Carbon steel and preparation method and application thereof
By adding trace amounts of lanthanum and cerium to carbon steel, the lanthanum cerium rare earth alloy is formed, which improves the lateral impact function and performance of carbon steel, solves the problem of insufficient impact performance of existing carbon steel, and realizes low-cost and high-performance carbon steel preparation.
Patent Information
- Application Number
- CN202411020986.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-12
AI Technical Summary
The impact performance of existing carbon steel is insufficient. Adding rare earth elements to improve performance will increase production costs and affect the castability of the steel, making it difficult to meet industrial production needs.
Add trace amounts of lanthanum and cerium to carbon steel to form lanthanum cerium rare earth alloy. Through converter steelmaking, LF refining and continuous casting processes, lanthanum cerium rare earth alloy is added to improve the impact performance of the steel liquid, and a lateral impact work is prepared from 100J~125J~ carbon steel reduces production costs.
It significantly improves the lateral impact work of carbon steel, reduces production costs, ensures the castability and material performance of the molten steel, and is suitable for mass production and further processing needs.
Smart Images

Figure CN118932244A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of metal casting, and in particular to a carbon steel and a preparation method and application thereof. Background Art
[0002] Ordinary carbon steel is widely used and has a relatively simple production process. It is a basic product of steel enterprises. However, the current common production process is difficult to meet the impact energy of ordinary carbon steel. At present, the impact performance of ordinary carbon steel is improved by increasing the content of effective alloy elements, but this will inevitably increase production costs and is not conducive to the industrial development of ordinary carbon steel.
[0003] It is known that for high-end steel varieties, the way to improve the performance of ordinary carbon steel in industry is to add rare earth elements to the steel to improve the corrosion resistance, wear resistance, plasticity and toughness of the steel. For example, after adding 0.0009% rare earth to NM450 wear-resistant steel, the wear resistance and corrosion resistance of the steel are significantly improved. Another example is that 0.0023% rare earth is added to low-alloy high-strength steel (HSLA) through the RH process, and the calcium aluminum oxide inclusions in the steel are transformed into aluminum oxide and sulfur oxide inclusions containing rare earths, which improves the cleanliness of the molten steel. For another example, when smelting electrical steel, rare earths are added to the raw materials and then subsequent smelting steps are carried out. The added rare earth forms rare earth oxysulfides, which makes the non-oriented electrical steel have excellent magnetic properties and high strength.
[0004] However, rare earth elements are expensive. Adding a large amount of rare earth elements to ordinary steel during smelting will inevitably increase the production cost of ordinary carbon steel. Moreover, adding a large amount of rare earth elements to the steel will deteriorate the castability of the molten steel, which is not conducive to continuous casting mass production. Summary of the invention
[0005] To solve the above problems, the present application proposes a carbon steel and its preparation method and application. The carbon steel contains rare earth elements at a concentration of parts per million and has a transverse impact energy of 100J to 125J, which is significantly higher than that of conventional steel.
[0006] This application is implemented through the following technical solutions:
[0007] In a first aspect, the present application provides a carbon steel, the components of which include iron, carbon, silicon, manganese, phosphorus, sulfur, aluminum, and also include lanthanum and cerium;
[0008] The content of the lanthanum is 5ppm to 15ppm, and the content of the cerium is 10ppm to 30ppm.
[0009] The carbon steel proposed in the first aspect of the present application contains rare earth metals lanthanum and cerium at a concentration level of parts per million. The transverse impact energy of the carbon steel containing trace amounts of lanthanum and cerium is 100J to 125J. The addition of trace amounts of lanthanum and cerium reduces the production cost for ordinary steel and allows continuous casting and mass production.
[0010] In some possible implementations, the lanthanum content is 8 ppm to 15 ppm.
[0011] In some possible implementations, the cerium content is 16 ppm to 30 ppm.
[0012] In some possible implementations, the mass ratio of lanthanum to cerium is 1:(1-4).
[0013] In some possible implementations, the mass ratio of lanthanum to cerium is 1:2.
[0014] In some possible implementations, the contents of carbon, silicon, manganese, phosphorus, sulfur, and aluminum are respectively: 0.15% to 0.20% carbon, 0.08% to 0.20% silicon, 0.15% to 0.25% manganese, phosphorus ≤ 0.018%, sulfur ≤ 0.015%, and 0.015% to 0.06% aluminum.
[0015] In a second aspect, the present application proposes a method for preparing the carbon steel proposed in the present application, the preparation method comprising the steps of converter steelmaking, LF refining, continuous casting and rolling; wherein, lanthanum-cerium rare earth alloy is added after the desulfurization step in the LF refining;
[0016] The addition amount of the lanthanum-cerium rare earth alloy is 0.08kg / t to 0.1kg / t.
[0017] The second aspect of the present application proposes a method for preparing carbon steel, in which rare earth alloys are added after the desulfurization step, and the addition of trace amounts of lanthanum and cerium denatures the aluminate inclusions, turning them into solid inclusions with high melting points and not easily deformed. Such rare earth-containing composite inclusions are not easily deformed into strips and strings during the rolling process, and have little effect on the transverse impact energy of the material. At the same time, due to the extremely strong activity of lanthanum and cerium rare earths, they will react with O and S elements in the molten steel first to generate rare earth sulfides and oxides, thereby inhibiting the generation of MnS inclusions in the material. MnS inclusions have good plasticity and are easy to become long lines after rolling, which has a great impact on the transverse performance of the material. Rare earth treatment deforms the strip-like inclusions and inhibits the MnS inclusions, thereby significantly improving the transverse impact energy of carbon steel; in addition, the continuous casting process of molten steel is smooth, without the rise of stopper rods, etc., and the hot-rolled coils obtained by hot rolling do not contain slender MnS inclusions, so that the transverse impact energy of the prepared carbon steel is 100J~125J, which meets the further processing requirements of higher ordinary carbon steel. In addition, the preparation method does not need to perform calcium treatment operation, which not only has a simple process and easy operation, but also reduces the overall production cost of carbon steel.
[0018] In some possible implementations, in the rolling step, the rolling conditions include: the slab furnace temperature is 1230°C to 1260°C, the initial rolling passes are 5 to 7 times, the finishing rolling entrance temperature is 1100°C to 1150°C, and the final rolling temperature is 880°C to 910°C.
[0019] In some possible implementations, in the rolling step, the coiling temperature is 550°C to 580°C.
[0020] In some possible implementations, in the rolling step, the total reduction ratio is 97.8% to 99.1%.
[0021] In some possible implementations, the molten steel is soft-blown after the lanthanum-cerium rare earth alloy is added, and the soft-blowing time is 8 minutes to 12 minutes.
[0022] On the third aspect, the present application proposes an application of the carbon steel provided by the present application in the fields of bridges, buildings, wire products or automobile bodies. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] In order to more clearly illustrate the embodiments of the present drawings or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present drawings. For ordinary technicians in this field, other drawings can be obtained based on the structures shown in these drawings without paying any creative work.
[0024] Figure 1 Schematic diagram of the comparison of transverse and longitudinal impact energy of silicon carbon steel prepared in Example 1 of the present application and Comparative Example 1 at temperatures of 0°C, room temperature, and -20°C;
[0025] Figure 2a This is a schematic diagram of rare earth inclusions in a hot-rolled coil in the carbon steel preparation method of Example 1 of the present application;
[0026] Figure 2b This is an energy spectrum diagram of rare earth inclusions in a hot-rolled coil in the carbon steel preparation method of Example 1 of the present application;
[0027] Figure 3a This is a schematic diagram of MnS inclusions in a hot-rolled coil in the carbon steel preparation method of Comparative Example 1 of the present application;
[0028] Figure 3b This is an energy spectrum diagram of MnS inclusions in the hot-rolled coil in the carbon steel preparation method of Comparative Example 1 of the present application.
[0029] The purpose, features and advantages of this figure will be further described in conjunction with the embodiments with reference to the accompanying drawings. DETAILED DESCRIPTION
[0030] In order to make the purpose, technical solutions and advantages of the present application clearer, the present application is described and illustrated below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not intended to limit the present application. Based on the embodiments provided in the present application, all other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of the present application.
[0031] Obviously, the following descriptions are only some examples or embodiments of the present application. For ordinary technicians in this field, the present application can also be applied to other similar scenarios without creative work. In addition, it can also be understood that although the efforts made in this development process may be complicated and lengthy, for ordinary technicians in the field related to the content disclosed in this application, some changes in design, manufacturing or production based on the technical content disclosed in this application are just conventional technical means, and should not be understood as insufficient content disclosed in this application.
[0032] However, unnecessary detailed descriptions may be omitted. For example, detailed descriptions of well-known matters and repeated descriptions of substantially the same structures may be omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate understanding by those skilled in the art. In addition, the following description is provided for those skilled in the art to fully understand the present application and is not intended to limit the subject matter described in the claims.
[0033] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.
[0034] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.
[0035] The "range" disclosed in the present application is defined in the form of a lower limit and an upper limit, and a given range is defined by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundaries of the particular range. The range defined in this way can be inclusive or exclusive of the end values, and can be arbitrarily combined, that is, any lower limit can be combined with any upper limit to form a range. For example, if a range of 60 to 120 and 80 to 110 is listed for a particular parameter, it is understood that a range of 60 to 110 and 80 to 120 is also expected. In addition, if the minimum range values 1 and 2 are listed, and if the maximum range values 3, 4 and 5 are listed, the following ranges can all be expected: 1 to 3, 1 to 4, 1 to 5, 2 to 3, 2 to 4 and 2 to 5. In the present application, unless otherwise specified, the numerical range "ab" represents an abbreviation of any real number combination between a and b, where a and b are both real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" are listed in this document, and "0-5" is just an abbreviation of these numerical combinations. In addition, when a parameter is expressed as an integer ≥ 2, it is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0036] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.
[0037] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.
[0038] If there is no special explanation, all steps of the present application can be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), which means that step (c) may be added to the method in any order. For example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.
[0039] If there is no special explanation, the "include" and "comprising" mentioned in this application are open-ended or closed-ended. For example, the "include" and "comprising" may mean that other components not listed may also be included or only the listed components may be included or only the listed components may be included.
[0040] If not specifically stated, in this application, the term "or" is inclusive. For example, the phrase "A or B" means "A, B, or both A and B". More specifically, any of the following conditions satisfies the condition "A or B": A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).
[0041] Explanation of terms: The contents in the examples of this application all represent mass fractions.
[0042] In a first aspect of an embodiment of the present application, a carbon steel is provided, the components of which include iron, carbon, silicon, manganese, phosphorus, sulfur, aluminum, and also include lanthanum and cerium;
[0043] The content of lanthanum is 5ppm to 15ppm, and the content of cerium is 10ppm to 30ppm.
[0044] The carbon steel proposed in the embodiment of the present application, which contains rare earth metals lanthanum and cerium at a concentration level of parts per million, has a transverse impact energy of 100J to 125J; and the addition of trace amounts of lanthanum and cerium reduces the production cost for ordinary steel, and can be produced in batches by continuous casting.
[0045] In the embodiment, the content of lanthanum can be 5ppm, 8ppm, 10ppm, 15ppm and other typical but non-limiting contents or the range between any two contents; the content of cerium can be 10ppm, 16ppm, 25ppm, 30ppm and other typical but non-limiting contents or the range between any two contents. The addition of these trace amounts of lanthanum and cerium denatures the aluminate inclusions and turns them into solid inclusions with high melting points and not easy to deform. Such rare earth-containing composite inclusions are not easy to deform into strips and strings during the rolling process, and have little effect on the transverse impact energy of the material.
[0046] In some specific embodiments, the content of lanthanum is 8ppm to 15ppm. In some specific embodiments, the content of cerium is 16ppm to 30ppm. In this case, the transverse impact energy of carbon steel is 120J to 125J.
[0047] In some specific embodiments, the content of lanthanum is 8 ppm and the content of cerium is 16 ppm. Under this content, the transverse impact energy of carbon steel is 120 J, which is 20% higher than the transverse impact energy of conventional steel.
[0048] In some embodiments, the mass ratio of lanthanum to cerium is 1:(1-4), and in exemplary embodiments, it can be a typical but non-limiting mass ratio of 1:1, 1:2, 1:3, 1:4, or a range between any two mass ratios. Within this mass ratio range, the lanthanum-cerium rare earth alloy has a high cost performance, and the cost of rare earth treatment is low. At the same time, the rare earth elements in the molten steel will fully react with elements such as oxygen, aluminum, and sulfur to obtain a composite inclusion containing lanthanum-cerium rare earth elements.
[0049] In some specific embodiments, the mass ratio of lanthanum to cerium is 1: 2. Within this mass ratio range, the lanthanum-cerium rare earth alloy has the highest cost performance and the lowest cost of rare earth treatment. At the same time, during preparation, the rare earth elements in the molten steel will fully react with elements such as oxygen, aluminum, and sulfur to obtain composite inclusions containing lanthanum-cerium rare earth elements.
[0050] In some embodiments, the contents of carbon, silicon, manganese, phosphorus, sulfur, and aluminum are respectively: 0.15% to 0.20% carbon, 0.08% to 0.20% silicon, 0.15% to 0.25% manganese, phosphorus ≤ 0.018%, sulfur ≤ 0.015%, and 0.015% to 0.06% aluminum.
[0051] In some specific embodiments, the carbon steel is composed of the following components: 0.15% to 0.20% carbon, 0.08% to 0.20% silicon, 0.15% to 0.25% manganese, phosphorus ≤ 0.018%, sulfur ≤ 0.015%, 0.015% to 0.06% aluminum, 5ppm to 15ppm lanthanum, 10ppm to 30ppm cerium, and the balance is iron and other inevitable impurities. In this case, the transverse impact energy of the carbon steel is 100J to 125J.
[0052] In some specific embodiments, the contents of carbon, silicon, manganese, phosphorus, sulfur, aluminum, lanthanum and cerium are respectively: 0.18% carbon, 0.12% silicon, 0.20% manganese, 0.012% phosphorus, 0.008% sulfur, 0.030% aluminum, 10ppm lanthanum and 20ppm cerium. At this content, the transverse impact energy of carbon steel is 115J.
[0053] In some specific embodiments, the contents of carbon, silicon, manganese, phosphorus, sulfur, aluminum, rhenium, lanthanum and cerium are respectively: 0.18% carbon, 0.15% silicon, 0.18% manganese, 0.010% phosphorus, 0.006% sulfur, 0.040% aluminum, 15ppm lanthanum and 30ppm cerium. At this content, the transverse impact energy of carbon steel is 121J.
[0054] In some embodiments, the yield strength of carbon steel is 400MPa-450MPa, the tensile strength is 540MPa-560MPa, and the elongation is 29%-35%. In the example, the yield strength of carbon steel can be 400MPa, 427.1MPa, 427.4MPa, 428.9MPa, 431.2MPa, 450MPa, etc., typical but non-limiting yield strengths or a range between any two yield strengths; the tensile strength can be 540MPa, 543.8MPa, 544.9MPa, 545.1MPa, 545.3MPa, 560MPa, etc., typical but non-limiting tensile strengths or a range between any two tensile strengths; the elongation can be 29%, 29.3%, 29.6%, 30.0%, 30.2%, 35%, etc., typical but non-limiting elongations or a range between any two elongations.
[0055] The second aspect of the embodiment of the present application provides a method for preparing the carbon steel provided in the present application, the preparation method comprising the steps of: converter steelmaking, LF refining, continuous casting and rolling; wherein, lanthanum-cerium rare earth alloy is added after the desulfurization step in LF refining;
[0056] The addition amount of lanthanum-cerium rare earth alloy is 0.04kg / t to 0.20kg / t.
[0057] The method for preparing carbon steel proposed in the embodiment of the present application adds a rare earth alloy after the desulfurization step. The addition of trace amounts of lanthanum and cerium denatures the aluminate inclusions and turns them into solid inclusions with high melting points and are not easily deformed. Such rare earth-containing composite inclusions are not easily deformed into strips and strings during the rolling process, and have little effect on the transverse impact energy of the material. At the same time, due to the extremely strong activity of lanthanum and cerium rare earths, they will react with O and S elements in the molten steel first to generate rare earth sulfides and oxides, which inhibits the generation of MnS inclusions in the material. MnS inclusions have good plasticity and are easy to become long lines after rolling, which has a great impact on the transverse performance of the material. Rare earth treatment deforms the strip-like inclusions and suppresses the MnS inclusions, thereby significantly improving the transverse impact energy of carbon steel; in addition, the continuous casting process of molten steel is smooth, without the rise of stopper rods, etc., and the hot-rolled coils obtained by hot rolling do not contain slender MnS inclusions, so that the transverse impact energy of the prepared carbon steel is 100J~125J, which meets the further processing requirements of higher ordinary carbon steel. In addition, the preparation method does not require calcium treatment operation, which not only has a simple process and easy operation, but also reduces the overall production cost of carbon steel.
[0058] In the embodiment, the addition amount of the lanthanum-cerium rare earth alloy can be 0.04 kg / t, 0.09 kg / t, 0.15 kg / t, 0.20 kg / t or other typical but non-limiting addition amounts or a range between any two addition amounts.
[0059] In some embodiments, the LF refining process adopts white slag or yellow-white slag operation, and the T.Fe in the slag is ≤1%, which can ensure that the molten steel will not be affected by the oxygen in the slag, and no additional Al2O3 inclusions will be generated during the molten steel transfer and continuous casting process; in the middle and late stages of LF refining (after desulfurization), after adding rare earth alloys, the molten steel is soft-blown (8min-12min) and then continuously casted on the platform. The soft-blowing operation (8min-12min) can ensure that large-sized inclusions in the steel are fully floated, ensuring the cleanliness of the molten steel.
[0060] In some embodiments, the amount of lanthanum-cerium rare earth alloy added is 0.098 kg / t. In this case, the transverse impact energy of the prepared carbon steel is 120 J.
[0061] In some embodiments, the purity of the lanthanum-cerium rare earth alloy is above 99.5%. In this case, on the one hand, the rare earth alloy brings very few impurities into the molten steel, which will not deteriorate the cleanliness of the molten steel; on the other hand, the content of rare earth alloy elements that can participate in the reaction is higher, and only a small amount of rare earth alloy needs to be added to achieve the expected effect of rare earth micro-treatment.
[0062] In some embodiments, after adding the lanthanum-cerium rare earth alloy, the molten steel is soft-blown, and the soft-blowing time is 8 minutes to 12 minutes. In the exemplary example, it can be a typical but non-restrictive time such as 8 minutes, 10 minutes, 12 minutes, or a range between any two times. In this case, soft blowing can reduce the content of dissolved gas (such as hydrogen, nitrogen, and oxygen) in the molten steel, and remove the remaining non-metallic inclusions (such as oxides, sulfides, nitrides, etc.) in the molten steel. At this time, the composite inclusions containing rare earth elements are mainly solid inclusions with relatively large density. Only by ensuring a certain time of soft blowing can the inclusions be well removed. In addition, soft blowing can also make the composition and temperature of the molten steel more uniform before pouring, reduce the pouring start temperature, realize low superheat continuous casting, improve the low-multiple quality of the continuous casting billet, and thus improve the impact toughness and other properties of the steel.
[0063] In some embodiments, continuous casting comprises the following steps:
[0064] S1. The molten steel after LF refining flows continuously from the ladle into the tundish and then into the crystallizer to solidify to obtain a casting with a liquid core.
[0065] S2. The ingot with liquid core is cut into required size after secondary cooling in the sector segment to obtain a continuous casting ingot.
[0066] In some specific embodiments, after the continuous casting billet is cooled for the second time, the surface temperature of the slab out of the continuous casting machine is 700°C to 900°C. In the exemplary embodiment, it can be a typical but non-limiting temperature such as 700°C, 800°C, 900°C, or a range between any two temperatures. The billet cooled by this system has relatively less internal looseness and segregation, and the low-multiple quality of the slab is better, which is conducive to improving the impact performance of the subsequent hot rolled coil.
[0067] In some specific embodiments, the thickness of the continuous casting slab is 200 mm to 300 mm. In the exemplary embodiment, the thickness can be 200 mm, 250 mm, 300 mm, etc., which are typical but non-limiting thicknesses, or a range between any two thicknesses. Within this thickness range, the reduction ratio of the continuous casting slab when rolling it into a hot rolled coil can be fully guaranteed, and the total reduction ratio can be guaranteed to be above 95%.
[0068] In some specific embodiments, in the rolling step, the rolling conditions include: the slab furnace temperature is 1230°C to 1260°C, and in the exemplary example, it can be a typical but non-limiting temperature such as 1230°C, 1240°C, 1250°C, 1260°C, or a range between any two temperatures; the initial rolling pass is 5 to 7 times, and in the exemplary example, it can be a typical but non-limiting pass such as 5, 6, 7 times, or a range between any two passes; the finishing rolling inlet temperature is 1100°C to 1150°C, and in the exemplary example, it can be a typical but non-limiting temperature such as 1100°C, 1110°C, 1130°C, 1150°C, or a range between any two temperatures; the final rolling temperature is 880°C to 910°C, and in the exemplary example, it can be a typical but non-limiting temperature such as 880°C, 900°C, 910°C, or a range between any two temperatures. In some specific embodiments, in the rolling step, the coiling temperature is 550°C to 580°C, and in the exemplary embodiment, it can be a typical but non-limiting temperature such as 550°C, 560°C, 570°C, 580°C, or a range between any two temperatures. In some specific embodiments, in the rolling step, the total reduction rate is 97.8% to 99.1%, and in the exemplary embodiment, it can be a typical but non-limiting total reduction rate such as 97.8%, 98.6%, 99%, 99.1%, or a range between any two total reduction rates. In this case, the carbon steel structure obtained after hot rolling is more uniform, with less banded structure, which further improves the comprehensive performance of the hot rolled coil.
[0069] The following is further described in conjunction with specific embodiments.
[0070] Example 1
[0071] Example 1 proposes a carbon steel, the components of which include iron, carbon, silicon, manganese, phosphorus, sulfur, aluminum and inevitable impurity elements, and also include lanthanum and cerium; wherein the contents of carbon, silicon, manganese, phosphorus, sulfur, aluminum, lanthanum and cerium are respectively: 0.18% carbon, 0.12% silicon, 0.20% manganese, 0.012% phosphorus, 0.008% sulfur, 0.030% aluminum, 8ppm lanthanum and 16ppm cerium.
[0072] Example 1 also provides a method for preparing carbon steel, comprising the following steps:
[0073] (1) Converter steelmaking: A 210t converter is used to smelt molten steel, with a steel output of 205 tons.
[0074] (2) LF refining:
[0075] ① Gradually add aluminum blocks, silicon manganese, ferrosilicon and other alloys into the molten steel to deoxidize and alloy the molten steel, add lime and pre-melted slag for slagging and desulfurization operations, and the final T.Fe content in the slag is ≤1%.
[0076] ② Add 20kg of LaCe rare earth alloy with a purity of 99.5% (La:Ce is about 1:2), and then soft blow the molten steel for 10 minutes before leaving the station.
[0077] (3) A vertical bending slab continuous casting machine with a thickness of 230 mm was used, and the continuous casting speed was stabilized at 1.2 m / min. The continuous casting slab was subjected to secondary cooling, and the surface temperature of the slab out of the continuous casting machine was 780°C. After cooling, the slab was cut to obtain the continuous casting slab of the required length.
[0078] (4) The continuous casting slab is hot rolled to obtain a steel coil, the hot rolled slab has a furnace temperature of 1245°C, the initial rolling is 7 passes, the hot rolling finishing inlet temperature is 1135°C; the hot rolling final rolling temperature is 902°C; the hot rolling coiling temperature is 565°C, and a hot rolled coil with a thickness of 3.2 mm is obtained, and the total reduction ratio is 98.6%.
[0079] Example 2
[0080] Example 2 proposes a carbon steel, the component contents of which are substantially the same as those of Example 1, except that the contents of lanthanum and cerium are 10 ppm lanthanum and 20 ppm cerium.
[0081] Example 2 also proposes a method for preparing carbon steel, and the steps are basically the same as those of Example 1, except that: the mass of LaCe rare earth alloy added in step ② is 25 kg (0.12 kg / t).
[0082] Example 3
[0083] Example 3 proposes a carbon steel, the component contents of which are substantially the same as those of Example 1, except that the contents of lanthanum and cerium are 5 ppm lanthanum and 10 ppm cerium.
[0084] Example 3 also proposes a method for preparing carbon steel, and the steps are basically the same as those of Example 1, except that: the mass of LaCe rare earth alloy added in step ② is 10 kg (0.049 kg / t).
[0085] Example 4
[0086] Example 4 proposes a carbon steel, the component contents of which are substantially the same as those of Example 1, except that the contents of lanthanum and cerium are 15 ppm lanthanum and 30 ppm cerium.
[0087] Example 4 also proposes a method for preparing silicon carbon steel, and the steps are basically the same as those of Example 1, except that: the mass of LaCe rare earth alloy added in step ② is 40 kg (0.20 kg / t).
[0088] Comparative Example 1
[0089] Comparative Example 1 proposes a carbon steel and a method for preparing carbon steel, and the steps are basically the same as those in Example 1, except that: Step ② adopts conventional calcium treatment operation, that is, using a wire feeder to feed 400m of pure calcium wire into the molten steel, and then the molten steel is soft-blown for 10 minutes.
[0090] Comparative Example 2
[0091] Comparative Example 2 proposes a carbon steel and a method for preparing carbon steel, and the steps are basically the same as those of Example 1, except that: the mass of the LaCe rare earth alloy added in step ② is 60 kg (0.29 kg / t).
[0092] Comparative Example 3
[0093] Comparative Example 3 proposes a carbon steel and a method for preparing carbon steel, and the steps are basically the same as those of Example 1, except that: the mass of the LaCe rare earth alloy added in step ② is 5 kg (0.024 kg / t).
[0094] Comparative Example 4
[0095] Comparative Example 4 proposes a carbon steel and a method for preparing the carbon steel. The components and preparation steps are basically the same as those of Example 1, except that the mass ratio of lanthanum to cerium in the carbon steel is 2:1.
[0096] Comparative Example 5
[0097] Comparative Example 5 proposes a carbon steel and a method for preparing carbon steel. The components and preparation steps are basically the same as those of Example 1, except that step ② is not included, and a wire feeder is used to feed 20 kg of LaCe rare earth alloy wire with a purity of 99.5% in the continuous casting step (La:Ce is about 1:2).
[0098] In order to verify the progressiveness of the carbon steel and its preparation method in the embodiments of the present application, the carbon steels of Examples 1 to 4 and Comparative Examples 1 to 5 or the prepared carbon steels were subjected to transverse and longitudinal impact energy detection experiments, yield strength tests, tensile strength tests and elongation tests at temperatures of 0°C, room temperature and -20°C; wherein, the standard for impact energy detection is GB / T 229-2020 Charpy pendulum impact test method for metal materials, and the standard for yield strength, tensile strength and elongation tests is GB / T 228. The impact energy results are shown in Table 1 below, and the yield strength, tensile strength and elongation are shown in Table 2 below. In addition, taking Example 1 and Comparative Example 1 as examples, the data comparison of impact energy is shown in the attached manual. Figure 1 As shown in the figure, the inclusions in the hot rolled plate are as follows Figure 2a , Figure 2b , Figure 3a and Figure 3b The cost calculation is shown in Table 2 below.
[0099] Table 1
[0100]
[0101] Table 2
[0102]
[0103] According to Tables 1 and 2 above and the instructions Figure 1 , Figure 2a , Figure 2b , Figure 3a and Figure 3b It can be seen that:
[0104] 1) According to the data of Example 1 and Comparative Example 1 in Table 1 (Table 1, Appendix Figure 1 , Figure 2a , Figure 2b , Figure 3a and Figure 3b ) It can be seen that the carbon steel with trace lanthanum and cerium rare earth metal alloys contained in the embodiments of the present application has a higher transverse impact energy than the existing conventional calcium treatment process at both low temperature and room temperature. This is because the addition of trace lanthanum and cerium denatures the aluminate inclusions and turns them into solid inclusions with a high melting point and are not easily deformed. Such rare earth-containing composite inclusions form granular inclusions during the rolling process, that is, they are not easily deformed into strips and strings, and have little effect on the transverse impact energy of the material. At the same time, due to the extremely strong activity of lanthanum, cerium and rare earths, they will react with O and S elements in the molten steel first to generate rare earth sulfides and oxides, thereby inhibiting the formation of MnS inclusions in the material. MnS inclusions have good plasticity and are easy to become long lines after rolling, which has a great impact on the transverse performance of the material. Rare earth treatment deforms the strip-like inclusions and inhibits the MnS inclusions, thereby significantly improving the transverse impact energy of carbon steel.
[0105] 2) From the data of Examples 1 to 4 and Comparative Examples 2 and 3 in Table 1 and Table 2, it can be seen that the addition of lanthanum and cerium in the examples of the present application can significantly increase the transverse impact energy of carbon steel; when less is added, the transverse impact energy is not much different from that of carbon steel obtained by conventional calcium treatment process, and even decreases in Comparative Example 3. When more is added, the refining cost increases, the castability of the molten steel deteriorates, and the rise of the furnace plug increases.
[0106] 3) From the data of Example 1 and Comparative Example 4 in Table 1, it can be seen that the transverse impact energy when the mass ratio of lanthanum to cerium in the carbon steel of the embodiment of the present application is 1:2 is slightly better than that of lanthanum to cerium in the mass ratio of 2:1, and the cost is significantly lower.
[0107] 4) From the data of Example 1 and Comparative Example 5 in Tables 1 and 2, it can be seen that the preparation method of carbon steel in the embodiment of the present application, by adding lanthanum-cerium rare earth alloy in the LF refining step, not only omits the wire feeding step and reduces the production cost, but also the transverse impact energy, yield strength, tensile strength and elongation of the prepared carbon steel are significantly higher.
[0108] 5) As shown in Table 2, compared with the conventional ordinary steel of Comparative Example 1, the yield strength, tensile strength and elongation of the carbon steel containing lanthanum and cerium rare earth metals in the examples of the present application are not significantly reduced.
[0109] 6) It can be seen from the comparison between Examples 1 to 4 and Comparative Examples 2 and 3 that the trace addition of lanthanum-cerium rare earth alloy in the preparation method of the present application does not affect the yield strength, tensile strength and elongation of carbon steel, and does not affect the stability of the continuous casting process. However, when less or more lanthanum-cerium rare earth alloy is added, the castability of molten steel deteriorates, and the refining cost of more rare earth alloys will also increase.
[0110] It should be noted that the present application is not limited to the above-mentioned embodiments. The above-mentioned embodiments are only examples, and the embodiments having the same structure as the technical idea and exerting the same effect within the scope of the technical solution of the present application are all included in the technical scope of the present application. In addition, without departing from the scope of the main purpose of the present application, various modifications that can be thought of by those skilled in the art to the embodiments and other methods of combining some of the constituent elements in the embodiments are also included in the scope of the present application.
Claims
1. A carbon steel comprising carbon, silicon, manganese, phosphorus, sulfur and aluminum, characterized in that: Also included are lanthanum and cerium; The content of the lanthanum is 5ppm to 15ppm, and the content of the cerium is 10ppm to 30ppm.
2. The carbon steel according to claim 1, characterized in that The lanthanum content is 8ppm to 15ppm; And / or, the cerium content is 16ppm to 30ppm.
3. The carbon steel according to claim 1 or 2, characterized in that: The mass ratio of lanthanum to cerium is 1:(1-4).
4. The carbon steel according to claim 3, characterized in that The mass ratio of lanthanum to cerium is 1:
2.
5. The carbon steel according to claim 1, characterized in that The contents of carbon, silicon, manganese, phosphorus, sulfur and aluminum are respectively: 0.15% to 0.20% carbon, 0.08% to 0.20% silicon, 0.15% to 0.25% manganese, phosphorus ≤ 0.018%, sulfur ≤ 0.015%, and 0.015% to 0.06% aluminum.
6. A method for preparing carbon steel according to any one of claims 1 to 5, comprising the steps of converter steelmaking, LF refining, continuous casting and rolling; characterized in that: adding lanthanum-cerium rare earth alloy after the desulfurization step in the LF refining; The addition amount of the lanthanum-cerium rare earth alloy is 0.04kg / t to 0.20kg / t.
7. The method for preparing carbon steel according to claim 6, characterized in that: After adding the lanthanum-cerium rare earth alloy, the molten steel is soft-blown for 8 to 12 minutes.
8. The method for preparing carbon steel according to claim 6, characterized in that: In the rolling step, the rolling conditions include: the slab furnace temperature is 1230°C to 1260°C, the initial rolling passes are 5 to 7 times, the finishing rolling entrance temperature is 1100°C to 1150°C, and the final rolling temperature is 880°C to 910°C.
9. The method for preparing carbon steel according to claim 8, characterized in that: In the rolling step, the coiling temperature is 550°C to 580°C; And / or, in the rolling step, the total reduction ratio is 97.8% to 99.1%.
10. Use of the carbon steel according to any one of claims 1 to 6 in the fields of bridges, buildings, wire products or automobile bodies.