Environment-friendly wear-resistant cow split PU dry-method leather retanning process

Through the use of modified polyurethane prepolymers and modified negative oxygen ion powder, the problem of formaldehyde and chromium pollution in the leather tanning process is solved, the mechanical properties and water solubility of the leather are improved, and the environmentally friendly and wear-resistant leather retanning effect is achieved. .

CN118932123APending Publication Date: 2024-11-12FENGAN LEATHER
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202411241794.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-05
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing leather tanning process will produce a lot of formaldehyde and chromium pollution, and the mechanical properties of the leather after tanning are poor.

Method used

Using an environmentally friendly wear-resistant beef two-layer PU dry leather retanning process, through the steps of washing, neutralization, retanning and secondary retanning, the retanning agent prepared by modified polyurethane prepolymer is used, combined with the modified negative Oxygen ion powder reduces chromium pollution and improves the mechanical properties of leather.

Benefits of technology

Effectively reduces chromium pollution, improves the mechanical properties and water solubility of the leather, enhances the chemical stability and physical properties of the leather, and removes formaldehyde, improving the flexibility and fullness of the leather.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118932123A_ABST
    Figure CN118932123A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of tanning, provides an environment-friendly wear-resistant cow split PU dry-method leather retanning process, and solves the problems that an existing leather tanning process can generate a large amount of formaldehyde and cause chromium pollution, and tanned leather is poor in mechanical property. Comprising the following steps: 1) washing; 2) primary neutralization; 4-10 parts by weight of a retanning agent, 150-200 parts by weight of water and 0.1-1 part by weight of formic acid are added, the pH is adjusted to be 5-5.5, rotation is conducted for 60-80 min, and liquid is discharged; 4) secondary neutralization; and 5) secondary retanning: adding 100-150 parts by weight of water, 5-10 parts by weight of melamine, 5-10 parts by weight of tannin extract, 1-5 parts by weight of modified negative oxygen ion powder and 0.5-2 parts by weight of phospholipid, adjusting the temperature to 50-55 DEG C, rotating for 60-75 minutes, discharging liquid, and washing with water to finish the retanning process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of tanning, in particular to an environmentally friendly wear-resistant cow split PU dry-process leather retanning process. Background Art

[0002] In the leather making process, tanning is a process that turns raw leather into leather, that is, the leather tanning agent and the leather collagen fibers react to form chemical bonds and produce a cross-linked structure, so that the tanned leather becomes a leather that is durable and has use value. Retanning is the re-tanning of the primary tanned leather. On the one hand, the purpose is to strengthen the tanning effect and supplement the main tanning. On the other hand, it can improve the properties of the leather in many aspects and increase the value of the leather. In leather making, formaldehyde mainly comes from the tanning or retanning process. Aldehyde-containing tanning agents / retanning agents are often used in these two processes, such as aromatic synthetic tanning agents / retanning agents, glutaraldehyde tanning agents / retanning agents, modified glutaraldehyde tanning agents / retanning agents, etc., which will release formaldehyde during use, endangering the health of leather workers.

[0003] Chinese patent application No. 202410092587.7 discloses a kind of cow suede leather that can be directly bonded to a stitch-free machine and its preparation process, wherein the leather blank is sequentially subjected to rewetting, degreasing, deashing, retanning, retanning, first filling, dyeing and fat-liquoring, second filling, fixing, stretching, softening, finishing, trimming, and packaging to obtain cow suede leather that can be directly bonded to a stitch-free machine; the retanning and retanning are as follows: first, a chrome tanning agent is added to retan the leather, the chrome tanning agent content is 1%, and the retanning is completed after rotating the drum for 100 minutes. After the retanning is completed, an acrylic resin-amino silicone oil composite emulsion with a solid content of 30% is used for retanning for 60 minutes, and the mass percentage of amino silicone oil in the acrylic resin-amino silicone oil composite emulsion is 6%, and then a mixed solution of sodium bicarbonate and ammonium bicarbonate is added for neutralization. The invention can significantly improve the softness, strength, and bonding strength of cow suede leather with hot melt adhesive through a specific retanning process and a unique filler and filling process. The obtained cow suede leather can be directly bonded to a stitch-free machine. However, the chrome tanning agent used in this process will produce wastewater containing Cr(III), which is easily oxidized to Cr(VI). Cr(VI) can induce mutations in organisms, directly damage human skin, accumulate in internal organs, and induce various diseases and cancers. Moreover, chrome tanning agents are almost entirely imported in my country and are relatively expensive.

[0004] Chinese patent application No. 202311292374.0 discloses a method for improving the effect of retanning and filling chrome-free tanned leather with leather scrap protein. The invention method is that the chrome-free tanned leather is conventionally neutralized and then filled with leather scrap protein filler, and after fat-liquoring, it is treated at a temperature greater than or equal to -200°C and less than or equal to -100°C for 1min to 48h, and dried; wherein the chrome-free tanned leather is aldehyde tanned leather and epoxy resin tanned leather; the leather scrap protein filler is a protein obtained by treating leather scraps with acid-base, acid-enzyme, alkali-enzyme or acid-base-enzyme, and then modified to obtain a retanning filling material; the modification is modification with formaldehyde, glyoxal, casein, polyurethane or phenol. The invention uses deep cold treatment and then dries the tanned leather filled with leather scrap protein filler and fat-liquored, which can make water form a large number of small ice crystals in the pores of the leather collagen fiber network, which will not damage the stable supporting structure of the macromolecular protein, and improve the plumpness and resilience of the tanned leather. Compared with the tanned leather obtained by the traditional technical route, the tanned leather prepared by the shavings protein retanning route has a 50% higher fullness, and the resilience is basically not affected, and the lightness is significantly improved. However, the aldehyde tanning agent used in the invention will release formaldehyde, which is harmful to the health of tanners and users. Summary of the invention

[0005] Therefore, in view of the above problems, the present invention provides an environmentally friendly wear-resistant cow split PU dry leather retanning process to solve the problems that the existing leather tanning process produces a large amount of formaldehyde, causes chromium pollution, and the mechanical properties of the tanned leather are poor.

[0006] To achieve the above object, the present invention adopts the following technical solutions:

[0007] An environmentally friendly wear-resistant cow split PU dry leather retanning process comprises the following steps:

[0008] S1. Washing: washing the aldehyde-tanned cow split PU leather and draining the liquid;

[0009] S2, primary neutralization: add 150-200 parts by weight of water, 0.8-2 parts by weight of NaHCO 3 , 1-2 parts by weight of CH 3 COONa and 8-10 parts by weight of NaCl, transfer for 1-2 hours, and adjust the pH to 7-7.5;

[0010] S3, primary retanning: add 4-10 parts by weight of retanning agent, 150-200 parts by weight of water and 0.1-1 parts by weight of formic acid, adjust pH to 5-5.5, rotate for 60-80 minutes, and drain;

[0011] S4, secondary neutralization: add 200-300 parts by weight of water, 0.8-2 parts by weight of NaHCO 3 , 1-2 parts by weight of CH3 COONa and 8-10 parts by weight of NaCl, transfer for 1-2 hours, and adjust the pH to 7-7.5;

[0012] S5, secondary retanning: add 100-150 parts of water, 5-10 parts of melamine, 5-10 parts of tannin extract, 1-5 parts of modified negative oxygen ion powder, 0.5-2 parts of phospholipid by weight, adjust the temperature to 50-55 ° C, rotate for 60-75 minutes, drain and wash with water to complete the retanning process;

[0013] Wherein, the preparation method of the retanning agent is:

[0014] I. According to the molar ratio of polypropylene glycol, isophorone diisocyanate and the first modifier being 10:5:0.5-1, polypropylene glycol, isophorone diisocyanate and the first modifier are weighed, mixed evenly, reacted for 4-5 hours under the condition of using dibutyltin dilaurate as a catalyst and raising the temperature to 60-70° C. to obtain a first intermediate reactant;

[0015] II. Add a second modifier to the first intermediate reactant obtained in step I, mix well, raise the temperature to 80-90° C., react for 3-4 hours, and obtain a second intermediate reactant;

[0016] III. Add ethanol to the second intermediate reactant obtained in step II, mix well, add a neutralizer after reacting for 1-2 hours, add 10-30 parts by weight of deionized water for emulsification, and treat through a dialysis bag to obtain the retanning agent.

[0017] Furthermore, the preparation process of the first modifier is:

[0018] a. Add L-threonine in Cl 2 Performing a substitution reaction under light conditions to obtain 2-amino-3,4-dihydroxy-carboxybutyric acid, then adding the 2-amino-3,4-dihydroxy-carboxybutyric acid into 100-200 parts by weight of tetrahydrofuran to dissolve it to obtain a first mixture for later use;

[0019] b. In an oil bath, add the trichloromethyl carbonate to the first mixture in a molar ratio of 2-amino-3,4-dihydroxy-carboxybutyric acid to trichloromethyl carbonate of 5-6:3, raise the temperature to 60-65° C., react for 1-2 hours, remove excess solvent after the solution becomes clear, and recrystallize to obtain the first modifier.

[0020] Furthermore, the structural formula of the second modifier is as shown in formula (1):

[0021]

[0022] In formula (1), the number n is an integer of 7-15.

[0023] Furthermore, the preparation process of the modified negative oxygen ion powder is as follows: according to the mass ratio of nano-tourmaline negative oxygen ion powder and anhydrous ethanol being 1:3-5, the nano-tourmaline negative oxygen ion powder is added to anhydrous ethanol, the temperature is increased to 70-80°C, the rotation speed is 1000-1200r / min, and stirring is performed for 3-4h, and then 1-3 parts by weight of silane coupling agent and 5-10 parts by weight of sodium dodecylbenzene sulfonate are added, the pH is adjusted to 3.5-4, the temperature is adjusted to 30-35°C, stirring is performed for 30-45min, and the reaction is allowed to stand for 10-12h. After filtering out the supernatant, washing, grinding, and drying are performed to obtain the modified negative oxygen ion powder.

[0024] Furthermore, the neutralizing agent is triethylamine.

[0025] Furthermore, the water washing is as follows: at room temperature, 200-300 parts by weight of water is added into a rotating drum, and the drum is rotated for 30-45 minutes.

[0026] Furthermore, the retanning process is carried out in a rotary drum at a rotation speed of 5-15 r / min.

[0027] By adopting the above technical solution, the beneficial effects of the present invention are:

[0028] 1. Prepare a polyurethane prepolymer using polypropylene glycol and isophorone diisocyanate as raw materials, and simultaneously modify the polyurethane prepolymer with a first modifier and a second modifier to obtain the retanning agent, which is an aldehyde tanning agent, replacing the use of a chrome tanning agent to reduce chrome pollution. Among them, the first modifier is It is prepared from natural amino acid (L-threonine) as raw material and contains two alcoholic hydroxyl groups, which can give the retanning agent higher hydrophilicity, thereby improving the water solubility of the retanning agent and making it easier for the retanning agent to penetrate into the leather and cross-link with the leather. It can be made from animal and plant fatty oleic acid, which is green, environmentally friendly and easy to obtain. The number of n is an integer of 7-15. The presence of long carbon chains can fill the pores in the dermal collagen fibers with fat, making the fibers gather into bundles with thick diameters, becoming tougher and stronger, not easy to tear, with high thermal stability, and rich leather feel; it contains a large number of amide groups Under neutral or alkaline conditions, it can undergo a methylation reaction with free formaldehyde in leather to generate hydroxymethyl compounds, thereby achieving the function of removing formaldehyde.

[0029] 2. Epoxy groups contained in both the first modifier and the second modifier The obtained retanning agent has high reactivity and can directly react with the amino groups on the leather collagen fibers, so that it reacts with the functional groups on the leather collagen fibers to generate a solidified product with a cross-linked structure, which plays a major tanning role and is beneficial to enhancing the chemical stability and physical and mechanical properties of the leather.

[0030] 3. The second modifier is used as an anionic chain extender, and the first modifier is used as a cationic chain extender. The amphoteric polyurethane retanning agent can not only solve the problem of single anionic retanning agent on leather, but also solve the defect of cumbersome operation of single cationic retanning agent, effectively solve the problem of loose surface, make the finished leather plump, flexible and elastic, and improve the subsequent anionic dyeing rate.

[0031] 4. The modified negative oxygen ion powder is added during the secondary retanning. The modified negative oxygen ion powder can stably exist in the leather, can continuously release negative oxygen ions, will not affect the mechanical properties of the leather, and can further remove formaldehyde and odor from the leather. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 It is the organic synthesis diagram of the retanning agent in Example 1 of the present invention. DETAILED DESCRIPTION

[0033] Example 1

[0034] refer to Figure 1 , an environmentally friendly wear-resistant cow split PU dry leather retanning process, comprising the following steps:

[0035] (1) Washing: Add 200 parts by weight of water into a drum at room temperature and rotate for 30 minutes to wash the aldehyde-tanned cow split PU leather and then drain the liquid;

[0036] (2) Primary neutralization: Add 150 parts by weight of water, 0.8 parts by weight of NaHCO 3 , 1 part by weight of CH 3 COONa and 8 parts by weight of NaCl, transfer for 1 hour, and adjust the pH to 7;

[0037] (3) Primary retanning

[0038] (3-1) Preparation of the first modifier

[0039] a. Add L-threonine in Cl 2 Performing a substitution reaction under light conditions to obtain 2-amino-3,4-dihydroxy-carboxybutyric acid, then adding the 2-amino-3,4-dihydroxy-carboxybutyric acid into 100 parts by weight of tetrahydrofuran to dissolve it to obtain a first mixture for later use;

[0040] b. In an oil bath, the trichloromethyl carbonate is added to the first mixture in a molar ratio of 2-amino-3,4-dihydroxy-carboxybutyric acid to trichloromethyl carbonate of 5:3, the temperature is raised to 60° C., the reaction is performed for 1 hour, and after the solution is clarified, the excess solvent is removed, and the first modifier is obtained by recrystallization;

[0041] (3-2) Preparation of retanning agent

[0042] I. According to the molar ratio of polypropylene glycol, isophorone diisocyanate and the first modifier being 10:5:1, polypropylene glycol, isophorone diisocyanate and the first modifier are weighed, mixed evenly, and reacted for 4 hours under the condition of using dibutyltin dilaurate as a catalyst and raising the temperature to 60° C. to obtain a first intermediate reactant;

[0043] II. Add a second modifier to the first intermediate reactant obtained in step I, mix well, raise the temperature to 80° C., react for 3 hours, and obtain a second intermediate reactant;

[0044] III. Add ethanol to the second intermediate reactant obtained in step II, mix well, add triethylamine after reacting for 1 hour, add 10 parts by weight of deionized water for emulsification, and treat through a dialysis bag to obtain the retanning agent;

[0045] Wherein, the structural formula of the second modifier is shown in formula (2):

[0046]

[0047] The organic synthesis diagram of the retanning agent is as follows Figure 1 As shown;

[0048] (3-3) adding 4 parts by weight of the retanning agent, 150 parts by weight of water and 0.1 parts by weight of formic acid, adjusting the pH to 5.5, rotating for 60 minutes, and draining;

[0049] (4) Secondary neutralization: Add 200 parts by weight of water, 0.8 parts by weight of NaHCO 3 , 1 part by weight of CH 3 COONa and 8 parts by weight of NaCl, transfer for 1.5 hours, and adjust the pH to 7;

[0050] (5) Secondary tanning

[0051] (5-1) Preparation of modified negative oxygen ion powder

[0052] According to the mass ratio of nano-tourmaline negative oxygen ion powder to anhydrous ethanol of 1:3, the nano-tourmaline negative oxygen ion powder is added to anhydrous ethanol, the temperature is increased to 70°C, the rotation speed is 1000r / min, and the mixture is stirred for 3h, then 1 part by weight of a silane coupling agent and 5 parts by weight of sodium dodecylbenzene sulfonate are added, the pH is adjusted to 3.5, the temperature is adjusted to 30°C, the mixture is stirred for 30min, the mixture is allowed to stand for reaction for 10h, the supernatant is removed by suction, and then the mixture is washed, ground, and dried to obtain the modified negative oxygen ion powder;

[0053] (5-2) Add 100 parts of water, 5 parts of melamine, 5 parts of tannin extract, 1 part of modified negative oxygen ion powder, and 0.5 parts of phospholipid by weight, adjust the temperature to 50°C, rotate for 60 minutes, drain and wash with water, add 200 parts by weight of water in the drum at room temperature, rotate for 30 minutes, and complete the retanning process. The retanning process is carried out in a rotating drum at a rotation speed of 5r / min.

[0054] Example 2

[0055] An environmentally friendly wear-resistant cow split PU dry leather retanning process comprises the following steps:

[0056] (1) Washing: Add 250 parts by weight of water into a drum at room temperature and rotate for 40 minutes to wash the aldehyde-tanned cow split PU leather and then drain the liquid;

[0057] (2) Primary neutralization: Add 180 parts by weight of water, 1 part by weight of NaHCO 3 , 1.5 parts by weight of CH 3 COONa and 8 parts by weight of NaCl, transfer for 1.5 hours, and adjust the pH to 7;

[0058] (3) Primary retanning

[0059] (3-1) Preparation of the first modifier

[0060] a. Add L-threonine in Cl 2 Performing a substitution reaction under light conditions to obtain 2-amino-3,4-dihydroxy-carboxybutyric acid, and then adding the 2-amino-3,4-dihydroxy-carboxybutyric acid into 150 parts by weight of tetrahydrofuran to dissolve it to obtain a first mixture for later use;

[0061] b. In an oil bath, the trichloromethyl carbonate is added to the first mixture in a molar ratio of 5:3 between the 2-amino-3,4-dihydroxy-carboxybutyric acid and trichloromethyl carbonate, the temperature is raised to 65° C., the reaction is carried out for 2 hours, and after the solution is clarified, the excess solvent is removed, and the first modifier is obtained by recrystallization;

[0062] (3-2) Preparation of retanning agent

[0063] I. According to the molar ratio of polypropylene glycol, isophorone diisocyanate and the first modifier being 10:5:1, polypropylene glycol, isophorone diisocyanate and the first modifier are weighed, mixed evenly, reacted for 4.5 hours under the condition of using dibutyltin dilaurate as a catalyst and raising the temperature to 65° C. to obtain a first intermediate reactant;

[0064] II. Add a second modifier to the first intermediate reactant obtained in step I, mix well, raise the temperature to 85° C., react for 4 hours, and obtain a second intermediate reactant;

[0065] III. Add ethanol to the second intermediate reactant obtained in step II, mix well, add triethylamine after reacting for 2 hours, add 20 parts by weight of deionized water for emulsification, and treat through a dialysis bag to obtain the retanning agent;

[0066] Wherein, the structural formula of the second modifier is shown in formula (3):

[0067]

[0068] (3-3) adding 8 parts by weight of the retanning agent, 180 parts by weight of water and 0.5 parts by weight of formic acid, adjusting the pH to 5, rotating for 70 minutes, and draining;

[0069] (4) Secondary neutralization: Add 250 parts by weight of water, 1 part by weight of NaHCO 3 , 1 part by weight of CH 3 COONa and 8 parts by weight of NaCl, transfer for 2 hours, and adjust the pH to 7;

[0070] (5) Secondary tanning

[0071] (5-1) Preparation of modified negative oxygen ion powder

[0072] According to the mass ratio of nano-tourmaline negative oxygen ion powder to anhydrous ethanol of 1:3, the nano-tourmaline negative oxygen ion powder is added to anhydrous ethanol, the temperature is increased to 75°C, the rotation speed is 1100r / min, and the mixture is stirred for 3.5h, then 2 parts by weight of a silane coupling agent and 8 parts by weight of sodium dodecylbenzene sulfonate are added, the pH is adjusted to 4, the temperature is adjusted to 35°C, the mixture is stirred for 45min, the mixture is allowed to react for 12h, the supernatant is removed by suction, and then the mixture is washed, ground, and dried to obtain the modified negative oxygen ion powder;

[0073] (5-2) Add 120 parts by weight of water, 8 parts of melamine, 8 parts of tannin extract, 3 parts of modified negative oxygen ion powder, and 1 part of phospholipid, adjust the temperature to 55°C, rotate for 75 minutes, drain and wash with water, add 250 parts by weight of water in the drum at room temperature, rotate for 35 minutes, and complete the retanning process. The retanning process is carried out in a rotating drum at a rotation speed of 10r / min.

[0074] Example 3

[0075] An environmentally friendly wear-resistant cow split PU dry leather retanning process comprises the following steps:

[0076] (1) Washing: At room temperature, add 300 parts by weight of water into a drum, rotate for 45 minutes, wash the aldehyde-tanned cow split PU leather with water, and then drain the liquid;

[0077] (2) Primary neutralization: Add 200 parts by weight of water, 2 parts by weight of NaHCO 3 , 2 parts by weight of CH 3 COONa and 10 parts by weight of NaCl, transfer for 2 hours, and adjust the pH to 7.5;

[0078] (3) Primary retanning

[0079] (3-1) Preparation of the first modifier

[0080] a. Add L-threonine in Cl 2 Performing a substitution reaction under light conditions to obtain 2-amino-3,4-dihydroxy-carboxybutyric acid, and then adding the 2-amino-3,4-dihydroxy-carboxybutyric acid into 200 parts by weight of tetrahydrofuran to dissolve it to obtain a first mixture for later use;

[0081] b. In an oil bath, the trichloromethyl carbonate is added to the first mixture in a molar ratio of 5:3 between the 2-amino-3,4-dihydroxy-carboxybutyric acid and trichloromethyl carbonate, the temperature is raised to 65° C., the reaction is carried out for 2 hours, and after the solution is clarified, the excess solvent is removed, and the first modifier is obtained by recrystallization;

[0082] (3-2) Preparation of retanning agent

[0083] I. According to the molar ratio of polypropylene glycol, isophorone diisocyanate and the first modifier being 10:5:1, polypropylene glycol, isophorone diisocyanate and the first modifier are weighed, mixed evenly, reacted for 5 hours under the condition of using dibutyltin dilaurate as a catalyst and raising the temperature to 70° C. to obtain a first intermediate reactant;

[0084] II. Add a second modifier to the first intermediate reactant obtained in step I, mix well, raise the temperature to 90° C., react for 4 hours, and obtain a second intermediate reactant;

[0085] III. Add ethanol to the second intermediate reactant obtained in step II, mix well, add a neutralizer after reacting for 2 hours, add 30 parts by weight of deionized water for emulsification, and treat through a dialysis bag to obtain the retanning agent;

[0086] Wherein, the structural formula of the second modifier is shown in formula (4):

[0087]

[0088] (3-3) adding 10 parts by weight of the retanning agent, 200 parts by weight of water and 1 part by weight of formic acid, adjusting the pH to 5.5, rotating for 80 minutes, and draining;

[0089] (4) Secondary neutralization: Add 300 parts by weight of water, 2 parts by weight of NaHCO 3 , 2 parts by weight of CH 3 COONa and 10 parts by weight of NaCl, transfer for 2 hours, and adjust the pH to 7.5;

[0090] (5) Secondary tanning

[0091] (5-1) Preparation of modified negative oxygen ion powder

[0092] According to the mass ratio of nano-tourmaline negative oxygen ion powder to anhydrous ethanol of 1:5, the nano-tourmaline negative oxygen ion powder is added to anhydrous ethanol, the temperature is increased to 80°C, the rotation speed is 1200r / min, and stirring is performed for 4h, and then 3 parts by weight of silane coupling agent and 10 parts by weight of sodium dodecylbenzene sulfonate are added, the pH is adjusted to 4, the temperature is adjusted to 35°C, stirring is performed for 45min, and the reaction is allowed to stand for 12h, and the supernatant is removed by suction, and then washed, ground, and dried to obtain the modified negative oxygen ion powder;

[0093] (5-2) Add 150 parts of water, 10 parts of melamine, 10 parts of tannin extract, 5 parts of modified negative oxygen ion powder, and 2 parts of phospholipids by weight, adjust the temperature to 55°C, rotate for 75 minutes, drain and wash with water, add 300 parts by weight of water in the drum at room temperature, rotate for 45 minutes, and complete the retanning process. The retanning process is carried out in a rotating drum at a rotation speed of 15r / min.

[0094] Comparative Example 1

[0095] The difference from Example 1 is that: instead of using the retanning agent and modified negative oxygen ion powder of Example 1, 4% of commercially known retanning agent MB-1, 3% of retanning agent RTD, and 2% of melamine resin type synthetic retanning agent are added. Other technical solutions are the same as those of Example 1.

[0096] Table 1 is the test data of the products of Example 1, Example 2, Example 3 and Comparative Example 1.

[0097] Table 1

[0098]

[0099]

[0100] The free formaldehyde content in Table 1 is tested in accordance with the national standard "Determination of Formaldehyde Content of Leather and Fur" (GB / T19941.2-2019).

[0101] The free formaldehyde limit value is classified and judged according to the "Limits of Hazardous Substances in Leather and Fur" (GB 20400-2006).

[0102] As can be seen from Table 1, the free formaldehyde content of the leather treated by the first retanning process of the present technical solution is 60.13-62.34 mg / kg, which is lower than 75 mg / kg, and meets the product requirements for direct contact with the skin (Class B); the free formaldehyde content of the leather treated by the second retanning process is ND (lower than 20 mg / kg), indicating that it is not detected, and meets the product requirements for infant products (Class A). In addition, the products of Examples 1, 2, and 3 all have good mechanical properties.

[0103] Although the present invention has been specifically shown and described in conjunction with the preferred embodiments, it should be understood by those skilled in the art that various changes may be made to the present invention in form and details without departing from the spirit and scope of the present invention as defined by the appended claims, all of which are within the scope of protection of the present invention.

Claims

1. An environmentally friendly wear-resistant cow split PU dry leather retanning process, characterized in that: The following steps are involved: S1. Washing: washing the aldehyde-tanned cow split PU leather and draining the liquid; S2, primary neutralization: add 150-200 parts by weight of water, 0.8-2 parts by weight of NaHCO3, 1-2 parts by weight of CH3COONa and 8-10 parts by weight of NaCl, rotate for 1-2h, and adjust the pH to 7-7.5; S3, primary retanning: add 4-10 parts by weight of retanning agent, 150-200 parts by weight of water and 0.1-1 parts by weight of formic acid, adjust pH to 5-5.5, rotate for 60-80 minutes, and drain; S4, secondary neutralization: add 200-300 parts by weight of water, 0.8-2 parts by weight of NaHCO3, 1-2 parts by weight of CH3COONa and 8-10 parts by weight of NaCl, rotate for 1-2 hours, and adjust the pH to 7-7.5; S5, secondary retanning: add 100-150 parts of water, 5-10 parts of melamine, 5-10 parts of tannin extract, 1-5 parts of modified negative oxygen ion powder, 0.5-2 parts of phospholipid by weight, adjust the temperature to 50-55 ° C, rotate for 60-75 minutes, drain and wash with water to complete the retanning process; Wherein, the preparation method of the retanning agent is: I. According to the molar ratio of polypropylene glycol, isophorone diisocyanate and the first modifier being 10:5:0.5-1, polypropylene glycol, isophorone diisocyanate and the first modifier are weighed, mixed evenly, reacted for 4-5 hours under the condition of using dibutyltin dilaurate as a catalyst and raising the temperature to 60-70° C. to obtain a first intermediate reactant; II. Add a second modifier to the first intermediate reactant obtained in step I, mix well, raise the temperature to 80-90° C., react for 3-4 hours, and obtain a second intermediate reactant; III. Add ethanol to the second intermediate reactant obtained in step II, mix well, add a neutralizer after reacting for 1-2 hours, add 10-30 parts by weight of deionized water for emulsification, and treat through a dialysis bag to obtain the retanning agent.

2. The environmentally friendly wear-resistant cow split PU dry leather retanning process according to claim 1, characterized in that: The preparation process of the first modifier is: a. subjecting L-threonine to a substitution reaction under Cl2 illumination to obtain 2-amino-3,4-dihydroxy-carboxybutyric acid, and then adding the 2-amino-3,4-dihydroxy-carboxybutyric acid to 100-200 parts by weight of tetrahydrofuran to dissolve it to obtain a first mixture for standby use; b. In an oil bath, add the trichloromethyl carbonate to the first mixture in a molar ratio of 2-amino-3,4-dihydroxy-carboxybutyric acid to trichloromethyl carbonate of 5-6:3, raise the temperature to 60-65° C., react for 1-2 hours, remove excess solvent after the solution becomes clear, and recrystallize to obtain the first modifier.

3. The environmentally friendly wear-resistant cow split PU dry leather retanning process according to claim 1, characterized in that: The structural formula of the second modifier is shown in formula (1): In formula (1), the number n is an integer of 7-15.

4. The environmentally friendly wear-resistant cow split PU dry leather retanning process according to claim 1, characterized in that: The preparation process of the modified negative oxygen ion powder is as follows: according to the mass ratio of nano-tourmaline negative oxygen ion powder to anhydrous ethanol of 1:3-5, the nano-tourmaline negative oxygen ion powder is added to anhydrous ethanol, the temperature is increased to 70-80°C, the rotation speed is 1000-1200r / min, stirring is performed for 3-4h, and then 1-3 parts by weight of a silane coupling agent and 5-10 parts by weight of sodium dodecylbenzene sulfonate are added, the pH is adjusted to 3.5-4, the temperature is adjusted to 30-35°C, stirring is performed for 30-45min, standing for reaction for 10-12h, filtering to remove the upper clear liquid, washing, grinding and drying to obtain the modified negative oxygen ion powder.

5. The environmentally friendly wear-resistant cow split PU dry leather retanning process according to claim 1, characterized in that: The neutralizing agent is triethylamine.

6. The environmentally friendly wear-resistant cow split PU dry leather retanning process according to claim 1, characterized in that: The water washing comprises: adding 200-300 parts by weight of water into a rotating drum at room temperature, and rotating for 30-45 minutes.

7. The environmentally friendly wear-resistant cow split PU dry leather retanning process according to claim 1, characterized in that: The retanning process is carried out in a rotary drum at a rotation speed of 5-15 r / min.

Citation Information

Patent Citations

  • Improvements in the production of tanning agents

    GB817101A