Adhesive with mildew-proof and antibacterial characteristics and preparation method thereof

By using hydrogen peroxide modification treatment in keratin-based adhesives, the cross-linking network structure is formed, and the problem of perishable keratin-based adhesives is solved, the bonding strength and antibacterial properties are significantly improved, and the utilization of waste resources is realized and the development of high-performance adhesives.

CN118931493APending Publication Date: 2024-11-12INST OF BIOLOGICAL & MEDICAL ENG GUANGDONG ACAD OF SCI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411153034.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Keratin-based functional materials are susceptible to fungi and bacteria, causing mold growth and decay, damaging bond strength and durability, making it difficult to develop viable wood adhesives with high mechanical properties.

Method used

Hydrogen peroxide is used as a modifier, and through enzymatic decomposition and hydrogen peroxide treatment, keratin molecules form a crosslinking network structure to prepare adhesives with anti-mold and antibacterial properties.

Benefits of technology

It significantly improves the adhesive strength and antibacterial properties, especially the antibacterial rate of E. coli reaches 100%, extends the shelf life, and realizes the resource utilization of waste resources.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118931493A_ABST
    Figure CN118931493A_ABST
Patent Text Reader

Abstract

The invention discloses an adhesive with mildew-proof and antibacterial characteristics and a preparation method thereof. Comprising the following steps: A, collecting waste keratin, washing, drying, puffing and crushing the waste keratin to obtain pretreated keratin powder; b, carrying out enzymolysis on the keratin powder obtained by pretreatment, and filtering and separating to obtain hydrolysate; c, adding a hydrogen peroxide solution into the hydrolysate, and stirring; and D, freeze-drying, and mixing with water to obtain the adhesive. The modification reagent used in the invention is hydrogen peroxide which is an effective oxidant which is environment-friendly, stable, non-toxic and pollution-free, and the final decomposition products of the hydrogen peroxide are only water and oxygen, so that the hydrogen peroxide is harmless to the environment and human health when being used at low concentration in industrial production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of industrial adhesives, and in particular relates to an adhesive with mildew-proof and antibacterial properties and a preparation method thereof. Background Art

[0002] The development of keratin-based functional materials has become a hot topic in scientific research, especially the conversion of keratin into adhesives, which has important value in terms of business and environmental protection. Moreover, the mildew resistance of adhesives is an important indicator for evaluating the durability of adhesives. However, nutrient-rich keratin adhesives are particularly susceptible to attack by fungi and bacteria, which promotes the growth of mold and subsequent decay. This degradation impairs the bond strength and durability of the adhesive. Therefore, it remains challenging to use keratin to produce industrially viable wood adhesives in the high-value utilization of biomass and the plywood manufacturing industry.

[0003] Hydrogen peroxide is an effective oxidant that is environmentally friendly, stable, non-toxic, and non-polluting. Its final decomposition products are only water and oxygen, so it is harmless to the environment and human health when used in low concentrations in industrial production. Therefore, hydrogen peroxide has been widely used in the oxidation of biomass-derived materials. In order to develop keratin-based adhesives with high mechanical properties, hydrogen peroxide was designed as a modifier to induce the formation of a strong and continuous cross-linked network structure between protein molecules. This is mainly due to the hydroxyl anions formed during the decomposition of hydrogen peroxide, which react with the functional groups of keratin as nucleophiles, thereby promoting cross-linking. In addition, hydrogen peroxide has the ability to oxidize substrates into corresponding sulfoxide compounds, thereby achieving strong sulfide oxidation. This unique property plays a key role in the preparation of high-performance keratin-based adhesives. Summary of the invention

[0004] The invention provides an adhesive with mildew-proof and antibacterial properties and a preparation method thereof.

[0005] The adhesive with mildew-proof and antibacterial properties of the present invention is prepared by the following method:

[0006] A. collecting waste keratin, washing, drying, puffing and crushing it to obtain pretreated keratin powder;

[0007] B. enzymatically hydrolyzing the keratin powder obtained by the pretreatment, and filtering and separating to obtain a hydrolyzate;

[0008] C. Add hydrogen peroxide solution to the hydrolyzate and stir;

[0009] D. After freeze-drying, mix with water to obtain an adhesive.

[0010] Preferably, the waste keratin in step A is one or more of chicken feathers, duck feathers, goose feathers and wool.

[0011] Preferably, the concentration of the enzyme in the enzymatic hydrolysis process in step B is 0.3-0.5 g / L.

[0012] The enzyme is one or more of papain, alkaline protease, keratinase, trypsin and pepsin.

[0013] Preferably, the concentration of keratin powder during the hydrolysis process in step B is 10-50 g / L.

[0014] Preferred is a combination of alkaline protease and keratinase, with concentrations of 30 g / L and 50 mg / L, respectively.

[0015] Preferably, the temperature of the enzymatic hydrolysis process in step B is 30-60° C., the pH is 8-11, and the time is 12-48 hours.

[0016] Preferably, the concentration of hydrogen peroxide in step C is 30%, and the amount used is 0.1-5 mL hydrogen peroxide per gram of keratin powder. More preferably, the amount used is 1-5 mL hydrogen peroxide per gram of keratin powder.

[0017] The adhesive prepared according to the method has good mildew-proof and antibacterial effects, especially the antibacterial effect on Escherichia coli reaches 100%.

[0018] Compared with the prior art, the present invention has the following beneficial effects:

[0019] The invention uses chicken feathers, duck feathers and the like as raw materials, which not only makes resource utilization of waste, but also the prepared adhesive product can be applied to industrial production.

[0020] The modification agent used in the present invention is hydrogen peroxide, which is an effective oxidant that is environmentally friendly, stable, non-toxic and pollution-free. Its final decomposition products are only water and oxygen. Therefore, when used in low concentrations in industrial production, it is harmless to the environment and human health.

[0021] The present invention is guided by the molecular recombination theory and uses hydrogen peroxide to modify keratin, aiming to develop a multifunctional keratin-based adhesive with mildew-proof, antibacterial and high-strength adhesive properties. The present invention not only solves the shelf life problem of current commercial adhesives, but also makes full use of waste resources, and has good industrial application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 This is a diagram of the anti-mildew effect of adhesives indoors;

[0023] Figure 2This is a graph showing the antibacterial effect of adhesives on Escherichia coli;

[0024] Figure 3 This is a graph showing the antibacterial effect of the adhesive on Staphylococcus aureus. DETAILED DESCRIPTION

[0025] In order to make the contents of the present invention easier to understand, the scheme of the present invention is further described below in conjunction with specific implementation methods.

[0026] Example 1

[0027] 1) washing, drying, puffing and crushing the discarded chicken feathers to obtain pretreated keratin powder;

[0028] 2) Prepare 100 mL of PBS buffer with a pH of 11, add 30 mg of alkaline protease and 50 mg of keratinase, and mix well;

[0029] 3) Weighing 1 g of the keratin powder obtained in step 1) and adding it to the mixed solution in step 2), placing it in a shaker at 50° C., hydrolyzing it for 24 hours, and then filtering it to obtain a hydrolyzate;

[0030] 4) Measure 1 mL of 30% hydrogen peroxide solution and add it, and stir at room temperature for 3 hours;

[0031] 5) freeze-drying to obtain adhesive 1, which has a bonding strength of 2.1 MPa.

[0032] Example 2

[0033] 1) washing, drying, puffing and crushing the discarded chicken feathers to obtain pretreated keratin powder;

[0034] 2) Prepare 100 mL of PBS buffer with a pH of 11, add 30 mg of alkaline protease and 50 mg of keratinase, and mix well;

[0035] 3) Weighing 1 g of the keratin powder obtained in step 1) and adding it to the mixed solution in step 2), placing it in a shaker at 50° C., hydrolyzing it for 24 hours, and then filtering it to obtain a hydrolyzate;

[0036] 4) Measure 5 mL of 30% hydrogen peroxide solution and add it, and stir at room temperature for 3 hours;

[0037] 5) freeze-drying to obtain adhesive 2, which has a bonding strength of 1.5 MPa.

[0038] Comparative Example 1

[0039] 1) washing, drying, puffing and crushing the discarded chicken feathers to obtain pretreated keratin powder;

[0040] 2) Prepare 100 mL of PBS buffer with a pH of 11, add 30 mg of alkaline protease and 50 mg of keratinase, and mix well;

[0041] 3) Weighing 1 g of the keratin powder obtained in step 1) and adding it to the mixed solution in step 2), placing it in a shaker at 50° C., hydrolyzing it for 24 hours, and then filtering it to obtain a hydrolyzate;

[0042] 4) freeze-drying to prepare adhesive 3, whose bonding strength is 0.78 MPa.

[0043] Performance Testing

[0044] 1. Determination of bond strength

[0045] Adhesive strength is the most important indicator for evaluating adhesives. In order to detect the adhesive effect of the adhesive prepared by the present invention, according to the method for determining the tensile shear strength of adhesives in GB / T 7124-2008, an electronic universal mechanical testing machine was used to determine the tensile shear strength of the prepared adhesive on the wood board. The following test experiment is provided: the sample size is 100mm×25mm×1.6mm, and the adhesives of Examples 1 and 2 and Comparative Example 1 are evenly applied to the sample by manual brushing, and the coating area is 12.5mm×25mm. Each sample is repeated 5 times to confirm the repeatability of the adhesive strength data.

[0046] 2. Anti-mildew and antibacterial experimental test

[0047] The antifungal properties of the adhesives were determined at 30°C and 50% humidity: the adhesives were placed at room temperature and the appearance of mold plaques and the size of the plaques were observed at regular intervals. The antibacterial effects of the adhesives on Escherichia coli ATCC 25922 and Staphylococcus aureus ATCC 6538 were evaluated by co-culture experiments with bacterial samples and solid medium inhibition zone tests. In short, the method for evaluating the effect of the adhesive on bacterial growth was as follows: 0.5 g of the adhesive sample (the control group was a sample without adhesive) was mixed with 100 μL of bacterial solution in 50 mL of phosphate buffer (pH 7.4), shaken evenly at 37°C for 20 min, 20 μL of the bacterial suspension was diluted to an appropriate concentration, transferred to LB agar plates, incubated at 37°C for 18 h, and bacterial growth was monitored and compared with the control sample by colony count. All antibacterial experiments were repeated at least 3 times.

[0048] 3. Experimental results

[0049] like Figure 1 , 2As shown in Figures 3 and 4, the experimental results of the embodiments and comparative examples show that when only hydrolyzed keratin is used to prepare the adhesive (Comparative Example 1), the anti-mildew effect of the adhesive is general. When it is placed indoors for about 7 days, mildew spots begin to appear on the adhesive surface, and it has no inhibitory effect on Escherichia coli and Staphylococcus aureus. However, after adding hydrogen peroxide for modification (Examples 1 and 2), the bonding strength of the prepared adhesive is not only increased significantly, but also has a significant anti-mildew effect (no mildew spots or bacterial infection appear on the surface of the adhesive within 28 days), and the antibacterial property is also significantly improved, especially the antibacterial rate of Escherichia coli reaches 100%. Therefore, the present invention provides a green and effective way to develop multifunctional, high-performance, all-biobased protein adhesives.

[0050] Although the present invention has been disclosed as above in the form of a preferred embodiment, it is not intended to limit the present invention. Anyone familiar with this technology can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the scope of protection of the present invention should be based on the definition of the claims.

Claims

1. A method for preparing an adhesive having mildew-proof and antibacterial properties, characterized in that: The following steps are involved: A. collecting waste keratin, washing, drying, puffing and crushing it to obtain pretreated keratin powder; B. enzymatically hydrolyzing the keratin powder obtained by the pretreatment, and filtering and separating to obtain a hydrolyzate; C. Add hydrogen peroxide solution to the hydrolyzate and stir; D. After freeze-drying, mix with water to obtain an adhesive.

2. The preparation method according to claim 1, characterized in that The waste keratin in step A is one or more of chicken feathers, duck feathers, goose feathers and wool.

3. The preparation method according to claim 1, characterized in that The enzymatic hydrolysis described in step B has an enzyme concentration of 0.3-0.5 g / L.

4. The preparation method according to claim 1, characterized in that The enzyme is one or more of papain, alkaline protease, keratinase, trypsin and pepsin.

5. The preparation method according to claim 4, characterized in that The concentration of keratin powder in the enzymatic hydrolysis in step B is 10-50 g / L.

6. The preparation method according to claim 1, characterized in that The enzymes used in the enzymolysis are a combination of alkaline protease and keratinase, with concentrations of 30 g / L and 50 mg / L respectively.

7. The preparation method according to claim 1, characterized in that The temperature of the enzymolysis process in step B is 30-60°C, the pH is 8-11, and the time is 12-48 hours.

8. The preparation method according to claim 1, characterized in that The concentration of the hydrogen peroxide solution in step C is 30%, and the amount used is 0.1-5 mL of hydrogen peroxide per gram of keratin powder.

9. The preparation method according to claim 8, characterized in that The amount of hydrogen peroxide solution used is 1-5 mL of hydrogen peroxide solution per gram of keratin powder.

10. An adhesive prepared according to any preparation method of claims 1-9.