Acidic spraying material for spraying and depositing zinc-aluminum-magnesium plating layer and preparation method of acidic spraying material

By activating zinc-aluminum magnesium powder in the acid spray material, the zinc-aluminum magnesium plating density and uniformity of zinc-aluminum magnesium plating in the prior art is solved, and the zinc-aluminum magnesium plating layer is achieved. The high-efficiency corrosion resistance and environmental protection performance of steel parts are improved.

CN118932271APending Publication Date: 2024-11-12KUNMING UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410980730.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing jet deposition galvanized coating technology is difficult to form a dense and uniform zinc-aluminum-magnesium coating, resulting in insufficient corrosion resistance and environmental protection performance of steel parts.

Method used

Acid spray materials are used, including component A (zinc-aluminum-magnesium powder and spray deposition medium) and component B (hexamethyltetramine, ammonium molybdate, ferrous sulfate, sodium pyrophosphate, polyethylene glycol, OP- 10 and inorganic strong acid), and then add component A to form an acid spray material sprayed with deposition galvanized aluminum-magnesium plating layer to improve the activity and deposition performance of zinc-aluminum-magnesium powder.

Benefits of technology

A zinc-aluminum-magnesium plating with excellent surface quality, dense and uniform surface quality is formed, which improves the corrosion resistance and environmental protection of steel parts, reduces weight and improves the efficiency of use.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118932271A_ABST
    Figure CN118932271A_ABST
Patent Text Reader

Abstract

The invention discloses an acidic spraying material for spraying and depositing a zinc-aluminum-magnesium plating layer and a preparation method of the acidic spraying material, and belongs to the technical field of spraying and depositing zinc-aluminum-magnesium plating layers. The acidic spraying material for spraying and depositing the zinc-aluminum-magnesium plating layer comprises a component A and a component B, the component A comprises zinc-aluminum-magnesium powder and a spray deposition medium; the component B comprises hexamethylenetetramine, ammonium molybdate, ferrous sulfate, sodium pyrophosphate, polyethylene glycol, OP-10, inorganic strong acid and water. The zinc-aluminum-magnesium powder is modified through hexamethylenetetramine, ammonium molybdate, ferrous sulfate, sodium pyrophosphate, polyethylene glycol, OP-10, inorganic strong acid and water, the probability that the zinc-aluminum-magnesium powder is peeled off when a deposition medium is sprayed is reduced, the zinc-aluminum-magnesium powder is deposited on the surface of a matrix, and a compact and uniform zinc-aluminum-magnesium coating is formed. Compared with a traditional coating workpiece, the zinc-aluminum-magnesium coating steel workpiece is more excellent in surface quality, the added value of the workpiece is improved, and the zinc-aluminum-magnesium coating steel workpiece has more excellent environmental protection performance and better corrosion resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of spray-deposited zinc-aluminum-magnesium coatings, and in particular relates to an acidic spray material for spray-deposited zinc-aluminum-magnesium coatings and a preparation method thereof. Background Art

[0002] The actual application environment of steel parts is becoming more and more complex, so the requirements for the corrosion resistance of steel parts have been greatly increased. Nowadays, environmental issues are also an issue that cannot be ignored in practical applications. The environmental performance and corrosion resistance of materials are equally important for steel parts. Zinc-aluminum-magnesium coating can make steel parts have excellent corrosion resistance while having good environmental performance. Zinc-aluminum-magnesium coating can also improve the wear resistance and high temperature resistance of steel parts.

[0003] Zinc-aluminum-magnesium powder and zinc powder have completely different chemical properties, electrode potentials, and surface activities. The reactions occurring on the surface of steel parts are not the same, which results in the existing developed spray material catalysts for spray-deposited zinc plating having no reference value. In addition, there is a large gap in chemical affinity between zinc-aluminum-magnesium powder and the surface of steel, making it difficult to form a dense and uniform zinc-aluminum-magnesium coating. Therefore, it has become inevitable to develop an acidic spray material suitable for zinc-aluminum-magnesium powder for the preparation of spray-deposited zinc-aluminum-magnesium coating. Summary of the invention

[0004] In view of the above-mentioned shortcomings of the prior art, the present invention provides an acidic spray material for spray-depositing zinc-aluminum-magnesium coating and a preparation method thereof.

[0005] To achieve the above object, the technical solution adopted by the present invention is:

[0006] An acidic spray material for spray-depositing zinc-aluminum-magnesium coating comprises component A and component B; the component A comprises zinc-aluminum-magnesium powder and a spray-depositing medium; the component B comprises hexamethylenetetramine, ammonium molybdate, ferrous sulfate, sodium pyrophosphate, polyethylene glycol, OP-10, a strong inorganic acid and water.

[0007] As a preferred embodiment of the present invention, the mass ratio of the zinc aluminum magnesium powder in the A component to the spray deposition medium is 1:100-200.

[0008] As a preferred embodiment of the present invention, the B component includes the following components in percentage by mass: 6% to 8% hexamethylenetetramine, 7% to 9% ammonium molybdate, 5% to 12% ferrous sulfate, 4% to 9% sodium pyrophosphate, 19% to 27% polyethylene glycol, 2% to 5% OP-10, 3% to 7% strong inorganic acid and the remainder water.

[0009] As a preferred embodiment of the present invention, the mass ratio of the spray deposition medium in the A component to the B component is 3:1.

[0010] As a preferred embodiment of the present invention, the inorganic strong acid is at least one of hydrochloric acid, sulfuric acid, nitric acid and hydrofluoric acid.

[0011] As a preferred embodiment of the present invention, the spray deposition medium is at least one of zirconium beads, alumina beads and steel beads.

[0012] The present invention also claims a method for preparing the acidic spray material for spray-deposited zinc-aluminum-magnesium coating, comprising:

[0013] (1) placing an inorganic strong acid in water and stirring, and adding hexamethylenetetramine, ammonium molybdate, ferrous sulfate, sodium pyrophosphate, polyethylene glycol and OP-10 during the stirring process until the mixture is uniformly stirred to obtain component B;

[0014] (2) Adding component A to component B obtains an acidic spray material for spray-deposited zinc-aluminum-magnesium coating.

[0015] Compared with the prior art, the present invention has the following beneficial effects:

[0016] The invention modifies zinc-aluminum-magnesium powder by using hexamethylenetetramine, ammonium molybdate, ferrous sulfate, sodium pyrophosphate, polyethylene glycol, OP-10 and inorganic strong acid, thereby reducing the probability of zinc-aluminum-magnesium powder peeling off when spraying a deposition medium, so that the zinc-aluminum-magnesium powder is deposited on the surface of a substrate and forms a dense and uniform zinc-aluminum-magnesium coating. Compared with traditional coated parts, zinc-aluminum-magnesium coated steel parts have better surface quality, improve the added value of the parts, and have better environmental protection performance and better anti-corrosion performance. In addition, compared with traditional coated parts of the same thickness, the weight is greatly reduced, thereby improving the use efficiency of the parts. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 This is an appearance diagram of a gasket with a zinc-aluminum-magnesium coating prepared in Example 3 of the present invention.

[0018] Figure 2 This is the XRD diagram of the zinc-aluminum-magnesium alloy coating of the gasket prepared in Example 3 of the present invention. DETAILED DESCRIPTION

[0019] In order to better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments.

[0020] Example 1

[0021] A method for preparing an acidic spray material for spray-depositing a zinc-aluminum-magnesium coating comprises the following steps:

[0022] (1) Add 480 ml of water to a beaker and slowly pour concentrated sulfuric acid and concentrated nitric acid into the beaker using a glass rod, then add hexamethylenetetramine, ammonium molybdate, ferrous sulfate, sodium pyrophosphate, polyethylene glycol, and OP-10 and stir evenly to obtain component B. Component B includes the following components in percentage by weight: 8% hexamethylenetetramine, 7% ammonium molybdate, 5% ferrous sulfate, 4% sodium pyrophosphate, 19% polyethylene glycol, 4% OP-10, 3% concentrated sulfuric acid, 2% concentrated nitric acid, and the balance water.

[0023] (2) Component A (15 g zinc aluminum magnesium powder, 2 kg zirconium beads and 1 kg steel beads) was added to component B and mixed evenly to obtain an acidic spray material for spray-deposited zinc aluminum magnesium coating; the mass ratio of the spray-deposited medium in component A to component B was 3:1.

[0024] The acidic spray material of the spray-deposited zinc-aluminum-magnesium coating is subjected to a spray-deposited coating preparation process to form a zinc-aluminum-magnesium coating, comprising:

[0025] S1: Add the acidic spray material of the spray-deposited zinc-aluminum-magnesium coating obtained above into the spray material chamber of the spray deposition plating device; then pickle 1kg of standard Q235 gasket with a thickness of 2mm to remove the oxide layer, then wash with alkali to remove the oil stains on the gasket, and then add it into the spray deposition chamber from the feed inlet.

[0026] S2: After the nozzle is turned on to perform spray deposition plating on the rotating gasket for 480 seconds, a dense and uniform zinc-aluminum-magnesium coating is formed on the surface of the gasket.

[0027] Example 2

[0028] A method for preparing an acidic spray material for spray-depositing a zinc-aluminum-magnesium coating comprises the following steps:

[0029] (1) Add 455 ml of water to a beaker and slowly pour concentrated sulfuric acid and concentrated nitric acid into the beaker using a glass rod, then add hexamethylenetetramine, ammonium molybdate, ferrous sulfate, sodium pyrophosphate, polyethylene glycol, and OP-10 and stir evenly to obtain component B. Component B includes the following components in percentage by weight: 6% hexamethylenetetramine, 8% ammonium molybdate, 9% ferrous sulfate, 9% sodium pyrophosphate, 27% polyethylene glycol, 2% OP-10, 1% concentrated sulfuric acid, 3% concentrated nitric acid, and the balance water.

[0030] (2) Component A (20 g zinc aluminum magnesium powder, 2 kg zirconium beads and 2 kg alumina beads) was added to component B and mixed evenly to obtain an acidic spray material for spray-deposited zinc aluminum magnesium coating; the mass ratio of the spray-deposited medium in component A to component B was 3:1.

[0031] The acidic spray material of the spray-deposited zinc-aluminum-magnesium coating is subjected to a spray-deposited coating preparation process to form a zinc-aluminum-magnesium coating, comprising:

[0032] S1: Add the acidic spray material of the spray-deposited zinc-aluminum-magnesium coating obtained above into the spray material chamber of the spray deposition plating device; then pickle 1kg of standard Q235 gasket with a thickness of 2mm to remove the oxide layer, then wash with alkali to remove the oil stains on the gasket, and then add it into the spray deposition chamber from the feed inlet.

[0033] S2: After opening the nozzle to perform spray deposition plating on the rotating gasket for 720 seconds, a dense and uniform zinc-aluminum-magnesium coating is formed on the surface of the gasket.

[0034] Example 3

[0035] A method for preparing an acidic spray material for spray-depositing a zinc-aluminum-magnesium coating comprises the following steps:

[0036] (1) Add 592 ml of water to a beaker and slowly pour concentrated sulfuric acid, concentrated nitric acid and concentrated hydrochloric acid into the beaker using a glass rod, then add hexamethylenetetramine, ammonium molybdate, ferrous sulfate, sodium pyrophosphate, polyethylene glycol, and OP-10 and stir evenly to obtain component B. Component B includes the following components in percentage by weight: 8% hexamethylenetetramine, 9% ammonium molybdate, 12% ferrous sulfate, 4% sodium pyrophosphate, 19% polyethylene glycol, 5% OP-10, 3% concentrated sulfuric acid, 2% concentrated nitric acid, 2% concentrated hydrochloric acid and the balance water.

[0037] (2) Component A (25 g zinc aluminum magnesium powder, 2 kg zirconium beads and 3 kg alumina beads) was added to component B and mixed evenly to obtain an acidic spray material for spray-deposited zinc aluminum magnesium coating; the mass ratio of the spray-deposited medium in component A to component B was 3:1.

[0038] The acidic spray material of the spray-deposited zinc-aluminum-magnesium coating is subjected to a spray-deposited coating preparation process to form a zinc-aluminum-magnesium coating, comprising:

[0039] S1: Add the acidic spray material of the spray-deposited zinc-aluminum-magnesium coating obtained above into the spray material chamber of the spray deposition plating device; then pickle 1kg of standard Q235 gasket with a thickness of 2mm to remove the oxide layer, then wash with alkali to remove the oil stains on the gasket, and then add it into the spray deposition chamber from the feed inlet.

[0040] S2: After opening the nozzle to perform spray deposition plating on the rotating gasket for 720 seconds, a dense and uniform zinc-aluminum-magnesium coating is formed on the surface of the gasket.

[0041] according to Figure 1 and Figure 2 It can be seen that Example 3 of the present invention successfully prepared a zinc-aluminum-magnesium coating on the surface of the gasket, and the zinc-aluminum-magnesium coating was dense and uniform.

[0042] Comparative Example 1

[0043] A spray deposition coating preparation process forms a zinc-aluminum-magnesium coating, comprising:

[0044] (1) The workpiece to be plated is a standard gasket with an outer diameter of Φ30 mm, an inner diameter of Φ20 mm, and a thickness of 2 mm. The surface area of ​​the workpiece to be plated is approximately 0.12 m 2 .

[0045] S1: Add 15g zinc aluminum magnesium powder into 1000ml water, then add 2kg zirconium beads and 1kg steel beads, mix evenly, and add into the spraying chamber; then pickle 1kg standard Q235 gasket with a thickness of 2mm to remove the oxide layer, then wash with alkali to remove the oil stain on the gasket, and then add into the spray deposition chamber from the feed port.

[0046] S2: After the nozzle is turned on to perform spray deposition plating on the rotating gasket for 480 seconds, no zinc-aluminum-magnesium plating layer is formed on the surface of the gasket.

[0047] Comparative Example 2

[0048] The only difference between the method for preparing the acidic spray material for spray-deposited zinc-aluminum-magnesium coating described in this comparative example and that in Example 1 is that in step (2), the zinc-aluminum-magnesium powder is replaced with zinc powder of equal mass.

[0049] The only difference between the acidic spraying material for the spray-deposited zinc-aluminum-magnesium coating in this comparative example, which is formed by the spray-deposited coating preparation process into a zinc-aluminum-magnesium coating, and Example 1 is that in step S1, the acidic spraying material for the spray-deposited zinc-aluminum-magnesium coating is replaced by an acidic spraying material for the spray-deposited zinc-aluminum-magnesium coating of equal mass prepared in this comparative example.

[0050] Comparative Example 3

[0051] The only difference between the method for preparing the acidic spray material for spray-deposited zinc-aluminum-magnesium coating described in this comparative example and that in Example 2 is that in step (2), the zinc-aluminum-magnesium powder is replaced with zinc powder of equal mass.

[0052] The only difference between the acidic spraying material for the spray-deposited zinc-aluminum-magnesium coating in this comparative example, which is formed by the spray-deposited coating preparation process into a zinc-aluminum-magnesium coating, and Example 2 is that in step S1, the acidic spraying material for the spray-deposited zinc-aluminum-magnesium coating is replaced by an acidic spraying material for the spray-deposited zinc-aluminum-magnesium coating of equal mass prepared in this comparative example.

[0053] Comparative Example 4

[0054] The only difference between the method for preparing the acidic spray material for spray-deposited zinc-aluminum-magnesium coating described in this comparative example and that in Example 3 is that in step (2), the zinc-aluminum-magnesium powder is replaced with zinc powder of equal mass.

[0055] The only difference between the acidic spraying material for the spray-deposited zinc-aluminum-magnesium coating in this comparative example, which is formed by the spray-deposited coating preparation process into a zinc-aluminum-magnesium coating, and Example 3 is that in step S1, the acidic spraying material for the spray-deposited zinc-aluminum-magnesium coating is replaced by an acidic spraying material for the spray-deposited zinc-aluminum-magnesium coating of equal mass prepared in this comparative example.

[0056] Comparative Example 5

[0057] The only difference between the preparation method of the acidic spray material for spray-deposited zinc-aluminum-magnesium coating described in this comparative example and that in Example 1 is that in the step (1), component B includes the following components in percentage by weight: 8% hexamethylenetetramine, 7% ammonium molybdate, 4% sodium pyrophosphate, 19% polyethylene glycol, 4% OP-10, 3% concentrated sulfuric acid, 2% concentrated nitric acid and the remainder water.

[0058] The only difference between the acidic spraying material for the spray-deposited zinc-aluminum-magnesium coating in this comparative example, which is formed by the spray-deposited coating preparation process into a zinc-aluminum-magnesium coating, and Example 1 is that in step S1, the acidic spraying material for the spray-deposited zinc-aluminum-magnesium coating is replaced by an acidic spraying material for the spray-deposited zinc-aluminum-magnesium coating of equal mass prepared in this comparative example.

[0059] Effect example

[0060] The coating density, coating bonding strength, coating average thickness and corrosion resistance of the spray-deposited zinc-aluminum-magnesium coating gaskets of the above-mentioned Examples 1-3 and Comparative Examples 2-5 were tested, and the results are shown in Table 1 below.

[0061] The density of the coating is determined by measuring the porosity.

[0062] Plating bonding strength test: Use the scribing and cross-grid method, refer to GC / T 5270-2005, and observe whether there is any lifting or shedding of the coating at the cross-intersection position of the scribing.

[0063] Neutral salt spray test: The sample is suspended in a salt spray chamber and sprayed continuously. The test environment temperature is 25°C and the corrosion resistance process is in NaCl salt spray with a mass fraction of 5%.

[0064] Table 1

[0065]

[0066] According to Table 1, it can be seen from Examples 1-3 and Comparative Examples 2-4 that a uniform zinc coating is also formed on the gasket in Comparative Example 2-4, but the bonding between the zinc coating and the substrate is weak and is prone to falling off, and the corrosion resistance of the zinc coating is significantly different from that of the zinc-aluminum-magnesium coating.

[0067] Compared with Example 5, in Example 5, the acidic spray material for spray-depositing the zinc-aluminum-magnesium coating lacks ferrous sulfate and therefore cannot activate the zinc-aluminum-magnesium powder, making it difficult to form a dense and uniform zinc-aluminum-magnesium coating on the substrate. Furthermore, the generated zinc-aluminum-magnesium coating has a weak bonding force with the substrate and is prone to falling off.

[0068] The hexamethylenetetramine, ammonium molybdate, ferrous sulfate, sodium pyrophosphate, polyethylene glycol, OP-10 and inorganic strong acid of the present invention synergistically improve the dissolution and activation of zinc-aluminum-magnesium powder and the bonding force between the deposited layer and the substrate. If one of the substances is missing, the acidic spray material for spray-depositing the zinc-aluminum-magnesium coating cannot form a zinc-aluminum-magnesium coating. Even if a zinc-aluminum-magnesium coating is formed, its bonding force with the substrate is weak, and it falls off, and the corrosion resistance is similar to that of Comparative Example 5: for example, if ferrous sulfate is missing, a zinc-aluminum-magnesium coating cannot be generated, and the generated coating is very easy to fall off, and has poor corrosion resistance. Lack of inorganic strong acid or replacement of inorganic strong acid with weak acid will reduce the reaction between zinc-aluminum-magnesium powder and other substances, reduce the activity of zinc-aluminum-magnesium powder, and the generated zinc-aluminum-magnesium coating has poor density and uniformity, and is very easy to fall off, and has poor corrosion resistance. Lack of polyethylene glycol and OP-10, zinc-aluminum-magnesium coating cannot be generated. Lack of hexamethylenetetramine will cause the solution acidity to be too high, resulting in rapid and violent reaction of zinc-aluminum-magnesium powder. Under extremely acidic conditions, the metal on the surface of the powder may dissolve rapidly, releasing a large amount of hydrogen and generating high heat, posing a risk of fire or explosion.

[0069] The above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the protection scope of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. An acidic spray material for spray-depositing zinc-aluminum-magnesium coating, characterized in that: The invention comprises component A and component B; the component A comprises zinc aluminum magnesium powder and a spray deposition medium; the component B comprises hexamethylenetetramine, ammonium molybdate, ferrous sulfate, sodium pyrophosphate, polyethylene glycol, OP-10, a strong inorganic acid and water.

2. The acidic spray material for spray-depositing zinc-aluminum-magnesium coating according to claim 1, characterized in that: The mass ratio of zinc aluminum magnesium powder to spray deposition medium in the A component is 1:100-200.

3. The acidic spray material for spray-depositing zinc-aluminum-magnesium coating as claimed in claim 1, characterized in that: The B component comprises the following components in percentage by mass: 6% to 8% hexamethylenetetramine, 7% to 9% ammonium molybdate, 5% to 12% ferrous sulfate, 4% to 9% sodium pyrophosphate, 19% to 27% polyethylene glycol, 2% to 5% OP-10, 3% to 7% inorganic strong acid and the balance water.

4. The acidic spray material for spray-depositing zinc-aluminum-magnesium coating as claimed in claim 1, characterized in that: The mass ratio of the spray deposition medium in the A component to the B component is 3:

1.

5. The acidic spray material for spray-depositing zinc-aluminum-magnesium coating as claimed in claim 1, characterized in that: The inorganic strong acid is at least one of hydrochloric acid, sulfuric acid, nitric acid and hydrofluoric acid.

6. The acidic spray material for spray-depositing zinc-aluminum-magnesium coating as claimed in claim 1, characterized in that: The spray deposition medium is at least one of zirconium beads, alumina beads and steel beads.

7. The method for preparing the acidic spray material for spray-deposited zinc-aluminum-magnesium coating according to any one of claims 1 to 6, characterized in that: include: (1) placing an inorganic strong acid in water and stirring, and adding hexamethylenetetramine, ammonium molybdate, ferrous sulfate, sodium pyrophosphate, polyethylene glycol and OP-10 during the stirring process until the mixture is uniformly stirred to obtain component B; (2) Adding component A to component B obtains an acidic spray material for spray-deposited zinc-aluminum-magnesium coating.