Mixture powder, coating, preparation method of mixture powder and coating and application of mixture powder and coating to TC bearing

By using a mixture of composite tungsten carbide material and nickel-iron alloy powder in TC bearings and forming a composite coating using laser cladding, the problems of wear, heat-affected zone and cost of TC bearings have been solved, and the bonding strength and production efficiency have been improved.

CN118932330APending Publication Date: 2024-11-12WEDO NEW MATERIAL TECH CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410984315.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Existing TC bearings suffer from uneven wear, easy peeling of carbide blocks, deep heat-affected zone, high cost, and low production efficiency during processing, especially in thin-walled parts and complex structural designs.

Method used

A composite powder containing tungsten carbide and nickel-iron alloy is used to form a composite coating between cemented carbide blocks through laser cladding, which improves the bonding strength and reduces the depth of the heat-affected zone, thereby increasing production efficiency.

Benefits of technology

This achieves metallurgical bonding between the cemented carbide block and the substrate, reduces the depth of the heat-affected zone, improves product production efficiency and surface smoothness, and reduces grinding allowance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118932330A_ABST
    Figure CN118932330A_ABST
Patent Text Reader

Abstract

The invention provides mixture powder, a coating, a preparation method of the mixture powder and the coating and application of the mixture powder and the coating to a TC bearing. The mixture powder is composed of, by mass, 10%-80% of a composite tungsten carbide material and 20%-90% of a nickel-iron alloy. The mixture powder is applied to the TC bearing, and a composite tungsten carbide material and a nickel-iron alloy material are cladded in gaps between hard alloy blocks by adopting a laser cladding method to form a composite coating material; therefore, metallurgical bonding of the base body, the hard alloy block, the nickel-iron alloy material and the tungsten carbide particles is achieved, the bonding strength among the hard alloy block, the nickel-iron-based composite tungsten carbide cladding layer and the base body is improved, the depth of a heat affected zone on the base body in the coating preparation process is reduced, and the production efficiency of a product is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of bearing technology, and in particular to a mixed material powder, a coating, a preparation method thereof, and an application thereof in a TC bearing. Background Art

[0002] TC bearing is one of the key parts of screw drill, mainly plays the role of straightening the transmission shaft, so it is also called radial straightening bearing. TC bearing is mainly composed of moving sleeve and static sleeve. The moving sleeve is fixed on the transmission shaft, and the static sleeve is connected to the transmission shaft housing. There is a certain gap between the moving sleeve and the static sleeve to facilitate the passage of mud for cooling and lubrication. When TC bearing is working, it is mainly subjected to the scouring of mud fluid, the abrasive wear of mud sand particles and the application of lateral load. Therefore, there are two main failure states of TC: first, wear and erosion of the matrix bonding phase; second, due to the lateral load, the contact surface of the moving sleeve and the static sleeve is subjected to thermal fatigue, resulting in cracking and falling off of the alloy block; third, the mechanical properties of the matrix are reduced after the coating, which leads to fatigue fracture of the steel parts.

[0003] The conventional preparation method for TC bearing processing is to use high-temperature sintering technology and plasma surfacing technology. High-temperature sintering technology is to embed carbide blocks, solder and additives on the surface of the inner and outer bearings of TC and sinter them at high temperature. However, due to the relatively soft hardness of the brazing filler metal between the carbide blocks, it wears before the carbide blocks, and there are problems such as uneven wear between the inner and outer sleeves of the TC bearings, and the hard blocks are easy to peel off, causing the TC bearings to fail and be scrapped in advance. Plasma surfacing technology refers to pre-setting carbide blocks on the surface of the inner and outer bearings of TC, and then filling the mixed solder between the carbide blocks by cladding. The mixed solder used is usually a mixed powder of cast spherical tungsten carbide and nickel-based self-fluxing alloy powder. Due to the large energy of plasma surfacing, it will cause a deeper heat-affected range on the substrate, usually reaching a depth of 4mm to 10mm. For thin-walled TC bearings, it will cause the mechanical properties to decrease and break during use; on the other hand, the spherical cast tungsten carbide used in the solder is expensive, the surface of the product is uneven after surfacing, and there is a lot of grinding allowance, which reduces the production efficiency of the product and increases the manufacturing cost of the product.

[0004] Application Contents

[0005] The present application is made in view of the above-mentioned problems, and its purpose is to provide a mixed powder, the coating obtained by laser cladding has high bonding strength with the TC bearing substrate and the cemented carbide block, and at the same time reduces the depth of the heat-affected zone of the substrate during the coating preparation process. The surface flatness of the product after laser cladding is good, the grinding allowance of the product is reduced, and the production efficiency of the product is improved.

[0006] Specifically, the first aspect of the present application provides a mixed material powder, which is composed of a composite tungsten carbide material with a mass fraction of 10% to 80% and a nickel-iron alloy with a mass fraction of 20% to 90%;

[0007] The composite tungsten carbide material includes the following preparation raw materials:

[0008] WC, Ni, Co and grain growth inhibitors;

[0009] The nickel-iron alloy includes the following elements:

[0010] Ni, Fe, B and Si.

[0011] According to some embodiments of the present application, the composite tungsten carbide material includes the following raw materials by weight:

[0012] WC 70% to 92%, Ni 4% to 28%, Co 4% to 28% and grain growth inhibitor 0.5% to 1%. According to some embodiments of the present application, the nickel-iron alloy includes the following elements in weight fractions:

[0013] Ni 35% to 95%, Fe 0.5% to 50%, B 1.5% to 3%, Si 2% to 4% and C<0.1%.

[0014] According to some embodiments of the present application, the first carbide grain growth inhibitor includes at least one of TaC or NbC.

[0015] According to some embodiments of the present application, the composite tungsten carbide material includes the following raw materials by weight:

[0016] WC 70% to 90%, Ni 4% to 28%, Co 4% to 28% and grain growth inhibitor 0.5% to 1%.

[0017] According to some embodiments of the present application, the composite tungsten carbide material includes the following raw materials by weight:

[0018] WC 72% to 90%, Ni 4% to 28%, Co 4% to 28% and grain growth inhibitor 0.5% to 1%.

[0019] According to some embodiments of the present application, the composite tungsten carbide material includes the following raw materials by weight:

[0020] WC 72% to 90%, Ni 4% to 10%, Co 10% to 28% and grain growth inhibitor 0.5% to 1%.

[0021] According to some embodiments of the present application, the composite tungsten carbide material includes the following raw materials by weight:

[0022] WC 72% to 90%, Ni 4% to 10%, Co 10% to 15% and grain growth inhibitor 0.5% to 1%.

[0023] According to some embodiments of the present application, the composite tungsten carbide material includes the following raw materials by weight:

[0024] WC 80% to 90%, Ni 4% to 10%, Co 10% to 15% and grain growth inhibitor 0.5% to 1%.

[0025] According to some embodiments of the present application, the composite tungsten carbide material includes the following raw materials by weight:

[0026] WC 80% to 85%, Ni 4% to 10%, Co 10% to 15% and grain growth inhibitor 0.5% to 1%.

[0027] According to some embodiments of the present application, the composite tungsten carbide material includes the following raw materials by weight:

[0028] WC 80% to 85%, Ni 4% to 10%, Co 10% to 15% and grain growth inhibitor 0.6% to 1%.

[0029] According to some embodiments of the present application, the composite tungsten carbide material includes the following raw materials by weight:

[0030] WC 80% to 85%, Ni 4% to 10%, Co 10% to 15% and grain growth inhibitor 0.6% to 0.8%.

[0031] According to some embodiments of the present application, the mass ratio of TaC to NbC is 1:0.5 to 1.5.

[0032] According to some embodiments of the present application, the mass ratio of TaC to NbC is 1:0.8-1.2.

[0033] According to some embodiments of the present application, the mass ratio of TaC to NbC is 1:0.9 to 1.1.

[0034] According to some embodiments of the present application, the mass ratio of TaC to NbC is 1:1.0 to 1.1.

[0035] According to some embodiments of the present application, the nickel-iron alloy includes the following elements by weight:

[0036] Ni 35% to 95%, Fe 0.5% to 60%, B 1.5% to 3%, Si 2% to 4% and C 0.001% to 0.1%. According to some embodiments of the present application, the nickel-iron alloy includes the following elements in weight fractions:

[0037] Ni 35% to 95%, Fe 0.5% to 60%, B 1.5% to 3%, Si 2% to 4% and C 0.001% to 0.08%. According to some embodiments of the present application, the nickel-iron alloy includes the following elements in weight fractions:

[0038] Ni 35% to 45%, Fe 0.5% to 60%, B 1.5% to 3%, Si 2% to 4% and C 0.001% to 0.08%. According to some embodiments of the present application, the nickel-iron alloy includes the following elements in weight fractions:

[0039] Ni 35% to 45%, Fe 50% to 60%, B 1.5% to 3%, Si 2% to 4% and C 0.001% to 0.08%. According to some embodiments of the present application, the nickel-iron alloy includes the following elements in weight fractions:

[0040] Ni 40% to 45%, Fe 50% to 55%, B 1.5% to 3%, Si 2% to 4%, and C 0.001% to 0.08%.

[0041] According to some embodiments of the present application, the particle size of the composite tungsten carbide material is 100 mesh to 300 mesh.

[0042] According to some embodiments of the present application, the nickel-iron alloy is 80 mesh to 200 mesh.

[0043] The second aspect of the present application provides a coating, which is prepared by laser cladding method using the mixed material powder described in the first aspect of the present application.

[0044] The third aspect of the present application provides a method for preparing a coating, comprising the following steps:

[0045] The mixed powder is prepared by laser cladding method;

[0046] The laser cladding method includes the following process parameters:

[0047] The output power of the laser is 1.0kW to 3.0kW;

[0048] The spot diameter is 2mm~4mm.

[0049] According to some embodiments of the present application, the scanning speed of the laser is 6 mm / s to 13 mm / s.

[0050] According to some embodiments of the present application, the defocus amount during the laser cladding process is -1 mm or 1 mm.

[0051] According to some embodiments of the present application, the overlap rate during the laser cladding process is 50%.

[0052] According to some embodiments of the present application, the laser energy density during the laser cladding process is 45 J / mm 2 ~75J / mm 2 .

[0053] According to some embodiments of the present application, the output power of the laser is 1.4 kW to 2.2 kW.

[0054] A fourth aspect of the present application provides a TC bearing, comprising:

[0055] matrix;

[0056] Part of the surface area of ​​the substrate is provided with a hard alloy block;

[0057] Another part of the surface of the substrate is provided with a coating;

[0058] The coating is composed of the following raw materials in mass fraction:

[0059] 10% to 80% of composite tungsten carbide material and 20% to 90% of nickel-iron alloy;

[0060] The composite tungsten carbide material includes the following raw materials in weight fraction:

[0061] WC 70% to 92%, Ni 4% to 28%, Co 4% to 28% and grain growth inhibitor 0.5% to 1%;

[0062] The nickel-iron alloy includes the following elements in weight fractions:

[0063] Ni 35% to 95%, Fe 0.5% to 50%, B 1.5% to 3%, Si 2% to 4% and C<0.1%.

[0064] According to some embodiments of the present application, the grain growth inhibitor includes at least one of TaC or NbC.

[0065] According to some embodiments of the present application, the thickness of the coating is 0.5 mm to 4 mm.

[0066] According to some embodiments of the present application, the composite tungsten carbide material includes the following raw materials by weight:

[0067] WC 70% to 90%, Ni 4% to 28%, Co 4% to 28% and grain growth inhibitor 0.5% to 1%.

[0068] According to some embodiments of the present application, the composite tungsten carbide material includes the following raw materials by weight:

[0069] WC 72% to 90%, Ni 4% to 28%, Co 4% to 28% and grain growth inhibitor 0.5% to 1%.

[0070] According to some embodiments of the present application, the particle size of the composite tungsten carbide material is 100 mesh to 300 mesh.

[0071] According to some embodiments of the present application, the nickel-iron alloy is 80 mesh to 200 mesh.

[0072] According to some embodiments of the present application, the cemented carbide block is composed of the following components in mass fractions:

[0073] 88%~90% WC and 10%~12% Co.

[0074] According to some embodiments of the present application, the grain size in the cemented carbide block is 2 μm to 4 μm.

[0075] The fifth aspect of the present application provides a method for preparing the TC bearing according to the fourth aspect of the present application, comprising the following steps:

[0076] A plurality of cemented carbide blocks are fixed on the surface of the substrate;

[0077] A laser cladding method is then used to form a coating on the cemented carbide block.

[0078] According to some embodiments of the present application, the laser cladding method includes the following parameters:

[0079] The output power of the laser is 1.0kW to 3.0kW;

[0080] The spot diameter is 2mm to 4mm;

[0081] According to some embodiments of the present application, the output power of the laser is 1.4 kW to 2.2 kW.

[0082] According to some embodiments of the present application, the carrier gas in the laser cladding process is argon.

[0083] According to some embodiments of the present application, the protector in the laser cladding process is argon gas.

[0084] This application has at least the following beneficial effects:

[0085] The mixed powder in the present application is applied to TC bearings, and a laser cladding method is used to clad a composite tungsten carbide material and a nickel-iron alloy material in the gaps between cemented carbide blocks to form a composite coating material; thereby achieving metallurgical bonding of the substrate, cemented carbide blocks, nickel-iron alloy materials and tungsten carbide particles, improving the bonding strength between the cemented carbide blocks, the nickel-iron-based composite tungsten carbide cladding layer and the substrate, reducing the depth of the heat-affected zone of the substrate during the coating preparation process, and improving the production efficiency of the product. BRIEF DESCRIPTION OF THE DRAWINGS

[0086] In order to more clearly illustrate the embodiments of the present drawings or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present drawings. For ordinary technicians in this field, other drawings can be obtained based on the structures shown in these drawings without paying any creative work.

[0087] Figure 1 This is a metallographic image of the TC bearing prepared in Example 1.

[0088] Figure 2 The following are sample block pictures after coating preparation corresponding to Example 1 and Comparative Examples 1 to 3.

[0089] Figure 3 The figure is a graph showing the wear resistance test results of Example 3 and Comparative Example 3.

[0090] Figure 4 It is a comparison diagram of the heat affected areas of Example 3 and Comparative Example 3.

[0091] The purpose, features and advantages of this figure will be further described in conjunction with the embodiments with reference to the accompanying drawings. DETAILED DESCRIPTION

[0092] In order to make the purpose, technical solutions and advantages of the present application clearer, the present application is described and illustrated below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not intended to limit the present application. Based on the embodiments provided in the present application, all other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of the present application.

[0093] Obviously, the drawings described below are only some examples or embodiments of the present application. For ordinary technicians in this field, the present application can also be applied to other similar scenarios based on these drawings without creative work. In addition, it can also be understood that although the efforts made in this development process may be complicated and lengthy, for ordinary technicians in this field related to the content disclosed in this application, some changes in design, manufacturing or production based on the technical content disclosed in this application are just conventional technical means, and should not be understood as insufficient content disclosed in this application.

[0094] However, unnecessary detailed descriptions may be omitted. For example, detailed descriptions of well-known matters and repeated descriptions of substantially the same structures may be omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate understanding by those skilled in the art. In addition, the drawings and the following description are provided to enable those skilled in the art to fully understand the present application and are not intended to limit the subject matter described in the claims.

[0095] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.

[0096] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.

[0097] "Scope" disclosed in the present application is limited in the form of lower limit and upper limit, and a given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of a special range. The scope limited in this way can be including end values ​​or not including end values, and can be arbitrarily combined, that is, any lower limit can be combined with any upper limit to form a scope. For example, if the scope of 60-120 and 80-110 is listed for a specific parameter, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range values ​​1 and 2 are listed, and if the maximum range values ​​3, 4 and 5 are listed, the following scope can be all expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In the present application, unless otherwise specified, the numerical range "ab" represents the abbreviation of any real number combination between a and b, wherein a and b are real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" are listed in this document, and "0-5" is just an abbreviation of these numerical combinations. In addition, when a parameter is expressed as an integer ≥ 2, it is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.

[0098] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.

[0099] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.

[0100] If there is no special explanation, all steps of the present application can be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), which means that step (c) may be added to the method in any order. For example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.

[0101] If there is no special explanation, the "include" and "comprising" mentioned in this application are open-ended or closed-ended. For example, the "include" and "comprising" may mean that other components not listed may also be included or only the listed components may be included or only the listed components may be included.

[0102] If not specifically stated, in this application, the term "or" is inclusive. For example, the phrase "A or B" means "A, B, or both A and B". More specifically, any of the following conditions satisfies the condition "A or B": A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).

[0103] Specifically, the first aspect of the present application provides a mixed material powder, which is composed of a composite tungsten carbide material with a mass fraction of 10% to 80% and a nickel-iron alloy with a mass fraction of 20% to 90%;

[0104] The composite tungsten carbide material includes the following preparation raw materials:

[0105] WC, Ni, Co and grain growth inhibitors;

[0106] The nickel-iron alloy includes the following elements:

[0107] Ni, Fe, B and Si.

[0108] According to some embodiments of the present application, the composite tungsten carbide material includes the following raw materials by weight:

[0109] WC 70% to 92%, Ni 4% to 28%, Co 4% to 28% and grain growth inhibitor 0.5% to 1%. According to some embodiments of the present application, the nickel-iron alloy includes the following elements in weight fractions:

[0110] Ni 35% to 95%, Fe 0.5% to 50%, B 1.5% to 3%, Si 2% to 4% and C<0.1%.

[0111] According to some embodiments of the present application, the grain growth inhibitor includes at least one of TaC or NbC.

[0112] According to some embodiments of the present application, the composite tungsten carbide material includes the following raw materials by weight:

[0113] WC 70% to 90%, Ni 4% to 28%, Co 4% to 28% and grain growth inhibitor 0.5% to 1%.

[0114] According to some embodiments of the present application, the particle size of the composite tungsten carbide material is 100 mesh to 300 mesh.

[0115] According to some embodiments of the present application, the nickel-iron alloy is 80 mesh to 200 mesh.

[0116] According to some embodiments of the present application, the nickel-iron alloy material is prepared by aerosolization.

[0117] According to some embodiments of the present application, the composite tungsten carbide material is produced by a pulse electric spark method.

[0118] According to some embodiments of the present application, the pulsed electric spark method comprises the following steps:

[0119] WC powder, Ni powder, Co powder and grain growth inhibitor powder are mixed and pressed to prepare a pressed block;

[0120] The pressed blocks are sintered at high temperature in a pressure furnace to obtain cemented carbide blocks with uniform composition and dense structure. The blocks are made into micron-sized spheres by a pulsed electric spark machine under appropriate pulse width and pulse interval parameters, and then the spherical powder material of the composite carbide is obtained by a screening system.

[0121] According to some embodiments of the present application, the pressing pressure is 100 MPa to 300 MPa.

[0122] According to some embodiments of the present application, the high temperature sintering temperature is 1350°C to 1500°C.

[0123] According to some embodiments of the present application, the high temperature sintering pressure is 1.5 MPa to 10 MPa.

[0124] According to some embodiments of the present application, the pulse width of the pulse electric spark machine is 200 μs to 300 μs.

[0125] According to some embodiments of the present application, the pulse interval of the pulse electric spark machine is 50 μs to 100 μs.

[0126] According to some embodiments of the present application, the regulated current of the pulse electric spark machine is 25A to 30A.

[0127] According to some embodiments of the present application, the voltage of the pulse electric spark machine is 40V to 50V.

[0128] The second aspect of the present application provides a coating, which is prepared by laser cladding method using the mixed material powder described in the first aspect of the present application.

[0129] The third aspect of the present application provides a method for preparing a coating, comprising the following steps:

[0130] The mixed powder is prepared by laser cladding method;

[0131] The laser cladding method includes the following process parameters:

[0132] The output power of the laser is 1.0kW to 3.0kW;

[0133] The spot diameter is 2mm~4mm.

[0134] According to some embodiments of the present application, the scanning speed of the laser is 6 mm / s to 13 mm / s.

[0135] According to some embodiments of the present application, the defocus amount during the laser cladding process is -1 mm or 1 mm.

[0136] According to some embodiments of the present application, the overlap rate during the laser cladding process is 50%.

[0137] According to some embodiments of the present application, the laser energy density during the laser cladding process is 45 J / mm 2 ~75J / mm 2 .

[0138] According to some embodiments of the present application, the output power of the laser is 1.4 kW to 2.2 kW.

[0139] A fourth aspect of the present application provides a TC bearing, comprising:

[0140] matrix;

[0141] Part of the surface area of ​​the substrate is provided with a hard alloy block;

[0142] Another part of the surface of the substrate is provided with a coating;

[0143] The coating is composed of the following raw materials in mass fraction:

[0144] 10% to 80% of composite tungsten carbide material and 20% to 90% of nickel-iron alloy;

[0145] The composite tungsten carbide material includes the following raw materials in weight fraction:

[0146] WC 70% to 92%, Ni 4% to 28%, Co 4% to 28% and grain growth inhibitor 0.5% to 1%;

[0147] The nickel-iron alloy includes the following elements in weight fractions:

[0148] Ni 35% to 95%, Fe 0.5% to 60%, B 1.5% to 3%, Si 2% to 4% and C less than 0.1%.

[0149] According to some embodiments of the present application, the grain growth inhibitor includes at least one of TaC or NbC.

[0150] According to some embodiments of the present application, the thickness of the coating is 0.5 mm to 4 mm.

[0151] According to some embodiments of the present application, the composite tungsten carbide material includes the following raw materials by weight:

[0152] WC 70% to 90%, Ni 4% to 28%, Co 4% to 28% and grain growth inhibitor 0.5% to 1%.

[0153] According to some embodiments of the present application, the particle size of the composite tungsten carbide material is 100 mesh to 300 mesh.

[0154] According to some embodiments of the present application, the nickel-iron alloy is 80 mesh to 200 mesh.

[0155] According to some embodiments of the present application, the cemented carbide block is composed of the following components in mass fractions:

[0156] 88%~90% WC and 10%~12% Co.

[0157] According to some embodiments of the present application, the grain size in the cemented carbide block is 2 μm to 4 μm.

[0158] The fifth aspect of the present application provides a method for preparing the TC bearing according to the fourth aspect of the present application, comprising the following steps:

[0159] A plurality of cemented carbide blocks are fixed on the surface of the substrate;

[0160] A laser cladding method is then used to form a coating on the cemented carbide block.

[0161] According to some embodiments of the present application, the laser cladding method includes the following parameters:

[0162] The output power of the laser is 1.0kW to 3.0kW;

[0163] The spot diameter is 2mm to 4mm;

[0164] According to some embodiments of the present application, the output power of the laser is 1.4 kW to 2.2 kW.

[0165] This application has at least the following beneficial effects:

[0166] The mixed powder in the present application is applied to TC bearings, and a laser cladding method is used to clad a composite tungsten carbide material and a nickel-iron alloy material in the gaps between cemented carbide blocks to form a composite coating material; thereby achieving metallurgical bonding of the substrate, cemented carbide blocks, nickel-iron alloy materials and tungsten carbide particles, improving the bonding strength between the cemented carbide blocks, the nickel-iron-based composite tungsten carbide cladding layer and the substrate, reducing the depth of the heat-affected zone of the substrate during the coating preparation process, and improving the production efficiency of the product.

[0167] According to some embodiments of the present application, the substrate is a metal substrate; preferably, the metal substrate can be made of steel, and the grade, performance, shape, size of the substrate steel and the distribution of the cemented carbide blocks on the surface of the steel are selected. The shape of the steel can be a plane or a curved surface.

[0168] A layer of nickel-based material is applied on the surface of the steel by flame spraying or conductive adhesive coating.

[0169] Using the "fast discharge" device, the cemented carbide block is placed on the surface of the above-mentioned nickel-based material, and then a large current is applied instantly, so that the cemented carbide block and the nickel-based material are instantly heated, and the temperature is higher than the melting point of the nickel-based material and lower than the liquidus point of the cemented carbide. At this time, the molten nickel-based material wets the lower surface of the cemented carbide block. When the current stops, the molten nickel-based material solidifies quickly and acts as a solder, welding the cemented carbide block and the steel together. At this time, there is a certain gap between the horizontal and vertical directions of the cemented carbide block.

[0170] The steel parts with the carbide blocks fixed on the surface are placed on the laser cladding device, which is equipped with an automatic powder feeder containing mixed powder of nickel-iron alloy material and composite tungsten carbide material. The walking track of laser cladding is compiled according to the required structure and size of the workpiece.

[0171] Start the program, the laser cladding device will generate a laser spot, the mixed powder in the automatic powder feeder enters the laser spot, the energy generated by the laser melts the nickel-iron alloy material to form a molten pool, the molten pool is mixed with composite tungsten carbide material particles and filled in the gaps between the above-mentioned cemented carbide blocks, when the laser spot leaves the molten pool, the molten pool will solidify and form a metallurgical bond between the steel and the cemented carbide blocks, thereby realizing the composite of steel, cemented carbide blocks, nickel-iron alloy materials and composite tungsten carbide material particles to form a TC bearing precursor.

[0172] After the composite hard material coating is prepared and cooled, the composite hard material is processed into industrial equipment parts with complex structure and size by grinding and milling.

[0173] In the present application, the cross-sectional shape of the cemented carbide block can be a polygon such as a rectangle, a circle, an ellipse, or a rhombus.

[0174] In the present application, the thickness of the cemented carbide block is 3 mm to 4 mm.

[0175] In the present application, taking the case where the cross-sectional shape of the cemented carbide block is rectangular as an example, the length of the cemented carbide block is 10 mm to 15 mm, and the width is 3 mm to 8 mm.

[0176] In the present application, during the process of flame spraying the nickel-based material layer on the surface of the base steel, the combustion medium is acetylene, propane or atomized kerosene, the injection combustion air flow pressure is 0.5MPa~0.8MPa, and the thickness of the formed nickel-based material is 0.06mm~1mm.

[0177] The conductive adhesive used is copper-nickel conductive tape or pure copper conductive adhesive, and the thickness of the solder powder layer is 0.06mm to 1mm.

[0178] In the present application, the current applied between the cemented carbide block and the nickel-based material during the process of fixing the cemented carbide block to the metal substrate is 550A to 700A.

[0179] Example 1

[0180] This embodiment is a mixed material powder and its application.

[0181] The mixed powder in this embodiment is composed of the following components by mass fraction:

[0182] The composite tungsten carbide powder is 25% and the nickel-iron alloy powder is 75%, wherein the particle size of the composite tungsten carbide is 100-300 meshes and is normally distributed, and the particle size of the nickel-iron alloy powder is 80-200 meshes and is normally distributed.

[0183] The composite tungsten carbide powder in this embodiment is composed of the following raw materials in mass fraction:

[0184] WC (grain size is 2μm to 10μm), 81.4%; Ni powder, 5%; Co powder, 13%; grain growth inhibitor 0.6% (TaC, 0.3%; NbC powder, 0.3%).

[0185] The preparation method of the composite tungsten carbide powder in this embodiment is prepared by the following preparation method:

[0186] WC, Ni powder, Co powder, TaC and NbC powder were mixed and wet-milled for 24 hours. The wet-milled mixed powder was pressed by conventional drying and granulation, and the pressing was carried out at a pressure of 150 MPa to obtain pressed blocks.

[0187] The pressed block is then sintered in a pressure furnace at high temperature to obtain a cemented carbide block with uniform composition and dense structure. The block is made into micron-sized spheres by a pulsed EDM machine under appropriate pulse width and pulse interval parameters, and then the spherical powder material of composite tungsten carbide is obtained by a screening system. The high-temperature sintering temperature is 1440℃ and the pressure is 6Mpa; the pulse width of the pulsed EDM machine is 220μs, the pulse interval is 60μs, the regulated current is 26A, and the voltage is 44V.

[0188] The nickel-iron alloy powder in this embodiment is composed of the following elements by mass fraction:

[0189] Ni, 42.52%; Fe, 50.7%; B, 2.9%; Si, 3.8%; C, 0.08%.

[0190] The preparation method of the nickel-iron alloy powder in this embodiment is prepared by the following preparation method:

[0191] It is made by gas atomization method. The raw material blocks with the corresponding proportions of each component are added to the smelting furnace, the smelting temperature is set to 1800℃, the smelting time is 2h, and then the spherical nickel-iron alloy powder is obtained by gas atomization device with nitrogen as cooling gas, and then the spherical nickel-iron alloy powder of the corresponding particle size is obtained by vibration screening system.

[0192] In this embodiment, the mixed material powder is used for preparing TC bearings.

[0193] In this embodiment, the TC bearing includes a base body;

[0194] A nickel-based material layer (thickness 0.08 mm) is provided on the surface of the substrate;

[0195] A plurality of hard alloy blocks and coatings are arranged on the surface of the nickel-based material layer;

[0196] The size of the carbide block is 13mm long*5mm wide*3mm thick;

[0197] The coating is made from the mixed material powder in this embodiment through a laser cladding process.

[0198] The preparation method of the TC bearing in this embodiment comprises the following steps:

[0199] A layer of nickel-based material is coated on the outer surface of a tubular 42CrMo substrate with a size of Φ100 mm outer diameter*Φ70 mm inner diameter*125 mm long by flame spraying using powdered nickel-based powder as a raw material.

[0200] The 40Cr substrate coated with a nickel-based material layer is placed on a fixture of an automatic rapid discharge device; the automatic rapid discharge device is provided with an automatic conveying and holding device for a hard alloy block.

[0201] Start the automatic rapid discharge device, apply 750A current between the cemented carbide block and the nickel-based material layer instantly and keep it for 0.3 seconds before stopping the current output immediately. The heat generated by the instantaneous application and stopping of the current melts the nickel-based material layer and cools and solidifies it. The molten nickel-based material layer spreads and wets the lower surface of the cemented carbide block. When the current stops, the solidified nickel-based alloy brazes the cemented carbide block to the outer surface of the 40Cr substrate.

[0202] The mixed material powder in this embodiment is loaded into the powder feeder of the laser cladding device, and the 40Cr substrate with the cemented carbide block fixed on the surface is placed on the chuck of the laser cladding device and fixed.

[0203] The parameters of laser cladding are as follows: the spot is selected as 3 mm, the power is selected as 1.5 kW, and 99.99% argon is selected as the shielding gas and the carrier gas.

[0204] The laser cladding layer was ground using a resin bond or ceramic bond diamond cylindrical grinding wheel produced by Zhengzhou Abrasives and Grinding Research Institute, and the 40Cr substrate was processed using a milling machine to obtain a component made of composite hard material (see the metallographic diagram of some areas). Figure 1 ).

[0205] Example 2

[0206] This embodiment is a mixed material powder and its application. The difference between this embodiment and embodiment 1 is that the mixed material powder is composed of the following components in mass fractions:

[0207] Composite tungsten carbide powder 10% and nickel-iron alloy powder 90%.

[0208] Example 3

[0209] This embodiment is a mixed material powder and its application. The difference between this embodiment and embodiment 1 is that the mixed material powder is composed of the following components in mass fractions:

[0210] Composite tungsten carbide powder 50% and nickel-iron alloy powder 50%.

[0211] Example 4

[0212] This embodiment is a mixed material powder and its application. The difference between this embodiment and embodiment 1 is that the mixed material powder is composed of the following components in mass fractions:

[0213] Composite tungsten carbide powder 70% and nickel-iron alloy powder 30%.

[0214] Example 5

[0215] This embodiment is a mixed material powder and its application. The difference between this embodiment and embodiment 1 is that the mixed material powder is composed of the following components in mass fractions:

[0216] Composite tungsten carbide powder 80% and nickel-iron alloy powder 20%.

[0217] Comparative Example 1

[0218] This comparative example is a mixed material powder and its application. The difference between this comparative example and Example 1 is only that:

[0219] The composite tungsten carbide powder in this comparative example is composed of the following raw materials by mass fraction:

[0220] WC (grain size is 2μm to 10μm), 67.4%; Ni powder, 19%; Co powder, 13%; TaC, 0.3%; NbC powder, 0.3%.

[0221] Comparative Example 2

[0222] This comparative example is a mixed material powder and its application. The difference between this comparative example and Example 1 is only that:

[0223] The nickel-iron alloy powder in this comparative example is composed of the following elements by mass fraction:

[0224] Ni, 18%; Fe, 75.1%; B, 2.9%; Si, 3.8%; C, 0.2%.

[0225] Comparative Example 3

[0226] This comparative example is a mixed material powder and its application. The difference between this comparative example and Example 1 is:

[0227] A mixed powder of commercial spherical casting tungsten carbide particles and Ni-B-Si self-fluxing alloy powder is selected to replace the mixed powder in Example 1, wherein the spherical casting tungsten carbide particle size is 80-200 mesh, accounting for 50wt% of the mixed powder; the Ni-B-Si self-fluxing alloy powder is 50wt%, with a particle size of 80-200 mesh, and the Ni-B-Si self-fluxing alloy powder includes 94wt% to 95wt% Ni, 1.5wt% to 2wt% B, and 3wt% to 3.5wt% Si. The preparation process of the coating selects the existing public plasma surfacing technology, the surfacing current is 85A to 90A, and the ion gas and shielding gas are high-purity argon.

[0228] The performance testing methods of the embodiments and comparative examples of the present application are as follows:

[0229] The mechanical properties of steel are tested using the universal testing machine of Gangyan Nanok, and the testing standard is based on ASTMA370; the depth of the heat-affected zone is tested by metallographic corrosion method, and 4% nitric acid alcohol is used for detection and analysis; the wear resistance is tested by a wet grinding tester, with a load of 130N, a speed of 200r / min, a time of 30min, and a medium of 50-70 mesh quartz sand; the bonding strength between the coating and the substrate is tested by the three-point bending method, and a comparative analysis is performed based on the peeling situation of the coating and the substrate; the holes and cracks are analyzed and tested by the metallographic method; the amount of machining allowance is measured and analyzed based on the feed size of the external cylindrical grinder after the external cylindrical grinding is flattened.

[0230] The test results are shown in Table 1.

[0231] The sample photos of Example 1, Comparative Example 1, Comparative Example 2, and Comparative Example 3 after coating are shown in the figure. Figure 2 shown.

[0232] The results show that the wear resistance of Comparative Example 1 is much lower than that of other examples due to the decrease in the proportion of tungsten carbide in the composite carbide. The high iron content in the nickel-iron alloy of Comparative Example 2 leads to poor fluidity of the molten pool during the laser cladding process, and the porosity of its coating is significantly increased compared with other examples. In addition, the wear resistance test results of Example 3 and Comparative Example 3 are shown in the following figure. Figure 3 As shown, the results show that under the same mass fraction of WC ratio, the wear resistance of the coating containing the composite tungsten carbide of the present application is better than that of the product with existing mature technology. The mechanical properties of the substrate in Example 3 are also significantly better than those of the existing mature technology product (Comparative Example 3) due to the shallow heat affected zone. The metallographic photograph of the depth comparison of the heat affected zone is as shown in Figure 4 As shown (the depth in Example 3 is 899.711 μm, and the depth in Comparative Example 3 is 4300.64 μm).

[0233] Table 1 Related test items and performance test comparison data record table

[0234]

[0235]

[0236] The mixed powder of the present application has lower manufacturing cost than the spherical casting tungsten carbide and nickel-based self-fluxing alloy mixed powder in the related art. It can be fully combined with cemented carbide blocks and steel parts through laser cladding in TC bearing products. It has excellent characteristics such as low melting point, good molten pool fluidity, good slag removal performance, and low cracking tendency of the weld layer after welding. The wear resistance of the weld layer can be adjusted according to different product working conditions.

[0237] The Hall flow rate of the composite WC powder of the present application can reach the normal level of conventional spherical casting WC, and the fusion property with nickel-iron alloy powder is better. The hole defect is less than 0.1%, and it can be evenly dispersed in the nickel-iron alloy powder. The internal stress of the weld layer after welding is low. Due to the high bonding strength with the nickel-iron alloy powder, the cracking tendency after welding is also low.

[0238] The mixed material powder of the present application has excellent welding performance in laser cladding, and can play an advantage in the welding of fillers of TC bearings, and enhance the bonding strength between the cladding layer and the substrate and the cemented carbide block;

[0239] The mixed material powder of the present application is used through a laser cladding process to produce some thin-walled TC bearings and TC bearings with complex structural designs. The preparation method of the present application has higher production efficiency and lower cost, and the surface flatness of the produced product is good and the processing allowance is small.

[0240] It should be noted that the present application is not limited to the above-mentioned embodiments. The above-mentioned embodiments are only examples, and the embodiments having the same structure as the technical idea and exerting the same effect within the scope of the technical solution of the present application are all included in the technical scope of the present application. In addition, without departing from the scope of the main purpose of the present application, various modifications that can be thought of by those skilled in the art to the embodiments and other methods of combining some of the constituent elements in the embodiments are also included in the scope of the present application.

Claims

1. A mixed material powder, characterized in that: It is composed of 10% to 80% by mass of composite tungsten carbide material and 20% to 90% by mass of nickel-iron alloy; The composite tungsten carbide material includes the following preparation raw materials: WC, Ni, Co and grain growth inhibitors; The nickel-iron alloy includes the following elements: Ni, Fe, B and Si.

2. The mixed material powder according to claim 1, characterized in that: The composite tungsten carbide material includes the following raw materials in weight fraction: WC 70% to 92%, Ni 4% to 28%, Co 4% to 28% and grain growth inhibitor 0.5% to 1%; And / or, the nickel-iron alloy includes the following elements in weight fractions: Ni 35%~95%, Fe 0.5%~60%, B 1.5%~3%, Si 2%~4% and C<0.1%; and / or, the grain growth inhibitor comprises at least one of TaC or NbC; And / or, the composite tungsten carbide material includes the following raw materials in weight fraction: WC 70% to 90%, Ni 4% to 28%, Co 4% to 28% and grain growth inhibitor 0.5% to 1%; And / or, the composite tungsten carbide material includes the following raw materials in weight fraction: WC 72%~90%, Ni 4%~28%, Co 4%~28% and grain growth inhibitor 0.5%~1%; And / or, the composite tungsten carbide material includes the following raw materials in weight fraction: WC 72% to 90%, Ni 4% to 10%, Co 10% to 28% and grain growth inhibitor 0.5% to 1%; And / or, the composite tungsten carbide material includes the following raw materials in weight fraction: WC 72% to 90%, Ni 4% to 10%, Co 10% to 15% and grain growth inhibitor 0.5% to 1%; And / or, the composite tungsten carbide material includes the following raw materials in weight fraction: WC 80% to 90%, Ni 4% to 10%, Co 10% to 15% and grain growth inhibitor 0.5% to 1%; And / or, the composite tungsten carbide material includes the following raw materials in weight fraction: WC 80%-85%, Ni 4%-10%, Co 10%-15% and grain growth inhibitor 0.5%-1%; And / or, the nickel-iron alloy includes the following elements in weight fractions: Ni 35%~95%, Fe 0.5%~60%, B 1.5%~3%, Si 2%~4% and C 0.001%~0.1%; And / or, the nickel-iron alloy includes the following elements in weight fractions: Ni 35%~95%, Fe 0.5%~60%, B 1.5%~3%, Si 2%~4% and C 0.001%~0.08%; And / or, the nickel-iron alloy includes the following elements in weight fractions: Ni 35%~45%, Fe 0.5%~60%, B 1.5%~3%, Si 2%~4% and C 0.001%~0.08%; And / or, the nickel-iron alloy includes the following elements in weight fractions: Ni 35%~45%, Fe 50%~60%, B 1.5%~3%, Si 2%~4% and C 0.001%~0.08%; And / or, the nickel-iron alloy includes the following elements in weight fractions: Ni 40% to 45%, Fe 50% to 55%, B 1.5% to 3%, Si 2% to 4%, and C 0.001% to 0.08%.

3. The mixed material powder according to claim 1, characterized in that: The particle size of the composite tungsten carbide material is 100 mesh to 300 mesh; And / or, the nickel-iron alloy is 80 mesh to 200 mesh.

4. A coating, characterized in that: The mixed material powder according to any one of claims 1 to 3 is prepared by laser cladding method.

5. A method for preparing a coating as claimed in claim 4, characterized in that: The following steps are involved: The mixed powder is prepared by laser cladding method; The laser cladding method includes the following process parameters: The output power of the laser is 1.0kW to 3.0kW; The spot diameter is 2mm~4mm.

6. The preparation method according to claim 5, characterized in that: The output power of the laser is 1.4 kW to 2.2 kW.

7. A TC bearing, characterized in that: include: matrix; Part of the surface area of ​​the substrate is provided with a hard alloy block; Another part of the surface of the substrate is provided with a coating; The coating is composed of the following raw materials in mass fraction: 10% to 80% of composite tungsten carbide material and 20% to 90% of nickel-iron alloy; The composite tungsten carbide material includes the following raw materials in weight fraction: WC 70% to 92%, Ni 4% to 28%, Co 4% to 28% and grain growth inhibitor 0.5% to 1%; The nickel-iron alloy includes the following elements in weight fractions: Ni 35% to 95%, Fe 0.5% to 60%, B 1.5% to 3%, Si 2% to 4% and C<0.1%.

8. The TC bearing according to claim 7, characterized in that: The grain growth inhibitor includes at least one of TaC or NbC; And / or, the coating has a thickness of 0.5 mm to 4 mm; And / or, the composite tungsten carbide material includes the following raw materials in weight fraction: WC 70% to 90%, Ni 4% to 28%, Co 4% to 28% and grain growth inhibitor 0.5% to 1%; And / or, the particle size of the composite tungsten carbide material is 100 mesh to 300 mesh; And / or, the nickel-iron alloy is 80 mesh to 200 mesh; And / or, the cemented carbide block consists of the following components in mass fraction: 88%-90% WC and 10%-12% Co; And / or, the grain size of the cemented carbide block is 2 μm to 4 μm.

9. A method for preparing a TC bearing according to claim 7 or 8, characterized in that: The following steps are involved: A plurality of cemented carbide blocks are fixed on the surface of the substrate; A laser cladding method is then used to form a coating on the cemented carbide block.

10. The preparation method according to claim 9, characterized in that: The laser cladding method includes the following parameters: The output power of the laser is 1.0kW to 3.0kW; The spot diameter is 2mm to 4mm; And / or, the output power of the laser is 1.4 kW to 2.2 kW.

Citation Information

Patent Citations

  • Preparation method of composite hard material

    CN114000087A

  • Tungsten carbide reinforced phase composite powder, coating and preparation method

    CN115055675A

  • High-toughness wear-resistant hard alloy as well as preparation method and application thereof

    CN117737543A

  • Tantalum-reinforced nickel-based tungsten carbide wear-resistant coating and preparation method thereof

    CN118086895A

  • Carbide with toughness-increasing structure

    US20190136353A1