Production method for controlling depth of decarburized layer of cold heading steel wire rod of high-strength fastener

By removing water vapor, heating and rolling and cooling, the depth of the decarbonization layer of the cold heading steel strip of high-strength fastener is controlled, which solves the problem of the impact of the decarbonization layer in the heating process, improves the material performance and service life, and achieves the realization of the material. The uniformity of metallographic structure.

CN118932152APending Publication Date: 2024-11-12HUNAN VALIN XIANGTAN IRON & STEEL CO LTD

Patent Information

Application Number
CN202411017344.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The cold heading steel strips with high-strength fasteners are prone to decarbonization layers during the production process, resulting in a decrease in material performance and shortening service life. Especially in the heating process, the influence of water vapor and oxide layer structure is greater, making it difficult to effectively control decarbonization. layer depth.

Method used

Through the process steps of removing water vapor, heating and controlling rolling and cooling, the chemical composition and heating conditions of the blank are controlled, the content of water vapor and oxide layers in the furnace is reduced, and low-temperature rolling and slow cooling are adopted to ensure that the depth of the decarbonized layer is less than 0.6%D.

Benefits of technology

It effectively reduces the depth of the surface decarbonization layer of the cold heading steel strip, improves the hardness, wear resistance and fatigue resistance of the material, extends the service life of the parts, and achieves fine uniformity of metallographic structure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118932152A_ABST
    Figure CN118932152A_ABST
Patent Text Reader

Abstract

The invention discloses a method for controlling the depth of a decarburized layer of a cold heading steel wire rod of a high-strength fastener. The cold heading steel wire rod comprises the following chemical components in percentage by weight: 0.32-0.38% of C, 0.15-0.30% of Si, 0.60-0.90% of Mn, less than or equal to 0.020% of P, less than or equal to 0.010% of S, more than or equal to 0.020% of Al, 0.80-1.10% of Cr, 0.15-0.30% of Mo and the balance of Fe and inevitable impurities. According to the invention, through the key process steps of water vapor removal, heating, controlled rolling and controlled cooling, the wire rod without full decarburization is obtained, and the total decarburization layer depth of the wire rod is less than 0.6% D. The method is characterized in that blank decarburization generated in the heating process is controlled by reducing the water vapor content in the furnace, reducing the residual oxygen content and heating temperature through blank drying and coal gas dehydration; the low spinning temperature is obtained through low-temperature rolling; heat collecting and coiling are carried out at a proper roller way speed, and temperature easily generated by a decarburization layer is avoided; the heat collecting coil enters the heat preservation vestibule for slow cooling, stress can be effectively released, and the plasticity of the wire rod is improved. The metallographic structure of the wire rod is fine and uniform, and a decarburized layer of the wire rod is greatly improved, so that the usability of the wire rod is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of metallurgy and relates to a production method for controlling the depth of a decarburized layer of a cold-headed steel wire rod of a high-strength fastener. Background Art

[0002] The presence of decarburized layer will seriously affect the performance and service life of the material. Decarburization leads to a decrease in the carbon content of the surface layer. The difference in the organization between the surface layer and the core may cause internal stress, affect the hardness and strength of the material, reduce the wear resistance, cutting performance, plasticity and fatigue resistance of the material, and may cause cracking during cold heading. The decarburized layer may reduce the impact toughness of the material and reduce the service life of the parts. Especially when the ferrite is completely decarburized on the surface of the material, its fatigue limit can be reduced by 50%.

[0003] The carbon content of cold heading steel used to produce high-strength fasteners is mostly above 0.30%, and the decarburization trend is obvious. High-strength fasteners have very high requirements for the surface decarburization of wire rods. Not only does it require that there is no full decarburization layer, but also that the total decarburization layer depth is less than 0.8%D or even lower. D is the nominal diameter of the wire rod, in mm, D = depth / diameter*100%.

[0004] In the steel production industry, the process that has the greatest impact on decarbonization is the heating process, among which the most influencing factors are the furnace atmosphere (H2O(g) content, residual oxygen content), heating temperature, and time in the furnace; the second most influential process is the cooling process.

[0005] The main way that H2O(g) affects the decarburization of metal surface is that it affects the structure of the oxide layer in the mixed atmosphere in the furnace. The presence of H2O(g) changes the composition and structure of the oxide layer. The thickness of the FeO layer in the wet air environment accounts for about 60%, which greatly improves the permeability of the decarburization medium. The structure of FeO is relatively loose, which will increase the degree of decarburization. In actual production, reducing the H2O(g) content in the furnace gas can greatly reduce surface decarburization and reduce oxidation burning.

[0006] In order to improve the quality of cold heading steel wire rod, how to reduce the surface decarburization of cold heading steel coil is an urgent problem to be solved. Therefore, it is of great significance to conduct technical research and development on the production technology of controlling the decarburization layer of wire rod. Summary of the invention

[0007] In order to solve the above technical problems, the present invention provides a method for controlling the production of high-strength fastener cold heading steel wire rods, wherein the key process steps include (1) removing water vapor; (2) heating; and (3) controlled rolling and controlled cooling to obtain wire rods without complete decarburization and with a total decarburization layer depth of less than 0.6%D.

[0008] The technical solution of the present invention is a production method for controlling the decarburization depth of a cold heading steel wire rod for high-strength fasteners, characterized in that the method comprises the following main process steps: removing water vapor from a billet, heating, controlled rolling and controlled cooling, wherein the chemical composition weight percentage of the cold heading steel wire rod is: C: 0.32-0.38%, Si: 0.15-0.30%, Mn: 0.60-0.90%, P≤0.020%, S≤0.010%, Al≥0.020%, Cr: 0.80-1.10%, Mo: 0.15-0.30%, and the rest is Fe and unavoidable impurities;

[0009] In certain embodiments of the present invention, the content of C is 0.34-0.36%, for example, 0.34%, 0.35%, 0.36%;

[0010] The content of Si is 0.20-0.23%, for example, 0.20%, 0.21%, 0.23%;

[0011] The content of Mn is 0.68% to 0.70%, for example, 0.68%, 0.69%, 0.70%;

[0012] P content ≤ 0.014%, for example 0.013% or 0.014%;

[0013] The content of S is ≤ 0.004%, for example 0.003% or 0.004%;

[0014] The content of Al is ≥ 0.028%, such as 0.028%, 0.030%, 0.032%;

[0015] The content of Cr is 0.80-1.10%, for example, 0.89%, 0.90%, 0.92%;

[0016] The content of Mo is 0.16-0.17%, for example, 0.16% or 0.17%.

[0017] In the present invention, the billet dehumidification means that the billet enters the furnace through a roller drying box; the high coke mixed gas is dehydrated through a gas dehydrator before entering the heating furnace, thereby reducing the water vapor content in the furnace and controlling the decarburization of the billet generated during the heating process;

[0018] In the present invention, the heating: the soaking section is 1050°C to 1100°C, the furnace time is 80 to 120 minutes, and the residual oxygen content and heating temperature are reduced to control the decarburization of the billet generated during the heating process;

[0019] In the present invention, the controlled rolling and controlled cooling are as follows: the starting rolling temperature is 960°C to 1020°C, the spinning temperature is 760°C to 820°C, the hot coiling temperature is 670°C to 720°C, and the hot coiling is then placed in a heat preservation corridor for slow cooling.

[0020] In the present invention, the H2O (g) content in the furnace is ≤ 6 g·m-3;

[0021] In the present invention, the residual oxygen content of the heating furnace is ≤2.5%;

[0022] Beneficial effects of the present invention:

[0023] (1) Control the decarburization of the billet during the heating process by drying the billet and dehydrating the coal gas to reduce the water vapor content in the furnace, lower the residual oxygen content, and the heating temperature;

[0024] (2) A lower spinning temperature is obtained by low-temperature rolling; hot coiling is performed by controlling the roller speed to avoid the temperature that is easily generated in the decarburized layer;

[0025] (3) After hot rolling, the wire rod is put into the insulation corridor for slow cooling, which can effectively release stress and improve the plasticity of the wire rod.

[0026] (4) The wire rod metallographic structure is fine and uniform, which greatly improves the decarburization layer of the wire rod and thus improves the performance of the wire rod. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0028] Figure 1 The decarburization layer diagram of the wire rod (decarburization layer 0.07 mm) was obtained by adopting the method of Example 1 for the Φ16 mm specification;

[0029] Figure 2 The decarburization layer diagram of the wire rod (decarburization layer 0.132 mm) was obtained by using the method of Comparative Example 1 for the Φ16 mm specification;

[0030] Figure 3 The decarburization layer diagram of the wire rod (decarburization layer 0.06 mm) was obtained by adopting the method of Example 2 for the Φ12 mm specification;

[0031] Figure 4 The decarburization layer diagram of the wire rod was obtained by using the method of comparative example 2 for the Φ12mm specification (decarburization layer 0.91mm);

[0032] Figure 5 The decarburization layer diagram of the wire rod (decarburization layer 0.05 mm) was obtained by adopting the method of Example 3 for the specification of Φ10 mm;

[0033] Figure 6 The decarburization layer diagram of the wire rod (decarburization layer 0.09 mm) was obtained by using the comparative example 3 method for the Φ10 mm specification; DETAILED DESCRIPTION

[0034] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0035] Embodiments of the present invention are described in detail below, examples of which are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are intended to be used to explain the present invention, and should not be construed as limiting the present invention.

[0036] Design Examples 1 to 3 and Comparative Examples 1 to 3, the weight percentages of the components of the cold heading steel wire rod in Examples 1-3 and Comparative Examples 1-3 are shown in Table 1.

[0037] Table 1 Comparison of composition contents of different embodiments and comparative examples (wt.%)

[0038]

[0039] The examples and comparative examples were produced according to the process of 180*180 mm square billet - removing moisture - heating - controlled rolling and controlled cooling.

[0040] Embodiment 1:

[0041] A method for controlling the depth of decarburized layer of cold heading steel wire rod for high strength fasteners, with rolling specification of Φ16mm. The chemical composition weight percentage of cold heading steel wire rod is: C=0.35%, Si=0.20%, Mn=0.68%, P=0.013%, S=0.003%, Al=0.028%, Cr=0.92%, Mo=0.16%, and the rest is Fe and unavoidable impurities. The process steps include:

[0042] (1) Removal of moisture: The billet enters the furnace through a roller drying box; the high coke mixed gas is dehydrated by a gas dehydrator before entering the heating furnace; the H2O (g) content in the furnace is 3 g·m -3 ;

[0043] (2) Heating: Soaking section 1070°C, residual oxygen content in the heating furnace ≤ 1.5%, furnace time 98 min;

[0044] (3) Controlled rolling and controlled cooling: the starting rolling temperature is 1002℃, the wire drawing temperature is 782℃, and the hot rolled coil is put into the insulation corridor at 695℃ for slow cooling.

[0045] Wire rod decarburization layer 0.07mm, see Figure 1 .

[0046] Embodiment 2:

[0047] A method for controlling the depth of decarburized layer of cold heading steel wire rod for high strength fasteners, with rolling specification of Φ12mm. The chemical composition weight percentage of cold heading steel wire rod is: C=0.34%, Si=0.21%, Mn=0.70%, P=0.014%, S=0.003%, Al=0.030%, Cr=0.90%, Mo=0.16%, and the rest is Fe and unavoidable impurities. The process steps include:

[0048] (1) Removal of moisture: The billet enters the furnace through a roller drying box; the high coke mixed gas is dehydrated by a gas dehydrator before entering the heating furnace; the H2O (g) content in the furnace is 3.5 g·m -3 ;

[0049] (2) Heating: Soaking section 1065°C, residual oxygen content in the heating furnace ≤ 1.36%, furnace time 102 min;

[0050] (3) Controlled rolling and controlled cooling: the starting rolling temperature is 995℃, the wire drawing temperature is 785℃, and the hot rolled coil is put into the insulation corridor at 702℃ for slow cooling.

[0051] Wire rod decarburization layer 0.06mm, see Figure 3 .

[0052] Embodiment 3:

[0053] A method for controlling the depth of decarburized layer of cold heading steel wire rod for high strength fasteners, with rolling specification of Φ10mm. The chemical composition weight percentage of cold heading steel wire rod is: C=0.36%, Si=0.23%, Mn=0.69%, P=0.013%, S=0.004%, Al=0.032%, Cr=0.89%, Mo=0.17%, and the rest is Fe and unavoidable impurities. The process steps include:

[0054] (1) Removal of moisture: The billet enters the furnace through a roller drying box; the high coke mixed gas is dehydrated by a gas dehydrator before entering the heating furnace; the H2O (g) content in the furnace is 4.2 g·m -3 ;

[0055] (2) Heating: soaking section 1080°C, residual oxygen content in the heating furnace ≤ 1.66%, furnace time 105 min;

[0056] (3) Controlled rolling and controlled cooling: the starting rolling temperature is 995℃, the wire drawing temperature is 785℃, and the hot rolled coil is put into the insulation corridor at 702℃ for slow cooling.

[0057] Wire rod decarburization layer 0.05mm, see Figure 5 .

[0058] Comparative Example 1:

[0059] A method for controlling the depth of decarburized layer of cold heading steel wire rod for high strength fasteners, with rolling specification of Φ16mm. The chemical composition weight percentage of cold heading steel wire rod is: C=0.35%, Si=0.20%, Mn=0.68%, P=0.013%, S=0.003%, Al=0.028%, Cr=0.92%, Mo=0.16%, and the rest is Fe and unavoidable impurities. The process steps include:

[0060] (1) Removal of moisture: The billet enters the furnace through a roller drying box; the high coke mixed gas is dehydrated by a gas dehydrator before entering the heating furnace; the H2O (g) content in the furnace is 12.5 g·m -3 ;

[0061] (2) Heating: Soaking section 1070°C, residual oxygen content in the heating furnace ≤ 1.5%, furnace time 98 min;

[0062] (3) Controlled rolling and controlled cooling: the starting rolling temperature is 1002℃, the wire drawing temperature is 781℃, and the hot rolled coil is put into the insulation corridor at 695℃ for slow cooling.

[0063] Wire rod decarburization layer 0.132mm, see Figure 2 .

[0064] Comparative Example 2:

[0065] A method for controlling the depth of decarburized layer of cold heading steel wire rod for high strength fasteners, with rolling specification of Φ12mm. The chemical composition weight percentage of cold heading steel wire rod is: C=0.34%, Si=0.21%, Mn=0.70%, P=0.014%, S=0.003%, Al=0.030%, Cr=0.90%, Mo=0.16%, and the rest is Fe and unavoidable impurities. The process steps include:

[0066] (1) Removal of moisture: The billet enters the furnace through a roller drying box; the high coke mixed gas is dehydrated by a gas dehydrator before entering the heating furnace; the H2O (g) content in the furnace is 3.5 g·m -3 ;

[0067] (2) Heating: Soaking section 1065°C, residual oxygen content in the heating furnace ≤ 6.5%, furnace time 105 min;

[0068] (3) Controlled rolling and controlled cooling: the starting rolling temperature is 995°C, the wire drawing temperature is 785°C, and the hot rolled coil is put into the insulation corridor at 702°C for slow cooling.

[0069] Wire rod decarburization layer 0.091mm, see Figure 4 .

[0070] Comparative Example 3:

[0071] A method for controlling the depth of decarburized layer of cold heading steel wire rod for high strength fasteners, with rolling specification of Φ10mm. The chemical composition weight percentage of cold heading steel wire rod is: C=0.36%, Si=0.23%, Mn=0.69%, P=0.013%, S=0.004%, Al=0.032%, Cr=0.89%, Mo=0.17%, and the rest is Fe and unavoidable impurities. The process steps include:

[0072] (1) Removal of moisture: The billet enters the furnace through a roller drying box; the high coke mixed gas is dehydrated by a gas dehydrator before entering the heating furnace; the H2O (g) content in the furnace is 4.2 g·m -3 ;

[0073] (2) Heating: Soaking section 1180°C, residual oxygen content in the heating furnace ≤ 1.66%, furnace time 104 min;

[0074] (3) Controlled rolling and controlled cooling: the starting rolling temperature is 1095℃, the wire drawing temperature is 785℃, and the hot rolled coil is put into the insulation corridor at 702℃ for slow cooling.

[0075] Wire rod decarburization layer 0.09mm, see Figure 6 .

[0076] The above description is only a preferred embodiment of the present invention and is not intended to limit the protection scope of the present invention. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention are included in the protection scope of the present invention.

Claims

1. A production method for controlling the depth of decarburization layer of cold heading steel wire rod for high-strength fasteners, characterized in that: The invention comprises the following main process steps: removing moisture from the billet, heating, controlled rolling and controlled cooling. The chemical composition by weight percentage of the cold heading steel wire rod is: C: 0.32-0.38%, Si: 0.15-0.30%, Mn: 0.60-0.90%, P≤0.020%, S≤0.010%, Al≥0.020%, Cr: 0.80-1.10%, Mo: 0.15-0.30%, and the rest is Fe and unavoidable impurities.

2. A production method for controlling the decarburization depth of cold heading steel wire rod for high-strength fasteners according to claim 1, characterized in that: The content of C is 0.34-0.36%, such as 0.34%, 0.35%, 0.36%; and / or the content of Si is 0.20-0.23%, such as 0.20%, 0.21%, 0.23%; and / or the content of Mn is 0.68-0.70%, for example 0.68%, 0.69%, 0.70%; and / or P content ≤ 0.014%, such as 0.013% or 0.014%; and / or the content of S is ≤ 0.004%, for example 0.003% or 0.004%; and / or Al content ≥ 0.028%, such as 0.028%, 0.030%, 0.032%; and / or Cr content is 0.80-1.10%, for example 0.89%, 0.90%, 0.92%; And / or the content of Mo is 0.16-0.17%, for example 0.16% or 0.17%.

3. A production method for controlling the decarburization depth of cold heading steel wire rod for high-strength fasteners according to claim 1 or 2, characterized in that: The dehumidification of the billet means that the billet enters the furnace through a roller drying box; the high-coke mixed gas is dehydrated through a gas dehydrator before entering the heating furnace, thereby reducing the water vapor content in the furnace and controlling the decarburization of the billet generated during the heating process.

4. A production method for controlling the decarburization depth of cold heading steel wire rod for high-strength fasteners according to claim 1 or 2, characterized in that: The heating: the soaking section is 1050-1100°C, the furnace time is 80-120 minutes, and the residual oxygen content and heating temperature are reduced to control the decarburization of the blank produced during the heating process.

5. A production method for controlling the decarburization depth of cold heading steel wire rod for high-strength fasteners according to claim 1 or 2, characterized in that: The controlled rolling and controlled cooling are as follows: the starting rolling temperature is 960-1020°C, the spinning temperature is 760-820°C, the hot coiling temperature is 670-720°C, and the hot coiling is then put into a heat preservation corridor for slow cooling.

6. A production method for controlling the decarburization depth of cold heading steel wire rod for high strength fasteners according to claim 3, characterized in that: H2O(g) content in the furnace ≤6g·m -3 .

7. A production method for controlling the depth of decarburization layer of cold heading steel wire rod for high strength fasteners according to claim 4, characterized in that: The residual oxygen content in the heating furnace is ≤2.5%.

8. A production method for controlling the depth of decarburized layer of cold heading steel wire rod for high strength fasteners as claimed in any one of claims 1 to 7, characterized in that: A wire rod without complete decarburization and with a total decarburization layer depth of less than 0.6%D is obtained.

Citation Information

Patent Citations

  • Production technology of high-alloy tool steel wire rod

    CN105149878A

  • GCr15 bearing steel with small decarburized layer depth and preparation method

    CN111394555A

  • Method for controlling depth of decarburized layer of hot-rolled and cold-forged steel coil

    CN114985468A

  • Production method for reducing depth of decarburized layer of wire coil

    CN116590505A

  • Method for preventing decarbonization of steel

    JP1989240614A

Cited By

  • Production method for reducing decarburized layer of low-carbon alloy carburizing steel cold drawing rod

    CN120366550A