Acidic electrolyzed water anode oxygen evolution electrocatalytic material as well as preparation method and application thereof

By assisting the ball mill to modify the support and loading iridium dioxide, metal oxide support interaction is formed, which solves the problems of high cost of Ir catalyst and poor stability of carbon-based materials, and achieves high stability and low cost acidic electrolytic catalysts , suitable for sustainable energy technology.

CN118932389AActive Publication Date: 2024-11-12TAIYUAN UNIVERSITY OF TECHNOLOGY
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202410644978.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-05-23
Publication Date
2024-11-12
Estimated Expiration
2044-05-23

AI Technical Summary

Technical Problem

In the existing acidic electrolytic hydrogen production technology, the high cost and limited resources of Ir catalysts limit their wide application, and typical carbon-based materials are prone to oxidation in acidic media and have poor electrochemical stability.

Method used

Plasma-assisted ball mill modification support (Nb2O5, Ta2O5, ZrO2 or TiO2) was used and iridium dioxide was supported by hydrothermal method to form metal oxide support interaction (SOSI) to enhance the stability and activity of the catalyst.

Benefits of technology

It improves the stability of the catalyst and the oxygen evolution performance of the acidic electrolytic water catalyzed anode, extends the service life of the catalyst, and maintains high electrocatalytic activity at low Ir content, which is suitable for sustainable energy needs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118932389A_ABST
    Figure CN118932389A_ABST
Patent Text Reader

Abstract

The invention discloses an acidic electrolyzed water anode oxygen evolution electrocatalytic material as well as a preparation method and application thereof. The catalytic material comprises a carrier and iridium dioxide loaded on the carrier, the carrier is selected from Nb2O5, Ta2O5, ZrO2 or TiO2, and the carrier has oxygen-rich defects after plasma-assisted ball milling modification. The method comprises the following steps: loading a carrier and grinding balls into a ball milling tank, and modifying the carrier by adopting plasma-assisted ball milling; weighing iridium trichloride and the modified carrier, and adding water to form a mixed solution; carrying out hydrothermal reaction on the mixed solution at 180-200 DEG C for 12-24 hours, cooling, washing and centrifuging; and drying a centrifugal product to obtain the catalytic material. Plasma-assisted ball milling is adopted for modifying the carrier, oxygen defects are increased, the defects on the carrier can promote interaction between a load and the carrier, the binding force between the load and the carrier is enhanced, the stability of the catalyst is improved, aggregation and stripping of the load are prevented, and therefore the service life of the catalyst is prolonged.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of water electrolysis hydrogen production materials, and in particular to an acidic water electrolysis anode oxygen evolution electrocatalytic material and a preparation method and application thereof. Background Art

[0002] As a clean and efficient secondary energy source, hydrogen energy has become the dominant means of large-scale development, storage and consumption of renewable energy. Among the many hydrogen production technologies, proton exchange membrane (PEM) water electrolysis hydrogen production is considered to be a very promising green hydrogen production technology due to its high efficiency, small footprint and high gas separation purity. However, the current market share of this technology is relatively small, mainly due to the high cost of catalysts, the key material of PEM membrane electrode.

[0003] In acidic environments, the benchmark catalysts are still noble metals such as Ir and Ru. Although Ru shows good catalytic performance in water electrolysis, it is easily oxidized to RuO under high voltage due to its stability issues, especially in the OER electrocatalytic process. 4 And dissolve and lose, affecting its practicality. In contrast, Ir is relatively stable in acidic environments, has good antioxidant properties, and can withstand the test of high voltage and strong oxidizing conditions, thereby reducing the risk of catalyst deactivation. However, the high cost and limited resources of Ir limit its widespread application. Therefore, we are committed to exploring new catalysts to overcome the limitations of Ir, reduce the Ir content while maintaining high catalytic activity, reduce costs, and promote acidic water electrolysis technology to better adapt to sustainable energy needs.

[0004] In this context, loading the catalyst on a carrier can reduce the amount of precious metals used. Anchoring the active material on a carbonaceous matrix is ​​a common approach. However, typical carbon-based materials are easily oxidized in acidic media and exhibit unsatisfactory electrochemical stability. Summary of the invention

[0005] The technical problem to be solved by the present invention is to provide an acidic water electrolysis anode oxygen evolution electrocatalytic material and a preparation method and application thereof, so as to at least achieve the purpose of improving the stability of the catalyst.

[0006] To solve the above technical problems, according to one aspect of the present invention, there is provided an acidic water electrolysis anode oxygen evolution electrocatalytic material, which comprises a carrier and iridium dioxide supported on the carrier, wherein the carrier is selected from Nb 2 O 5 、 2 O 5 、ZrO 2 or TiO 2 , the support has oxygen-rich defects after plasma-assisted ball milling modification.

[0007] According to another aspect of the present invention, provided is a method for preparing the above-mentioned acidic water electrolysis anode oxygen evolution electrocatalytic material, comprising: Step 1, placing the carrier and the grinding balls into a ball milling jar, and modifying the carrier by plasma-assisted ball milling; Step 2, weighing iridium trichloride and the modified carrier, and adding water to form a mixed solution; Step 3, hydrothermally reacting the mixed solution at 180°C-200°C for 12 hours-24 hours, washing and centrifuging after cooling; Step 4: After centrifugation and drying, the catalytic material is obtained.

[0008] Furthermore, in step 1, the mass ratio of the carrier to the grinding ball is 1:(50-100).

[0009] Furthermore, in step 1, the plasma voltage is 10 kV-11 kV.

[0010] Furthermore, in step 1, the time of plasma-assisted ball milling should be 2 hours to 6 hours.

[0011] Furthermore, in step 2, the mass ratio of the carrier to iridium trichloride is 1:(0.5-1.5).

[0012] Furthermore, in step three, after cooling, the mixture is washed and centrifuged alternately with water and ethanol for 3 times.

[0013] Furthermore, in step 4, the centrifuged product is dried at 60°C to 80°C.

[0014] According to another aspect of the present invention, provided is the use of the acidic water electrolysis anode oxygen evolution electrocatalytic material for performing an anode oxygen evolution reaction in an acidic environment.

[0015] According to another aspect of the present invention, provided is an anode material, comprising the above-mentioned acidic water electrolysis anode oxygen evolution electrocatalytic material, wherein the acidic water electrolysis anode oxygen evolution electrocatalytic material is drop-coated on carbon paper.

[0016] By constructing metal oxide support interaction (SOSI), the metal cations of the oxide catalyst are tightly bound to the oxide support to form a binary oxide nanostructure. At the same time, the defects on the oxide support can promote the interaction between the support and the support, enhance the binding force between them, improve the stability of the catalyst, help prevent the aggregation and stripping of the support, and extend the service life of the catalyst. SOSI can effectively control the catalytic activity and selectivity by adjusting the geometric and electronic properties of the metal. The repositioning interface of electrons on the support will adjust the electronic properties of the active site, and unique structural deformations and different atomic coordination environments will appear at the interface, thereby changing the adsorption behavior of the reaction intermediates and the energy barriers of the reaction substeps.

[0017] Based on this, the overall concept of the present invention is to modify the carrier by plasma-assisted ball milling to increase oxygen defects, and then use a hydrothermal method to load iridium dioxide on defect-rich niobium pentoxide, or defect-rich tantalum pentoxide, or defect-rich zirconium dioxide, or defect-rich titanium dioxide to form a metal oxide-carrier interaction to prepare an electrocatalyst for anode oxygen evolution in an acidic environment.

[0018] Compared with the prior art, the beneficial technical effects of the present invention are: 1. Through plasma-assisted ball milling technology, it is possible to control the synthesis of carriers with different oxygen vacancy structures (Nb 2 O 5-x , 2 O 5-x 、ZrO 2-x 、TiO 2-x ).

[0019] 2. The catalytic material prepared by the present invention has excellent anodic oxygen evolution performance in acidic water electrolysis. The defects on the carrier can promote the interaction between the support and the carrier (SOSI), enhance the binding force between them, improve the stability of the catalyst, and help prevent the aggregation and peeling of the support, thereby extending the service life of the catalyst.

[0020] 3. The present invention successfully regulated IrO 2 The electronic structure of the catalyst is stabilized by the enhanced oxide-support interaction, further improving the stability of the electrocatalyst.

[0021] 4. Specifically, IrO 2 / Nb 2 O 5-x Catalyst at 0.5 MH 2 SO 4 Reach 10mA / cm 2 and 50 mA / cm 2The current density overpotential is only 225mV and 277mV, and the durability is more than 200 hours. When used in a PEM electrolyzer, it can be used at 500 mA / cm 2 It can run stably for 200 hours at the same current density, and the Ir content is only 0.2852 mg, which proves its prospect for practical application.

[0022] 5. The preparation process of the present invention is simple, the electrode components and types are adjustable, and it has good application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 The IrO obtained in Example 1 2 / Nb 2 O 5-x Scanning electron microscope image of the catalyst.

[0024] Figure 2 The IrO obtained in Example 1 2 / Nb 2 O 5-x X-ray diffraction spectrum of the catalyst.

[0025] Figure 3 The IrO obtained in Example 1 2 / Nb 2 O 5-x Electron paramagnetic resonance spectrum of the catalyst.

[0026] Figure 4 The IrO obtained in Example 1 2 / Nb 2 O 5-x Linear voltammetric curve of catalyst oxygen evolution performance test (0.5 mol / LH 2 SO 4 Solution) diagram.

[0027] Figure 5 The IrO obtained in Example 1 2 / Nb 2 O 5-x Stability curve of the catalyst’s oxygen evolution performance test.

[0028] Figure 6 The IrO obtained in Example 1 2 / Nb 2 O 5-x Linear voltammetry curve of the catalyst in PEM electrolyzer test.

[0029] Figure 7 The IrO obtained in Example 1 2 / Nb 2 O 5-x PEM electrolyzer test stability graph of the catalyst.

[0030] Figure 8 The IrO obtained in Example 2 2 / Ta 2 O 5-x Linear voltammetric curve of the catalyst’s oxygen evolution performance test.

[0031] Fig. 9 The IrO obtained in Example 2 2 / Ta 2 O 5-x Stability curve of the catalyst’s oxygen evolution performance test.

[0032] Fig.10 IrO obtained in Example 3 2 / ZrO 2-x Linear voltammetric curve of the catalyst’s oxygen evolution performance test.

[0033] Fig.11 The IrO obtained in Example 3 2 / ZrO 2-x Stability curve of the catalyst’s oxygen evolution performance test.

[0034] Fig.12 IrO obtained in Example 4 2 / TiO 2-x Stability curve of the catalyst’s oxygen evolution performance test.

[0035] Fig.13 IrO obtained in Example 4 2 / TiO 2-x Stability curve of the catalyst’s oxygen evolution performance test.

[0036] Fig.14 IrO obtained in Example 5 2 / Nb 2 O 5-x Linear voltammetric curve of the catalyst’s oxygen evolution performance test.

[0037] Fig.15 IrO obtained in Example 6 2 / Nb 2 O 5-x Linear voltammetric curve of the catalyst’s oxygen evolution performance test.

[0038] Fig.16 The commercial IrO obtained in Comparative Example 1 2 Linear voltammetric curve of the catalyst’s oxygen evolution performance test.

[0039] Fig.17 IrO obtained in Comparative Example 2 2 / Nb 2 O5 Linear voltammetric curve of the catalyst’s oxygen evolution performance test.

[0040] Fig.18 IrO obtained in Comparative Example 2 2 / Nb 2 O 5 Stability curve of the catalyst’s oxygen evolution performance test. DETAILED DESCRIPTION

[0041] The technical scheme claimed in the present invention is further described below by some examples. However, the examples and comparative examples are used to explain the embodiments of the present invention and do not exceed the scope of the subject matter of the present invention. The protection scope of the present invention is not limited by the examples. Unless otherwise specified, the materials and reagents used in the present invention can be obtained from commercial products in the art.

[0042] Example 1 (IrO 2 / Nb 2 O 5-x ) Put 2g of niobium pentoxide and 100g of grinding balls into the ball mill, connect the vacuum pump and the vacuum air valve through a hose, evacuate the ball mill, and then fill it with oxygen. Repeat the gas washing for more than 2 times to improve the purity of the gas in the tank.

[0043] Install the ball mill on the frame of the ball mill, connect the positive line of the high-voltage power supply to the metal electrode, and connect the ground line to the bolt of the front cover. Turn on the ball mill control power supply, and the ball mill starts to vibrate. After the vibration of the ball mill stabilizes, turn on the plasma power supply to achieve plasma-assisted ball milling. The plasma voltage is 11kV, and the plasma-assisted ball milling time is 2h.

[0044] The niobium pentoxide powder after plasma-assisted ball milling was collected, 0.015 g of niobium pentoxide and 0.015 g of iridium trichloride were weighed, added into 20 ml of deionized water, and stirred for 20 minutes to obtain a mixed solution.

[0045] The mixed solution was placed in a polytetrafluoroethylene hydrothermal reactor and hydroheated at 180°C for 12 h. After cooling, it was washed alternately with water and ethanol and centrifuged three times.

[0046] The centrifugal product was dried at 80 °C to obtain iridium dioxide / niobium pentoxide (IrO 2 / Nb 2 O 5-x ) catalyst and drop-coat the catalyst on carbon paper to obtain the anode material.

[0047] The IrO prepared in Example 1 2 / Nb 2 O 5-x The scanning electron microscope image of the catalyst is shown in Figure 1As shown, Figure 1 It can be seen that the prepared IrO 2 / Nb 2 O 5-x The catalyst morphology is small particles uniformly loaded on a niobium pentoxide carrier. The carrier provides a large surface area for the loading of the metal, which can effectively improve the utilization rate of the precious metal and thus improve the electrocatalytic activity.

[0048] The IrO prepared in Example 1 2 / Nb 2 O 5-x The X-ray diffraction spectrum of the catalyst is shown in Figure 2 As shown by Figure 2 It can be seen that IrO 2 / Nb 2 O 5-x The characteristic peaks of the electrocatalyst correspond to IrO 2 and Nb 2 O 5 characteristic peaks.

[0049] The IrO prepared in Example 1 2 / Nb 2 O 5-x The electron paramagnetic resonance image of the catalyst is shown in Figure 3 As shown by Figure 3 It can be seen that IrO 2 / Nb 2 O 5-x The catalyst is rich in oxygen defects.

[0050] The IrO prepared in Example 1 2 / Nb 2 O 5-x The linear voltammetric curve of the catalyst oxygen evolution performance test is as follows Figure 4 As shown by Figure 4 It can be seen that the prepared IrO 2 / Nb 2 O 5-x The catalyst only needs 225mV to reach 10mA / cm 2 Current density.

[0051] The IrO prepared in Example 1 2 / Nb 2 O 5-x Catalyst at 10mA / cm 2 and 50mA / cm 2 The stability test curve is as follows Figure 5 As shown by Figure 5 It can be seen that the prepared IrO 2 / Nb 2 O 5-xThe catalyst can stably drive the oxygen evolution reaction in an acidic environment for a long time.

[0052] In order to determine the IrO 2 / Nb 2 O 5-x In order to demonstrate the potential for industrial applications, we used Nafion 117 membrane and IrO 2 / Nb 2 O 5-x As the anode and commercial Pt / C as the cathode, a 1*1 cm 2 A proton exchange membrane electrolysis (PEMWE) device with a catalyst mass loading of 1 mg / cm 2 The linear voltammetric curve in the PEM electrolyzer is as follows: Figure 6 As shown by Figure 6 It can be seen that IrO 2 / Nb 2 O 5-x ||Pt / C reaches 500 mA / cm 2 The required battery voltage is 1.79 V.

[0053] The IrO prepared in Example 1 2 / Nb 2 O 5-x ||Pt / C catalyst in PEM electrolyzer 500mA / cm 2 The stability test curve is as follows Figure 7 As shown by Figure 7 Remarkable stability is observed over 200 h without noticeable decay, making it a promising acidic OER electrocatalyst for practical PEMWE applications.

[0054] Example 2 (IrO 2 / Ta 2 O 5-x ) Put 2g of tantalum pentoxide and 100g of grinding balls into the ball mill, connect the vacuum pump and the vacuum air valve through a hose, evacuate the ball mill, and then fill it with oxygen. Repeat the gas washing for more than 2 times to improve the purity of the gas in the tank.

[0055] Install the ball mill on the frame of the ball mill, connect the positive line of the high-voltage power supply to the metal electrode, and connect the ground line to the bolt of the front cover. Turn on the ball mill control power supply, and the ball mill starts to vibrate. After the vibration of the ball mill stabilizes, turn on the plasma power supply to achieve plasma-assisted ball milling. The plasma voltage is 11kV, and the plasma-assisted ball milling time is 2h.

[0056] The tantalum pentoxide after plasma-assisted ball milling was collected, and 0.015 g of tantalum pentoxide and 0.015 g of iridium trichloride were weighed and added into 20 ml of deionized water, and stirred for 20 min to obtain a mixed solution.

[0057] The mixed solution was placed in a polytetrafluoroethylene hydrothermal reactor and hydroheated at 180°C for 12 h. After cooling, it was washed alternately with water and ethanol and centrifuged three times.

[0058] The centrifugal product was dried at 80 °C to obtain iridium dioxide / tantalum pentoxide (IrO 2 / Ta 2 O 5-x ) catalyst and drop-coat the catalyst on carbon paper to obtain the anode material.

[0059] The IrO prepared in Example 2 2 / Ta 2 O 5-x The linear voltammetric curve of the catalyst oxygen evolution performance test is as follows Figure 8 As shown by Figure 8 It can be seen that the prepared IrO 2 / Ta 2 O 5-x Catalyst at 10mA / cm 2 The overpotential at the current density is 245mV.

[0060] The IrO prepared in Example 2 2 / Ta 2 O 5-x Catalyst at 10mA / cm 2 The stability test curve is as follows Fig. 9 As shown by Fig. 9 It can be seen that the prepared IrO 2 / Ta 2 O 5-x Catalyst at 10mA / cm 2 The current density can be kept stable for 100h.

[0061] Example 3 (IrO 2 / ZrO 2-x ) Put 2g zirconium dioxide and 100g grinding balls into the ball mill, connect the vacuum pump and the vacuum valve through a hose, evacuate the ball mill, and then fill it with oxygen. Repeat the gas washing for more than 2 times to improve the purity of the gas in the tank.

[0062] Install the ball mill on the frame of the ball mill, connect the positive line of the high-voltage power supply to the metal electrode, and connect the ground line to the bolt of the front cover. Turn on the ball mill control power supply, and the ball mill starts to vibrate. After the vibration of the ball mill stabilizes, turn on the plasma power supply to achieve plasma-assisted ball milling. The plasma voltage is 11kV, and the plasma-assisted ball milling time is 2h.

[0063] The zirconium dioxide after plasma-assisted ball milling was collected, and 0.015 g of zirconium dioxide and 0.015 g of iridium trichloride were weighed, added into 20 ml of deionized water, and stirred for 20 min to obtain a mixed solution.

[0064] The mixed solution was placed in a polytetrafluoroethylene hydrothermal reactor and hydroheated at 180°C for 12 h. After cooling, it was washed alternately with water and ethanol and centrifuged three times.

[0065] The centrifugal product was dried at 80 °C to obtain iridium dioxide / zirconium dioxide (IrO 2 / ZrO 2-x ) catalyst and drop-coat the catalyst on carbon paper to obtain the anode material.

[0066] IrO prepared in Example 3 2 / ZrO 2-x The linear voltammetric curve of the catalyst oxygen evolution performance test is as follows Fig.10 As shown by Fig.10 It can be seen that the prepared IrO 2 / ZrO 2-x Catalyst at 10mA / cm 2 The overpotential at the current density is 248 mV.

[0067] IrO prepared in Example 3 2 / ZrO 2-x Catalyst at 10mA / cm 2 The stability test curve is as follows Fig.11 As shown by Fig.11 It can be seen that the prepared IrO 2 / ZrO 2-x Catalyst at 10mA / cm 2 The current density can be kept stable for 100h.

[0068] Example 4 (IrO 2 / TiO 2-x ) Put 2g titanium dioxide and 100g grinding balls into the ball mill, connect the vacuum pump and the vacuum air valve through a hose, evacuate the ball mill, and then fill it with oxygen. Repeat the gas washing for more than 2 times to improve the purity of the gas in the tank; Install the ball mill on the frame of the ball mill, connect the positive line of the high-voltage power supply to the metal electrode, and connect the ground line to the bolt of the front cover. Turn on the ball mill control power supply, and the ball mill starts to vibrate. After the vibration of the ball mill stabilizes, turn on the plasma power supply to achieve plasma-assisted ball milling. The plasma voltage is 11kV, and the plasma-assisted ball milling time is 2h.

[0069] The titanium dioxide after plasma-assisted ball milling was collected, and 0.015 g of titanium dioxide and 0.015 g of iridium trichloride were weighed, added into 20 ml of deionized water, and stirred for 20 min to obtain a mixed solution.

[0070] The above solution was placed in a polytetrafluoroethylene hydrothermal autoclave and hydroheated at 180°C for 12 hours. After cooling, it was washed alternately with water and ethanol and centrifuged three times.

[0071] The centrifugal product was dried at 80 °C to obtain iridium dioxide / titanium dioxide (IrO 2 / TiO 2-x ) catalyst and drop-coat the catalyst on carbon paper to obtain the anode material.

[0072] IrO prepared in Example 4 2 / TiO 2-x The linear voltammetric curve of the catalyst oxygen evolution performance test is as follows Fig.12 As shown by Fig.12 It can be seen that the prepared IrO 2 / TiO 2-x Catalyst at 10mA / cm 2 The overpotential at the current density is 241 mV.

[0073] IrO prepared in Example 4 2 / TiO 2-x Catalyst at 10mA / cm 2 The stability test curve is as follows Fig.13 As shown by Fig.13 It can be seen that the prepared IrO 2 / TiO 2-x Catalyst at 10mA / cm 2 The current density can be kept stable for 100h.

[0074] Example 5 (IrO 2 / Nb 2 O 5-x ) Put 2g of niobium pentoxide and 200g of grinding balls into the ball mill, connect the vacuum pump and the vacuum air valve through a hose, evacuate the ball mill, and then fill it with oxygen. Repeat the gas washing for more than 2 times to improve the purity of the gas in the tank.

[0075] Install and fix the ball mill on the frame of the ball mill, connect the positive line of the high-voltage power supply to the metal electrode, and connect the ground line to the bolt of the front cover. Turn on the ball mill control power supply, and the ball mill starts to vibrate. After the vibration of the ball mill stabilizes, turn on the plasma power supply to achieve plasma-assisted ball milling. The plasma voltage is 10kV, and the plasma-assisted ball milling time is 6h.

[0076] The niobium pentoxide powder after plasma-assisted ball milling was collected, 0.030 g of niobium pentoxide and 0.015 g of iridium trichloride were weighed, added into 20 ml of deionized water, and stirred for 20 minutes to obtain a mixed solution.

[0077] The mixed solution was placed in a polytetrafluoroethylene hydrothermal reactor and hydroheated at 200°C for 18 h. After cooling, it was washed alternately with water and ethanol and centrifuged three times.

[0078] The centrifugal product was dried at 60 °C to obtain iridium dioxide / niobium pentoxide (IrO 2 / Nb 2 O 5-x ) catalyst and drop-coat the catalyst on carbon paper to obtain the anode material.

[0079] IrO prepared in Example 5 2 / Nb 2 O 5-x The linear voltammetric curve of the catalyst oxygen evolution performance test is as follows Fig.14 As shown by Fig.14 It can be seen that the prepared IrO 2 / Nb 2 O 5-x Catalyst at 10mA / cm 2 The overpotential at the current density is 250 mV.

[0080] Example 6 (IrO 2 / Nb 2 O 5-x ) Put 2g of niobium pentoxide and 150g of grinding balls into the ball mill, connect the vacuum pump and the vacuum valve through a hose, evacuate the ball mill, and then fill it with oxygen. Repeat the gas washing for more than 2 times to improve the purity of the gas in the tank.

[0081] Install and fix the ball mill on the frame of the ball mill, connect the positive line of the high-voltage power supply to the metal electrode, and connect the ground line to the bolt of the front cover. Turn on the ball mill control power supply, and the ball mill starts to vibrate. After the vibration of the ball mill stabilizes, turn on the plasma power supply to achieve plasma-assisted ball milling. The plasma voltage is 11kV, and the plasma-assisted ball milling time is 4h.

[0082] The niobium pentoxide powder after plasma-assisted ball milling was collected, 0.010 g of niobium pentoxide and 0.015 g of iridium trichloride were weighed, added into 20 ml of deionized water, and stirred for 20 minutes to obtain a mixed solution.

[0083] The mixed solution was placed in a polytetrafluoroethylene hydrothermal reactor and hydroheated at 190°C for 24 hours. After cooling, it was washed alternately with water and ethanol and centrifuged three times.

[0084] The centrifugal product was dried at 70 °C to obtain iridium dioxide / niobium pentoxide (IrO 2 / Nb 2 O 5-x ) catalyst and drop-coat the catalyst on carbon paper to obtain the anode material.

[0085] The IrO prepared in Example 6 2 / Nb 2 O 5-x The linear voltammetric curve of the catalyst oxygen evolution performance test is as follows Fig.15 As shown by Fig.15 It can be seen that the prepared IrO 2 / Nb 2 O 5-x Catalyst at 10mA / cm 2 The overpotential at the current density is 229mV.

[0086] Comparative Example 1 (Commercial IrO 2 catalyst) Weigh 0.005 g of commercial iridium dioxide, add 150 μL of ethanol, 100 μL of water and 11 μL of Nafion, and ultrasonicate for 40 min. Then drop the solution on carbon paper to obtain the anode material.

[0087] Commercial IrO provided in Comparative Example 1 2 The linear voltammetric curve of the catalyst oxygen evolution performance test is as follows Fig.16 As shown by Fig.16 It can be seen that the prepared IrO 2 Catalyst at 10mA / cm 2 The overpotential at the current density is 399 mV, indicating that commercial IrO 2 The catalyst performance is far inferior to that of the catalysts prepared by plasma-assisted ball milling.

[0088] Comparative Example 2 (IrO 2 / Nb 2 O 5 catalyst) 0.015 g of unmodified niobium pentoxide and 0.015 g of iridium trichloride were weighed, added into 20 ml of deionized water, and stirred for 20 minutes to obtain a mixed solution.

[0089] The mixed solution was placed in a polytetrafluoroethylene hydrothermal reactor and hydroheated at 180°C for 12 h. After cooling, it was washed alternately with water and ethanol and centrifuged three times.

[0090] The centrifugal product was dried at 80 °C to obtain iridium dioxide / niobium pentoxide (IrO 2 / Nb 2 O 5 ) catalyst and drop-coat the catalyst on carbon paper to obtain the anode material.

[0091] IrO prepared in Comparative Example 2 2 / Nb 2 O 5 The linear voltammetric curve of the catalyst oxygen evolution performance test is as follows Fig.17 As shown by Fig.17 It can be seen that the prepared IrO 2 / Nb 2 O 5 Catalyst at 10mA / cm 2 The overpotential at the current density is 259 mV.

[0092] IrO prepared in Comparative Example 2 2 / Nb 2 O 5 Catalyst at 10mA / cm 2 The stability test curve is as follows Fig.18 As shown by Fig.18 It can be seen that the prepared IrO 2 / Nb 2 O 5 Catalyst at 10mA / cm 2 The current density can only remain stable for 15h.

[0093] The above experiments prove that the presence of oxygen vacancies in the support enhances the interaction between the support and the loaded material, forming a strong metal oxide support interaction (SOSI), thereby improving the stability of the catalyst. The SOSI effect induces charge transfer from Nb 2 O 5-x Transfer to IrO 2 , thus inhibiting the formation of Ir peroxides. In addition, the use of IrO in PEM electrolyzers 2 / Nb 2 O 5-x As the anode, it exhibits excellent overall water electrolysis activity and stability at an ultra-low Ir loading of 0.2852 mg.

Claims

1. An acidic water electrolysis anode oxygen evolution electrocatalytic material, characterized in that: The invention comprises a carrier and iridium dioxide loaded on the carrier, wherein the carrier is selected from Nb2O5, Ta2O5, ZrO2 or TiO2, and the carrier has oxygen-rich defects after being modified by plasma-assisted ball milling.

2. The method for preparing the electrocatalytic material for oxygen evolution at the anode of acidic water electrolysis according to claim 1, characterized in that: include: Step 1, placing the carrier and the grinding balls into a ball milling jar, and modifying the carrier by plasma-assisted ball milling; Step 2, weighing iridium trichloride and the modified carrier, and adding water to form a mixed solution; Step 3, hydrothermally reacting the mixed solution at 180°C-200°C for 12 hours-24 hours, washing and centrifuging after cooling; Step 4: After centrifugation and drying, the catalytic material is obtained.

3. The method according to claim 2, characterized in that: In step 1, the mass ratio of the carrier to the grinding ball is 1:(50-100).

4. The method according to claim 2 or 2, characterized in that: In step 1, the plasma voltage is 10 kV-11 kV.

5. The method according to claim 4, characterized in that: In step 1, the plasma-assisted ball milling time should be 2 hours to 6 hours.

6. The method according to claim 2 or 5, characterized in that: In step 2, the mass ratio of the carrier to iridium trichloride is 1:(0.5-1.5).

7. The method according to claim 6, characterized in that: In step 3, after cooling, the mixture is washed alternately with water and ethanol and centrifuged three times.

8. The method according to claim 7, characterized in that: In step 4, the centrifuged product is dried at 60°C to 80°C.

9. Use of the acidic water electrolysis anode oxygen evolution electrocatalytic material according to claim 1 for performing an anode oxygen evolution reaction in an acidic environment.

10. An anode material, characterized in that: The method comprises the acidic water electrolysis anode oxygen evolution electrocatalytic material as claimed in claim 1, wherein the acidic water electrolysis anode oxygen evolution electrocatalytic material is drop-coated on carbon paper.

Citation Information

Patent Citations

  • Preparation method of Sm-Fe-N permanent magnet powder

    CN108777204A

  • Oxygen evolution catalyst with low noble metal loading amount for water electrolysis unit

    CN109589974A

  • Method for preparing metal nano oxide by plasma enhanced mechanochemistry and application of metal nano oxide

    CN111453756A

  • Method for preparing electro-catalytic material through ion implantation and related application

    CN113976121A

  • PEM electrolyzed water catalyst as well as preparation method and application thereof

    CN114561662A