Non-quenched and tempered steel for integral piston rod of oil cylinder and manufacturing method of piston rod
By using non-tempered steel with specific chemical components in the piston rod of hydraulic cylinder and using induction heating, forging, and cooling, the problems of uneven bending and hardness in traditional piston rod processing are solved, and the mechanics of the piston rod are improved Performance and service life.
Patent Information
- Application Number
- CN202411003269.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-11-12
AI Technical Summary
During the processing process, the piston rod of traditional hydraulic cylinders has problems such as bending, uneven tempering and hardness and inconsistent internal and external mechanical properties, which affects its service life and efficiency.
Using non-tempered steel, V/N and (V+Al+Nb+Ti)/ is controlled through specific chemical composition and processing processes, such as induction heating, forging, cooling, local upsetting, precision plating and electroplating. The mass ratio of N is to refine ferrite and pearlite grains to improve the strength and toughness of the steel.
It significantly improves the comprehensive mechanical properties of the piston rod, reduces processing allowance, improves processing efficiency, avoids heat treatment deformation, extends service life, and improves hardness, tensile strength and impact work.
Smart Images

Figure CN118932248A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of hydraulic oil cylinders, and in particular to a non-quenched and tempered steel for an integral piston rod of an oil cylinder and a method for manufacturing the piston rod. Background Art
[0002] The jack in the hydraulic support is the key component to realize the action function of the hydraulic support, and the piston rod is the key component of the jack. The traditional split type is usually manufactured by round steel such as 27SiMn, 35CrMnSi, 30CrMo, etc. The processing technology is fixed length → tempering → flat end face → center hole punching → rough turning → semi-finishing turning → finishing turning → electroplating. During the whole processing process, due to the processing allowance of 5 to 7mm, the rough turning processing allowance is large, and the processing efficiency is low. At the same time, the piston rod with a large aspect ratio is prone to bending or uneven tempering hardness during the heat treatment process, and needs to be straightened or re-tempered. In addition, the piston rod with a large diameter is affected by the depth of the hardened layer, and there is a defect of inconsistent internal and external mechanical properties, which will affect the service life of the piston rod.
[0003] In order to improve the performance of the piston rod, the invention patent with the authorization announcement number C109487155B discloses a non-quenched and tempered steel for a high-pressure cylinder hydraulic rod and a production method thereof. The non-quenched and tempered steel for a high-pressure cylinder hydraulic rod achieves a reasonable match of strength and toughness under the principle of lowest cost through composition design, and at the same time meets the requirements of the surface induction quenching hardening layer of the high-pressure cylinder rod, has high plasticity, toughness, good surface, subcutaneous quality and surface induction quenching performance, and has a low manufacturing cost, which is suitable for the production of high-pressure cylinder hydraulic rods. At the same time, when manufacturing non-quenched and tempered steel for high-pressure cylinder hydraulic rods, through the micro-alloying composition design and the controlled rolling and controlled cooling production method, high-pressure cylinder rod steel that does not require quenching and tempering treatment is produced, which simplifies the production process, saves equipment, and has the characteristics of saving materials, energy, and reducing production costs. However, the comprehensive mechanical properties of the non-quenched and tempered steel for the high-pressure cylinder hydraulic rod are still lacking, and it cannot adapt well to the application scenarios of the hydraulic support cylinder piston rod. Summary of the invention
[0004] In order to improve the comprehensive mechanical properties of the integral piston rod of the oil cylinder, omit the steel quenching and tempering step, and improve the microstructure and distribution, the technical solution adopted by the present invention is: a non-quenched and tempered steel for the integral piston rod of the oil cylinder, composed of the following chemical components in percentage by mass:
[0005] C 0.24%~0.36%, Si 0.5%~0.85%, Mn 1.2%~1.6%, V 0.075%~0.15%, Ti 0.02%~0.05%, Nb 0.005%~0.01%, Al 0.014%~0.036%, N 0.025%~0.04%, S0.045%~0.06%, P<0.02%, Mo≤0.02%, Cr≤0.01%, Ni≤0.01%, the balance is Fe and unavoidable impurities;
[0006] Among them, the mass ratio of V / N is controlled at 3.0-4.0, and the mass ratio of (V+Al+Nb+Ti) / N is controlled at 4.7-5.7.
[0007] Based on the above, the chemical composition and mass percentage of the non-quenched and tempered steel used for the integral piston rod of the oil cylinder are:
[0008] C 0.28%~0.30%, Si 0.65%~0.75%, Mn 1.3%~1.4%, V 0.09%~0.13%, Ti 0.03%~0.04%, Nb 0.005%~0.01%, Al 0.020%~0.029%, N 0.03%~0.035%, S0.045%~0.06%, P<0.02%, Mo≤0.02%, Cr≤0.01%, Ni≤0.01%, the balance is Fe and unavoidable impurities;
[0009] Among them, the mass ratio of V / N is controlled at: 3.3-3.7, and the mass ratio of (V+Al+Nb+Ti) / N is controlled at: 5.0-5.4.
[0010] Based on the above, the chemical composition and mass percentage of the non-quenched and tempered steel used for the integral piston rod of the oil cylinder are:
[0011] C 0.285%, Si 0.67%, Mn 1.32%, V 0.108%, Ti 0.031%, Nb 0.0055%, Al 0.021%, N 0.032%, P 0.005%, S 0.05%, Mo 0.01%, Cr 0.005%, Ni 0.003%, and the remainder is Fe and unavoidable impurities, among which the mass ratio of V / N is 3.43, and the mass ratio of (V+Al+Nb+Ti) / N is 5.17.
[0012] Based on the above, the chemical composition and mass percentage of the non-quenched and tempered steel used for the integral piston rod of the oil cylinder are:
[0013] C 0.295%, Si 0.73%, Mn 1.38%, V 0.12%, Ti 0.0375%, Nb 0.008%, Al0.026%, N 0.035%, P 0.004%, S 0.05%, Mo 0.01%, Cr 0.005%, Ni 0.003%, and the balance is Fe and unavoidable impurities, among which the mass ratio of V / N is 3.43, and the mass ratio of (V+Al+Nb+Ti) / N is 5.47.
[0014] The present invention also provides a method for manufacturing a piston rod, comprising the following steps:
[0015] Provide a non-quenched and tempered steel for an integral piston rod of an oil cylinder;
[0016] The non-quenched and tempered steel is processed through induction heating, controlled forging, secondary controlled cooling, local upsetting, precision turning, grinding and electroplating to obtain a piston rod.
[0017] Based on the above, the steps of providing the non-quenched and tempered steel for the integral piston rod of the oil cylinder include: electric furnace steelmaking, ladle refining, ladle vacuum degassing, continuous casting, controlled rolling, and primary controlled cooling steps;
[0018] The chemical composition and mass percentage of the ingot in the continuous casting step are as follows: C 0.24%-0.36%, Si 0.5%-0.85%, Mn 1.2%-1.6%, V 0.075%-0.15%, Ti 0.02%-0.05%, Nb 0.005%-0.01%, Al 0.014%-0.036%, N 0.025%-0.04%, S 0.045%-0.06%, P < 0.02%, Mo ≤ 0.02%, Cr ≤ 0.01%, Ni ≤ 0.01%, the balance is Fe and unavoidable impurities, the mass ratio of V / N is controlled at 3.0-4.0, and the mass ratio of (V+Al+Nb+Ti) / N is controlled at 4.7-5.7;
[0019] During the controlled rolling step, the heating temperature of the ingot is 1180°C to 1250°C, the initial rolling temperature is 1100°C to 1200°C, the final rolling temperature is 970°C to 1030°C, and the temperature of the finishing process is 920°C to 970°C;
[0020] During the primary controlled cooling step, the cooling rate from the forging temperature to 850°C is 5°C / s to 20°C / s, the cooling rate from 850°C to 620°C is 1°C / s to 8°C / s, 600°C to 620°C is the critical temperature. After cooling to the critical temperature, it enters the material box for stack cooling and is cooled to room temperature at a cooling rate of less than 5°C / min. Among them, air cooling and mist cooling are carried out from the forging temperature to 850°C, and air cooling is carried out from 850°C to the critical temperature.
[0021] Based on the above, during the local upsetting process, the initial forging temperature is 1150°C to 1200°C, the final forging temperature is 950°C to 1000°C, and the upsetting force is P=kF, where k is 1078 to 1225, and F is the projection area of the non-quenched and tempered steel blank.
[0022] Based on the above, in the secondary controlled cooling process, the cooling rate from the forging temperature to 850℃ is 5℃ / s~20℃ / s, and the cooling rate from 850℃~620℃ is 1℃ / s~8℃ / s; 600℃~620℃ is the critical temperature, and after cooling to the critical temperature, it enters the material box for stack cooling and is cooled to room temperature at a cooling rate of less than 5℃ / min. Among them, the forging temperature to 850℃ is air-cooled and mist-cooled, and 850℃~critical temperature is air-cooled
[0023] Among them, in the induction heating step, when the induction heating reaches 950℃~1000℃, the current frequency is reduced to half of the original setting value to increase the effective heating depth, which is helpful for the uniform temperature inside and outside of the non-quenched and tempered round steel. When the temperature of the non-quenched and tempered steel section tends to be consistent, the original current frequency is restored and the heating is continued to 1200℃~1250℃. The machining allowance of the electroplating area of the piston rod is 0.4mm~1mm.
[0024] The present invention has outstanding substantive features and significant progress compared to the prior art. Specifically, the present invention improves the plastic toughness of steel by appropriately reducing the C content on the basis of the traditional ferrite and pearlite non-quenched and tempered steel composition, inhibits the generation of bainite and martensite by controlling the content of Mn, Cr, Mo, and Ni, refines the original austenite grain size by Ti-N-Nb-Al microalloying, improves the ferrite nucleation rate, and cooperates with controlled cooling to make the ferrite dispersed instead of forming a network ferrite at the original austenite grain boundary. Ensure that the non-quenched and tempered steel has high strength and high toughness. In the continuous casting process, the crystallizer + electromagnetic stirring at the end of solidification is used to control the composition uniformity of the ingot from the surface to the inside.
[0025] At the same time, in the manufacturing process of non-quenched and tempered steel round steel, the controlled rolling and controlled cooling process methods are adopted. The use of higher heating temperature can make the second phase particles such as AlN and V (C / N) fully dissolved in austenite, and can be finely dispersed and precipitated in the subsequent forging and cooling process, thereby achieving the purpose of dispersion strengthening. At the same time, the heating temperature is not higher than 1300℃, which ensures that the Nb element and Ti (C / N) particles are not dissolved in austenite, playing a role in fine grain strengthening.
[0026] The starting rolling temperature of the controlled rolling process is 1100℃~1200℃. The starting rolling temperature is relatively high because the Nb contained increases the termination temperature of austenite recrystallization. Rolling or forging in the non-recrystallization zone of austenite obtains elongated deformed austenite, increases the total area of effective austenite grain boundaries, and increases the ferrite nucleation position, thereby obtaining fine ferrite grains and improving the toughness of the steel.
[0027] At the same time, after the non-quenched and tempered round steel is rolled, a finishing process can be added to improve the dimensional accuracy of the non-quenched and tempered round steel. After the round steel is rolled, it enters the cooling chamber and controls the cooling speed by controlling the wind speed, spray flow rate and spray water temperature. In the controlled cooling process, the cooling rate of 950℃~850℃ is 5℃ / s~20℃ / s and the cooling method of air cooling + mist cooling is adopted. Since the round steel is in the high temperature section after the rolling, a higher cooling rate is adopted and bainite will not be produced. At the same time, the higher cooling rate increases the nucleation rate of ferrite, and the ferrite nucleates at the grain boundary and in the crystal, making the ferrite dispersed and the grains fine.
[0028] The cooling rate at 850℃~600℃ is 1℃ / s~8℃ / s, and air cooling is adopted. At this time, the round steel is in the medium temperature section after rolling. At this time, austenite begins to transform into ferrite and pearlite, among which ferrite first nucleates in the original austenite grain and grain boundary, and then pearlite nucleates again; the cooling rate in the medium temperature section cannot be greater than 8℃ / s, otherwise bainite will be produced. After a certain temperature between 600℃~620℃, it enters the material bin pile for slow cooling, and cools to room temperature at a cooling rate of less than 5℃ / min to ensure sufficient self-tempering of the workpiece.
[0029] Furthermore, in the processing technology of non-quenched and tempered steel cylinder piston rod, the process method of controlled forging and controlled cooling is adopted. The upsetting force is 1.5 times of the standard upsetting force. Increasing the upsetting force can increase the deformation rate, which is conducive to grain refinement and at the same time ensures good piston rod forming effect. In the heating stage, the non-quenched and tempered round steel is heated evenly inside and outside at 950℃~1000℃ to avoid coarse grains on the outer surface of the round steel, reduce thermal stress, and improve the temperature uniformity of the round steel.
[0030] The heating temperature of the controlled forging process is 1200℃~1250℃, which has the same benefits as controlled rolling. The initial forging temperature of the controlled forging process is 1150℃~1200℃. The integral piston rod adopts a higher initial forging temperature. This is because the high-temperature austenite has higher plasticity, which ensures the forming effect of the integral piston rod after local upsetting; the benefits of the initial forging temperature are the same as those of the initial rolling temperature. After the piston rod is upset, it enters the through cooling chamber. The high-temperature cooling chamber is equipped with a high-speed fan and a spray device, and the medium-temperature cooling chamber is equipped with a high-speed fan. The cooling speed is controlled by controlling the wind speed, spray flow and spray water temperature.
[0031] Furthermore, the traditional piston rod needs quenching and tempering and rough turning, while the non-quenched and tempered steel can be exempted from quenching and tempering and rough turning, which reduces the processing steps, shortens the processing cycle, and significantly improves the processing efficiency; at the same time, no heat treatment is required, which avoids heat treatment deformation and further reduces the processing allowance. Through the finishing process of the rolling process and the forming control of the upsetting process, the processing allowance of the electroplating area, that is, the non-upsetting area, is 0.4mm~1mm. Compared with the 5mm~7mm processing allowance of the traditional piston rod, the processing allowance is significantly reduced and the machining efficiency is significantly improved.
[0032] Furthermore, tensile tests, impact tests, and hardness tests were conducted on the non-tempered steel of the present invention that controls the mass ratio of (V+Al+Nb+Ti) / N by "controlled forging and controlled cooling", the non-tempered steel of the present invention that does not "control forging and controlled cooling", and the traditional non-tempered steel of "controlled forging and controlled cooling". The experiments show that the comprehensive mechanical properties of the non-tempered steel of the present invention are higher than those of the traditional non-tempered steel and the non-tempered steel of the present invention that does not "control forging and controlled cooling".
[0033] Meanwhile, the microstructure inspection results show that the pearlite and ferrite in the present invention are equiaxed crystals, the average grain size of pearlite is 19.2 μm, the relative content is 47%, and the average grain size of ferrite is 18.4 μm, the relative content is 53%.
[0034] The metallographic appearance of the conventional non-quenched and tempered steel is that the pearlite is equiaxed, with a maximum grain size of 58.4μm, a minimum grain size of 19.4μm, an average grain size of 36.7μm, and a relative content of 59%; the ferrite is fine equiaxed, with an average grain size of 21.3μm and a relative content of 41%. It can be seen that the relative content of ferrite in the present invention is relatively high, the average grain sizes of ferrite and pearlite are relatively close, and the metallographic structure has good uniformity, thereby improving the mechanical properties and service life of the oil cylinder piston rod made of non-quenched and tempered steel for the integral piston rod of the oil cylinder, so that it has higher hardness, tensile strength, yield strength, cross-sectional shrinkage, elongation after fracture and impact energy. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 The present invention provides a metallographic structure diagram of a non-quenched and tempered steel for an integral piston rod of an oil cylinder.
[0036] Figure 2 It is a traditional non-quenched and tempered steel metallographic structure diagram. DETAILED DESCRIPTION
[0037] The technical solution of the present invention is further described in detail below through specific implementation methods.
[0038] Example 1
[0039] The present embodiment provides a non-quenched and tempered steel for an integral piston rod of an oil cylinder, wherein the chemical composition and mass percentage are: C 0.285%, Si 0.67%, Mn 1.32%, V 0.108%, Ti 0.031%, Nb 0.0055%, Al 0.021%, N 0.032%, P 0.005%, S 0.05%, Mo 0.01%, Cr 0.005%, Ni 0.003%, and the balance is Fe and unavoidable impurities. Among them, the mass ratio of V / N is 3.43, and the mass ratio of (V+Al+Nb+Ti) / N is 5.17.
[0040] Example 2
[0041] The present embodiment provides a non-quenched and tempered steel for an integral piston rod of an oil cylinder, wherein the chemical composition and mass percentage thereof are: C 0.295%, Si 0.73%, Mn 1.38%, V 0.12%, Ti 0.0375%, Nb 0.008%, Al 0.026%, N 0.035%, P 0.004%, S 0.05%, Mo 0.01%, Cr 0.005%, Ni 0.003%, and the remainder is Fe and unavoidable impurities, wherein the mass ratio of V / N is 3.43, and the mass ratio of (V+Al+Nb+Ti) / N is 5.47.
[0042] Example 3
[0043] The present embodiment provides a non-quenched and tempered steel for an integral piston rod of an oil cylinder, wherein the chemical composition and mass percentage thereof are: C 0.24%, Si 0.5%, Mn 1.2%, V 0.075%, Ti 0.02%, Nb 0.005%, Al 0.014%, N 0.025%, S 0.045%, P < 0.02%, Mo 0.01%, Cr 0.005%, Ni 0.003%, and the balance is Fe and unavoidable impurities;
[0044] Among them, the mass ratio of V / N is controlled at 3.0, and the mass ratio of (V+Al+Nb+Ti) / N is 4.7.
[0045] Example 4
[0046] The present embodiment provides a non-quenched and tempered steel for an integral piston rod of an oil cylinder, wherein the chemical composition and mass percentage thereof are: C 0.36%, Si 0.85%, Mn 1.6%, V 0.15%, Ti 0.05%, Nb 0.01%, Al 0.036%, N 0.04%, S 0.06%, P < 0.02%, Mo 0.01%, Cr 0.005%, Ni 0.003%, the remainder being Fe and unavoidable impurities, the mass ratio of V / N being controlled at 3.0-4.0, and the mass ratio of (V+Al+Nb+Ti) / N being 5.7.
[0047] Specifically, the functions and bases of the various elements in the non-quenched and tempered steel provided by the present invention are as follows:
[0048] C element: C is the most economical and basic strengthening element in steel, which can significantly improve the strength of steel. As the carbon content in steel increases, the yield and tensile strengths increase, but the plasticity and impact resistance decrease. The C content range in this case can ensure that the ferrite-pearlite non-quenched and tempered steel has a high strength, while the plasticity and toughness do not decrease significantly.
[0049] Si element: Si significantly strengthens ferrite, and its solid solution strengthening effect is higher than that of manganese, which effectively improves the strength of steel. The mass percentage of Si in the non-quenched and tempered steel described in the present invention is limited to 0.5-0.85%, which can improve the toughness of the steel and avoid the phenomenon of reducing toughness by producing martensite or bainite due to Si content higher than 0.85%.
[0050] Mn element: Mn is an important alloying element for improving the strength and toughness of non-quenched and tempered steel. Mn is a weak carbide-forming element. It mainly exists in the form of solid solution in steel and is solid-dissolved in ferrite at room temperature. The solid-dissolved Mn has a strong solid-solution strengthening effect. The solid-solution strengthening effect of Mn is second only to P and Si. When the Mn content is lower than 0.80%, its strengthening effect is not obvious. When the Mn content exceeds 1.6%, it promotes the bainitization of steel, and the productivity of bainite in steel increases with the increase of Mn content. In addition, Mn combines with sulfur in steel to form MnS, which has less harm to the performance of steel, reduces or inhibits the generation of FeS, can improve cutting performance and expansion performance, and reduce wear on the tool.
[0051] V element: V is the main alloying element for strengthening non-quenched and tempered steel. It mainly exists in the steel in the form of V carbonitride compounds, and these V carbonitrides are dispersed in the proeutectoid ferrite in very fine particles, resulting in precipitation strengthening, thereby achieving the effect of improving the strength of ferrite-pearlite non-quenched and tempered steel, especially significantly improving the yield strength of steel. In addition, during the rolling or forging process of steel, a part of V carbonitrides will precipitate due to strain induction, which plays a role in pinning the austenite grain boundary, thereby inhibiting the recrystallization of austenite and preventing grain growth, which has the effect of refining grains and achieving the purpose of improving strength and toughness. This effect is particularly obvious when the V content is high.
[0052] Ti element: By adding Ti, stable and fine dispersed TiN / TiC particles can be formed. TiN / TiC can effectively prevent the growth of austenite grains. Non-quenched and tempered steel containing Ti still has fine austenite grains when heated to 1250℃, which can increase the initial forging temperature of the piston rod. However, the Ti content cannot be too high, because the affinity of Ti to N is greater than that of V. Too high Ti will consume more N, thereby reducing the precipitation strengthening effect of V. At the same time, based on economic considerations, the Ti content should not be too high.
[0053] Nb element: Nb can significantly increase the austenite recrystallization termination temperature. After forging, non-quenched and tempered steel forms elongated deformed austenite through large deformation in the austenite non-recrystallization zone, increasing the effective grain boundary area of austenite, increasing the ferrite nucleation position, obtaining fine ferrite grains, and improving the toughness of steel. Nb can combine with N and C to have the effect of precipitation strengthening. However, the cost of Nb is relatively high.
[0054] Al element: Al is added to steel for deoxidation during the steelmaking process. In addition, Al and N form AlN particles that can effectively refine the grains and play a role in pinning the austenite grain boundaries, thereby inhibiting the recrystallization of austenite and preventing grain growth, thus refining the grains and achieving the purpose of improving strength and toughness. To achieve the above effects, the mass percentage of aluminum should be no less than 0.016%, but when the mass percentage of aluminum exceeds 0.033%, aluminum oxide impurities are easily generated.
[0055] N element: N plays an important role in V-containing steel. First, N and alloying elements such as V, Ti, and Nb are easy to produce nitrides or nitrogen carbides. These nitrides can pin the austenite grain boundaries, inhibit their growth, effectively organize the coarse austenite grains, and play a role in refining the grains, thereby improving the strength and toughness of the steel through precipitation strengthening; second, with the increase of N content, the precipitation strengthening effect of VN is enhanced, and the strength of non-quenched and tempered steel is improved; third, V (N, C) particles precipitated independently or attached to MnS can serve as the nucleation core of ferrite to form ferrite. These ferrites formed inside austenite play a role in segmenting the austenite grains that have not been transformed, which is equivalent to refining the austenite grains, and finally refining the ferrite-pearlite structure, improving the strength and toughness of ferrite-pearlite non-quenched and tempered steel; on the other hand, if the mass percentage of N in the steel is too high, it is easy to produce void defects and even cracks.
[0056] P element: P is a harmful element in steel, especially reducing the toughness of steel. The P content should be controlled below 0.02%.
[0057] S element: S combines with Mn to form MnS, VN will precipitate on MnS, ferrite and VN have high lattice coherence, VN can become the nucleus of ferrite. Too high S content will damage the hot working performance of steel.
[0058] In order to make V, Nb, Ti, and Al fully and stably play their roles, the mass ratio of (V+Al+Nb+Ti) / N and V / N should be accurately controlled. The mass ratio of V / N is controlled at: 3.0-4.0, and the mass ratio of (V+Al+Nb+Ti) / N is controlled at: 4.7-5.7, so that ferrite-pearlite non-quenched and tempered steel with good comprehensive performance can be obtained. Below this value, there will be free N in the steel, which will damage the toughness of the steel; above this value, that is, the N content in the steel is insufficient, and a large amount of V exists in the form of solid solution, which in a sense causes a waste of V.
[0059] Example 5
[0060] This embodiment provides a method for manufacturing the non-quenched and tempered steel for the integral piston rod of the oil cylinder described in Embodiment 1, comprising: using electric furnace steelmaking, ladle refining, ladle vacuum degassing, completing steelmaking, and then continuous casting.
[0061] During the continuous casting process, the crystallizer + electromagnetic stirring at the end of solidification is used to control the uniformity of the composition of the ingot from the surface to the inside, and then controlled rolling and controlled cooling are performed. During the controlled rolling process, the heating temperature of the ingot is 1200℃, the initial rolling temperature is 1130℃, the final rolling temperature is 1000℃, and the temperature of the finishing process is 950℃.
[0062] During the primary controlled cooling process, the cooling rate from 920℃ to 850℃ is 8℃ / s, and the cooling rate from 850℃ to 600℃ is 3℃ / s; after cooling to 610℃, it enters the material box for stack cooling and cools to room temperature at a cooling rate of 3.4℃ / min.
[0063] Among them, the cooling method of air cooling + mist cooling is adopted at 950℃~850℃, and the cooling method of air cooling is adopted at 850℃~600℃, and the Φ100.6mm round steel is obtained as the original material for the subsequent manufacturing of cylinder piston rod.
[0064] Example 6
[0065] This embodiment provides a cylinder piston rod made of the non-quenched and tempered steel for the cylinder integral piston rod provided in Embodiment 1 and Embodiment 5. The cylinder piston rod is made by the following steps:
[0066] Step (1), the size is determined according to the design process requirements, and the processing allowance of the electroplating area is 0.6mm.
[0067] Step (2), locally upsetting the sized round steel to obtain an integral piston rod blank.
[0068] Among them, local upsetting deformation adopts vertical closed die forging, and the heating method is medium frequency induction heating. When induction heating reaches 980℃, the current frequency is reduced to half of the original setting value to increase the effective heating depth, which is helpful for the uniform temperature inside and outside of non-quenched and tempered round steel. When the temperature of the non-quenched and tempered steel section tends to be consistent, the original current frequency is restored and continued to heat to 122℃. During the local upsetting process, the initial forging temperature is 1180℃, the final forging temperature is 970℃; the upsetting force is 14000kN. During the secondary controlled cooling process, the cooling rate of 950℃~850℃ is 7℃ / s, and the cooling rate of 850℃~600℃ is 2.5℃ / s; after cooling to 610℃, it enters the material box for stack cooling, and cools to room temperature at a cooling rate of 3.3℃ / min. Among them, 950℃~850℃ adopts the cooling method of air cooling + mist cooling, and 850℃~600℃ adopts the cooling method of air cooling.
[0069] Step (2), the whole piston rod blank is finely turned and ground, and then electroplated. The electroplating method is to first plate milky white chrome and then hard chrome, and finally polish to the drawing size.
[0070] Example 7
[0071] This embodiment provides a method for manufacturing the non-quenched and tempered steel for the integral piston rod of the oil cylinder described in Example 2, including: using electric furnace steelmaking, ladle refining, ladle vacuum degassing, completing steelmaking, and then continuous casting.
[0072] During the continuous casting process, the crystallizer + electromagnetic stirring at the end of solidification is used to control the uniformity of the composition of the ingot from the surface to the inside, and then controlled rolling and primary controlled cooling are performed. During the controlled rolling process, the heating temperature of the ingot is 1220℃, the initial rolling temperature is 1180℃, the final rolling temperature is 990℃, and the temperature of the finishing process is 950℃. During the primary controlled cooling process, the cooling rate from 920℃ to 850℃ is 115℃ / s, and the cooling rate from 850℃ to 600℃ is 7℃ / s; after cooling to 600, it enters the material box for stack cooling, and cools to room temperature at a cooling rate of 4.3℃ / min. Among them, 950℃ to 850℃ adopts the cooling method of air cooling + mist cooling, and 850℃ to 600℃ adopts the cooling method of air cooling. Obtained Φ180.9mm round steel as the original material for the subsequent manufacture of cylinder piston rods.
[0073] Example 8
[0074] This embodiment provides a cylinder piston rod made of the non-quenched and tempered steel for the integral cylinder piston rod provided in Embodiment 2 and Embodiment 7. The cylinder piston rod is made by the following steps:
[0075] Step (1), the size is determined according to the design process requirements, and the processing allowance of the electroplating area is 0.9mm.
[0076] Step (2), locally upsetting the sized round steel to obtain an integral piston rod blank.
[0077] Among them, local upsetting deformation adopts vertical closed die forging, and the heating method is medium frequency induction heating. When the induction heating reaches 950-1000℃, the current frequency is reduced to half of the original setting value to increase the effective heating depth, which is conducive to the uniform temperature inside and outside of the non-quenched and tempered round steel. When the temperature of the non-quenched and tempered steel section tends to be consistent, the original current frequency is restored and continued to heat to 1200℃-1250℃. During the local upsetting process, the initial forging temperature is 1170℃, the final forging temperature is 970℃; the upsetting force is 14500kN. During the controlled cooling process, the cooling rate of 950℃-850℃ is 15℃ / s, and the cooling rate of 850℃-600℃ is 6.5℃ / s; after cooling to 610℃, it enters the material box for stack cooling, and cools to room temperature at a cooling rate of 4.4℃ / min. Among them, 950℃-850℃ adopts the cooling method of air cooling + mist cooling, and 850℃-600℃ adopts the cooling method of air cooling.
[0078] Step (3), the whole piston rod blank is finely turned and ground, and then electroplated. The electroplating method is to first plate milky white chrome and then hard chrome, and finally polish to the drawing size.
[0079] Specifically, the mechanical properties of the oil cylinder piston rod prepared in Example 6 were tested. At the same time, two groups of comparative tests were performed for comparison.
[0080] They are respectively comparative test 1: the components in the present invention are replaced with the non-quenched and tempered steel components in publication number CN101492788A, and other manufacturing steps and parameters remain unchanged.
[0081] Comparative experiment 2: Only the step of "controlled forging and controlled cooling" in manufacturing the oil cylinder piston rod of the present invention is omitted, and the composition and other steps remain unchanged.
[0082] Specific test data are shown in Table 1. It can be found from Table 1 that the comprehensive mechanical properties of the oil cylinder piston rod prepared by the present invention are higher than those of the comparative test 1 and the comparative test 2, and also have higher impact energy.
[0083] At the same time, the non-quenched and tempered steel for the integral piston rod of the oil cylinder obtained in Example 1 of the present invention and the comparative test 1 were subjected to microstructural analysis, and the results were as follows: Figure 1 and Figure 2 shown.
[0084] from Figure 1 It can be seen that the specific metallographic structure of the non-quenched and tempered steel for the integral piston rod of the oil cylinder obtained in Example 1 of the present invention is: black is pearlite, and white is ferrite. Pearlite and ferrite are equiaxed crystals, the average grain size of pearlite is 19.2μm, the relative content is 47%, and the average grain size of ferrite is 18.4μm, and the relative content is 53%.
[0085] from Figure 2 It can be seen that the specific metallographic structure of the non-quenched and tempered steel obtained in the comparative test 1 is as follows: pearlite is equiaxed, with a maximum grain size of 58.4μm, a minimum grain size of 19.4μm, an average pearl grain size of 36.7μm, and a relative content of 59%; ferrite is fine equiaxed, with an average grain size of 21.3μm and a relative content of 41%.
[0086] It can be seen that the ferrite content in the present invention is relatively high, the average grain size of ferrite and pearlite is relatively close, and the metallographic structure is uniform, thereby improving the mechanical properties and service life of the oil cylinder piston rod made of non-quenched and tempered steel for the oil cylinder integral piston rod. It has higher hardness, tensile strength, yield strength, cross-sectional shrinkage, elongation after fracture and impact energy.
[0087] Table 1 Comparison of piston rod process performance in this application process and comparative test
[0088]
[0089]
[0090] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, ordinary technicians in the field should understand that the specific implementation methods of the present invention can still be modified or some technical features can be replaced by equivalents without departing from the spirit of the technical solution of the present invention, which should be included in the scope of the technical solution for protection of the present invention.
Claims
1. A non-quenched and tempered steel for an integral piston rod of an oil cylinder, characterized in that: It is composed of the following chemical components in percentage by mass: C 0.24%~0.36%, Si 0.5%~0.85%, Mn 1.2%~1.6%, V 0.075%~0.15%, Ti 0.02%~0.05%, Nb 0.005%~0.01%, Al 0.014%~0.036%, N 0.025%~0.04%, S 0.045%~0.06%, P<0.02%, Mo≤0.02%, Cr≤0.01%, Ni≤0.01%, the balance is Fe and unavoidable impurities; Among them, the mass ratio of V / N is controlled at 3.0-4.0, and the mass ratio of (V+Al+Nb+Ti) / N is controlled at 4.7-5.
7.
2. The non-quenched and tempered steel for the integral piston rod of the oil cylinder according to claim 1, characterized in that: The chemical composition is composed of the following percentages by mass: C 0.28%~0.30%, Si 0.65%~0.75%, Mn 1.3%~1.4%, V 0.09%~0.13%, Ti 0.03%~0.04%, Nb 0.005%~0.01%, Al 0.020%~0.029%, N 0.03%~0.035%, S 0.045%~0.06%, P<0.02%, Mo≤0.02%, Cr≤0.01%, Ni≤0.01%, the balance is Fe and unavoidable impurities; The mass ratio of V / N is controlled within the range of 3.3 to 3.7, and the mass ratio of (V+Al+Nb+Ti) / N is controlled within the range of 5.0 to 5.
4.
3. The non-quenched and tempered steel for the integral piston rod of the oil cylinder according to claim 1 or 2, characterized in that: It is composed of the following chemical components in percentage by mass: C 0.285%, Si 0.67%, Mn 1.32%, V 0.108%, Ti 0.031%, Nb 0.0055%, Al 0.021%, N0.032%, P 0.005%, S 0.05%, Mo 0.01%, Cr 0.005%, Ni 0.003%, and the balance is Fe and unavoidable impurities. Among them, the mass ratio of V / N is 3.43, and the mass ratio of (V+Al+Nb+Ti) / N is 5.
17.
4. The non-quenched and tempered steel for the integral piston rod of the oil cylinder according to claim 1 or 2, characterized in that: It is composed of the following chemical components in percentage by mass: C 0.295%, Si 0.73%, Mn 1.38%, V 0.12%, Ti 0.0375%, Nb 0.008%, Al 0.026%, N0.035%, P 0.004%, S 0.05%, Mo 0.01%, Cr 0.005%, Ni 0.003%, and the balance is Fe and unavoidable impurities. Among them, the mass ratio of V / N is 3.43, and the mass ratio of (V+Al+Nb+Ti) / N is 5.
47.
5. A method for manufacturing a piston rod, comprising the following steps: Provided is a non-quenched and tempered steel for an integral piston rod of a cylinder as claimed in any one of claims 1 to 4; The non-quenched and tempered steel is processed through induction heating, controlled forging, secondary controlled cooling, local upsetting, precision turning, grinding and electroplating to obtain a piston rod.
6. The method for manufacturing a piston rod according to claim 5, characterized in that: The steps of providing the non-quenched and tempered steel for the integral piston rod of the oil cylinder include: electric furnace steelmaking, ladle refining, ladle vacuum degassing, continuous casting, controlled rolling, and primary controlled cooling; The chemical composition and mass percentage of the ingot in the continuous casting step are as follows: C 0.24%-0.36%, Si 0.5%-0.85%, Mn 1.2%-1.6%, V 0.075%-0.15%, Ti 0.02%-0.05%, Nb 0.005%-0.01%, Al 0.014%-0.036%, N 0.025%-0.04%, S 0.045%-0.06%, P < 0.02%, Mo ≤ 0.02%, Cr ≤ 0.01%, Ni ≤ 0.01%, the balance is Fe and unavoidable impurities, the mass ratio of V / N is controlled at 3.0-4.0, and the mass ratio of (V+Al+Nb+Ti) / N is controlled at 4.7-5.7; During the controlled rolling step, the heating temperature of the ingot is 1180°C to 1250°C, the initial rolling temperature is 1100°C to 1200°C, the final rolling temperature is 970°C to 1030°C, and the temperature of the finishing process is 920°C to 970°C; During the primary controlled cooling step, the cooling rate from the forging temperature to 850°C is 5°C / s to 20°C / s, the cooling rate from 850°C to 620°C is 1°C / s to 8°C / s, 600°C to 620°C is the critical temperature. After cooling to the critical temperature, it enters the material box for stack cooling and is cooled to room temperature at a cooling rate of less than 5°C / min. Among them, air cooling and mist cooling are carried out from the forging temperature to 850°C, and air cooling is carried out from 850°C to the critical temperature.
7. The method for manufacturing a piston rod according to claim 5 or 6, characterized in that: During the local upsetting process, the initial forging temperature is 1150℃~1200℃, the final forging temperature is 950℃~1000℃, and the upsetting force is P=kF, where k is 1078~1225, and F is the projection area of the non-quenched and tempered steel blank.
8. The method for manufacturing a piston rod according to claim 7, characterized in that: During the secondary controlled cooling process, the cooling rate from the forging temperature to 850°C is 5°C / s to 20°C / s, and the cooling rate from 850°C to 620°C is 1°C / s to 8°C / s; 600°C to 620°C is the critical temperature. After cooling to the critical temperature, it enters the material box for pile cooling and is cooled to room temperature at a cooling rate of less than 5°C / min. Among them, air cooling and mist cooling are carried out from the forging temperature to 850°C, and air cooling is carried out from 850°C to the critical temperature.
Citation Information
Patent Citations
Microalloy non-hardened and tempered steel and controlled forging and cooling process
CN101492788A
Cited By
Manufacturing method for stainless steel integral inner liquid inlet piston rod of hydraulic support oil cylinder
CN119549995A