocyanato-1-isocyanatomethylcyclohexane, 1,6-diisocyanatohexane and 4,4′-dicyclohexylmethane diisocyanate; The active diluent is one or more of 4-(1-oxo-2-propenyl)morpholine, tetrahydrofurfuryl acrylate, 2-methyl-2-propenoic acid 1,7,7-trimethylbicyclo[2.2.1]hept-2-ol ester, and 1,7,7-trimethylbicyclo[2.2.1]hept-2-ol-2-propenoate; The hydroxyl-containing acrylate monomer is one or more of ethylene glycol monomethacrylate, 2-hydroxyethyl methacrylate, 2-hydroxyethyl acrylate, propylene glycol monoacrylate, hydroxypropyl methacrylate, trimethylolpropane diacrylate and pentaerythritol triacrylate; The catalyst is one of dibutyltin laurate, organic bismuth, stannous octoate, triethanolamine and zinc naphthenate; The second polymerization inhibitor is one of p-hydroxyanisole, hydroquinone and 2,6-di-tert-butyl-p-cresol.
4. The high bonding strength and high water resistance UV glue according to claim 3, characterized in that: The polyol is T5652 or T4692.
5. The high bonding strength and high water resistance UV glue according to claim 3, characterized in that: The isocyanate is the 1,3,3-trimethyl-5-isocyanato-1-isocyanatomethylcyclohexane or 4,4′-dicyclohexylmethane diisocyanate.
6. The high bonding strength and high water resistance UV glue according to claim 3, characterized in that: The active diluent is a combination of 2-methyl-2-acrylic acid 1,7,7-trimethylbicyclo[2.2.1]hept-2-ol ester and tetrahydrofurfuryl acrylate, and the mass ratio of 2-methyl-2-acrylic acid 1,7,7-trimethylbicyclo[2.2.1]hept-2-ol ester and tetrahydrofurfuryl acrylate is 2:
1.
7. The high bonding strength and high water resistance UV glue according to claim 3, characterized in that: The hydroxyl-containing acrylic acid ester monomer is the 2-hydroxyethyl acrylate or hydroxypropyl methacrylate.
8. The high bonding strength and high water resistance UV glue according to claim 1, characterized in that: The acrylic acid ester monomer is one or more of 2-methyl-2-acrylic acid dodecyl ester, 2-propionic acid-(5-ethyl-1,3-dioxane-5-yl)methyl ester, 1,7,7-trimethylbicyclo[2.2.1]hept-2-ol-2-acrylate and dicyclopentane acrylate; The photoinitiator is one or more of a benzil photoinitiator, an aromatic acylphosphine oxide benzene, an alkyl phenone photoinitiator, an acetone derivative, and an aromatic ketone photoinitiator; the acetone derivative is one of 1-hydroxycyclohexylacetophenone, 2,2-dimethyl-α-hydroxyacetophenone, or p-isopropylphenyl-2-hydroxy-2,2-dimethyl-1-propanone; the aromatic ketone photoinitiator is one of benzophenone, dimethylthioxanthone, or diethylthioxanthone; The first polymerization inhibitor is one or both of p-hydroxyanisole and 1,4-benzoquinone.
9. The high bonding strength and high water resistance UV glue according to claim 8, characterized in that: The photoinitiator is 1-hydroxycyclohexylacetophenone.
10. A method for preparing the UV glue with high bonding strength and high water resistance according to any one of claims 1 to 9, characterized in that: The following steps are involved: Weigh the acrylic acid ester monomer and the oligomer in proportion, place in a container, and stir at a temperature of 60-70° C. and a speed of 200-300 r / min for 1.5 hours to obtain a mixed solution; The mixed solution is cooled to 45-55° C., the photoinitiator and the first polymerization inhibitor are added in sequence according to proportion, and the mixture is stirred at a speed of 1200-1500 r / min for 30-40 minutes to obtain the UV glue with high bonding strength and high water resistance.
Citation Information
Cited By
A method for preparing a multifunctional silicone-epoxy polyurethane resin, uv adhesive and a method for preparing the same and applications thereof
CN122749848A