Precious metal-based integrated self-supporting electrode limited by metal carbide and preparation method of precious metal-based integrated self-supporting electrode
By using precious metal-based integrated self-support electrodes with metal carbide domains in hydrogen energy preparation, the stability and energy consumption problems of the catalyst in acidic environment are solved, and efficient and stable hydrogen hydrogen evolution reaction is achieved, suitable for large-scale Industrialized production.
Patent Information
- Application Number
- CN202410996377.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-11-12
AI Technical Summary
In the prior art, hydrogen energy preparation cost is high, and ruthenium catalysts are easily dissolved and oxidized in an acidic environment, resulting in low catalyst activity and stability, and large energy consumption in the preparation process, uneven materials, and unsatisfactory mass transfer efficiency.
The precious metal-based integrated self-supporting electrode with a metal carbide domain is used to enhance the hydrophilicity of the carbon-based substrate by concentrated nitric acid treatment. The tungsten-based polyoxygenate with Keggin structure is used as a support, and the noble metal Ru salt is mixed to perform Electrojoule thermal pulse reaction prepares nanoparticle catalysts to improve catalytic activity and stability.
It improves hydrogen evolution activity and charge transfer rate, reduces the risk of dissolution and shedding of catalysts under high current density, and achieves efficient and stable electrocatalytic performance, which is suitable for large-scale industrial production.
Smart Images

Figure CN118932395A_ABST
Abstract
Description
Technical field:
[0001] The present invention belongs to the field of electrocatalytic material applications, and in particular relates to a noble metal-based integrated self-supporting electrode confined by metal carbides and a preparation method thereof. Background technology:
[0002] Hydrogen energy has the advantages of wide sources, high combustion calorific value, clean and pollution-free, and good safety, and is widely used in the field of energy storage. Proton exchange membrane water electrolysis hydrogen production technology is an important application outlet for hydrogen energy, but the source and cost of hydrogen energy restrict its application and progress. PEM acidic proton exchange membrane water electrolysis hydrogen production technology is currently in the commercial application stage because of its advantages such as high current density, high voltage efficiency, low electrolyte resistance, good safety, and good adaptability to fluctuating renewable energy. It has greater advantages than alkaline water electrolyzers. However, the PEM electrolyte is an acidic environment with a pH of 0-3, and the current density is high. The electrode materials are mainly noble metal PGM-based catalysts, which greatly increases the cost of hydrogen production by water electrolysis. Ruthenium, as a widely used noble metal, has Pt-like hydrogen evolution activity, and its cost is one-tenth of Pt. Research on low-load ruthenium-based hydrogen evolution catalysts can effectively reduce the hydrogen production cost of PEM fuel cells. However, under harsh acidic and strong oxidizing potential conditions, ruthenium is easily dissolved and oxidized into high-valent species, which is the main difficulty in the current research stage.
[0003] Transition metal carbides have Pt-like electronic structures, high electrical conductivity, and are resistant to acid and alkali corrosion. They are ideal materials for hydrogen evolution electrocatalysts. Many theoretical and practical application results have been reported on the application of metal carbides in acidic HER. The metal carbides studied include single metal carbides (WC, Mo2C, etc.), but the HER activity of single metal carbides needs to be improved. Since the binding energy between transition metals and H bonds is too strong, it is not conducive to the desorption of hydrogen, thereby reducing its activity. Further activity regulation can effectively improve the catalytic activity. For example, doping, introducing other heterogeneous atoms into the transition metal carbide lattice, can change the electronic structure of the main catalyst, and further optimize the adsorption and desorption behavior of intermediates in the hydrogen evolution reaction of the catalyst to improve the catalytic activity. In addition, in order to improve the conductivity, carbon materials can be introduced. Carbon materials have porous properties and large specific surface area, which can effectively disperse the active components in the catalyst, avoid the reduction of activity caused by agglomeration, and expose more active sites, as well as accelerate the charge transfer and mass transfer of bubbles during the reaction.
[0004] The document with application number "202311134833.2" discloses "a tungsten carbide material, preparation method and application thereof". The invention mixes dopamine hydrochloride, ruthenium salt and tungsten salt to generate a precipitate, then centrifuges to obtain a precipitate, then dries the precipitate, grinds it into powder and anneals it in an argon environment for 10 hours in a tubular furnace to obtain a carbon carrier-loaded Ru-WC powder. The problems with this invention are: 1. The preparation process is complicated, and the tubular furnace annealing technology is used in the preparation process, and its calcination technology consumes a lot of energy; 2. The catalyst needs to be added with a conductive agent and a polymer binder (such as Nafion, etc.) to form a slurry, and then made into an electrode. In this process, some active sites of the catalyst will be covered, making the mass transfer efficiency and charge transfer rate of the catalyst less than ideal; 3. The material grown on the carbon carrier by this technology is uneven, resulting in reduced catalyst activity; 4. The catalyst falls off at high current density, which reduces the activity and stability of the catalyst. Summary of the invention:
[0005] The present invention provides a metal carbide confined noble metal-based integrated self-supporting electrode and a preparation method thereof, so as to overcome the problems existing in the prior art.
[0006] In order to achieve the purpose of the present invention, the technical solution provided by the present invention is a metal carbide confined noble metal-based integrated self-supporting electrode and a preparation method thereof, comprising the following steps:
[0007] The first step is to immerse the pretreated carbon-based substrate material in a polyethyleneimine solution and treat it at 60-70°C for 1-2 hours, take out the carbon-based substrate material, rinse it with deionized water, and dry it;
[0008] Step 2: weigh polyoxometalate and noble metal salt hydrate, mix them in ethanol solution and stir evenly to obtain a uniformly dispersed precursor solution; take a certain amount of the precursor solution and evenly drop it on the surface of the carbon-based substrate and immerse it for 30 to 40 minutes; put the carbon-based substrate into a vacuum oven and dry it for 6 to 8 hours;
[0009] The third step is to subject the dried carbon-based substrate to Joule heat treatment in an inert atmosphere, and perform 10 pulse reactions at 1400-1800°C, with each pulse lasting 0.1-0.5s, to obtain a carbide-confined precious metal-based nanocatalytic electrode supported on a carbon-based substrate.
[0010] Preferably, the pretreatment in step 1 is as follows: immersing the carbon-based substrate material in a hydrothermal reactor filled with 65% concentrated nitric acid, sealing it at 80-100°C, keeping it warm for 12-15 hours, taking out the carbon cloth after cooling, ultrasonically treating it with anhydrous ethanol and deionized water, and then vacuum drying it to obtain a pretreated carbon-based substrate.
[0011] Preferably, the carbon-based substrate is selected from one or more carbon-based substrates such as carbon cloth, carbon paper, and carbon felt.
[0012] Preferably, in the suspension of step 2, the concentration of polyoxometalate is 0.05-0.2 g / ml, and the concentration of noble metal is 0.015-0.035 g / ml.
[0013] Preferably, the polyoxometalate in step 2 is selected from one or more of phosphotungstic acid, silicotungstic acid and ammonium tungstate.
[0014] Preferably, the noble metal salt hydrate in step 2 is selected from one or more of ruthenium chloride hydrate, iridium chloride hydrate and palladium chloride hydrate.
[0015] Preferably, the inert atmosphere in the above step 3 is one of a vacuum environment, argon or helium.
[0016] Preferably, in the above step three, the Joule heat heating voltage is 40-70V, and the current is 50-100A.
[0017] The above preparation method obtains a metal carbide-confined noble metal-based integrated self-supporting electrode.
[0018] Compared with the prior art, the present invention has the following beneficial effects:
[0019] 1. The present invention heat-treats the carbon cloth with concentrated nitric acid, and can produce abundant defects on the surface of the carbon cloth by acid etching the surface of the carbon cloth, thereby enhancing the hydrophilicity of the carbon cloth, uniformly growing nanoparticles, fully exposing active sites, and accelerating the stripping of bubbles to increase mass transfer efficiency and accelerate the charge transfer rate, thereby facilitating the improvement of HER activity. In addition, the treated carbon cloth can more firmly anchor the nanoparticles, which can effectively prevent the catalyst from dissolving and falling off at high current density, thereby enhancing the activity and stability of the catalyst at high current density.
[0020] 2. The present invention uses tungsten-based polyoxometalate with Keggin structure as a carrier, introduces noble metal Ru salt for mixing, and can prepare W x The metal Ru loaded on C nanoparticles can change the particle size of the synthesized catalyst by controlling the concentration of noble metal salts and polyoxometalates. The resulting metal carbide and noble metal ruthenium can improve the adsorption strength of the intermediate H* through electronic interaction, regulate the HER reaction path, reduce the dissociation energy barrier of the intermediate H*, and promote the rapid mass transfer of hydrogen, thereby improving the HER hydrogen evolution activity.
[0021] 3. The present invention rapidly synthesizes Ru-doped W by one-step reaction using electric Joule heat xThe method is a hydrogen evolution electrocatalyst composed of C nanoparticles. Compared with the traditional technology, this method has fast reaction time and cooling rate, low energy consumption, uniform material dispersion and high stability, and can accurately control the electric Joule heat reaction time to change the organizational structure and size of the nanoparticles. The lower the reaction time, the smaller the particle size of the catalyst, and the size of the nanoparticles is only 20 to 50nm.
[0022] 4. The loading amount of precious metal in the material of the present invention is controlled at 1 mg / cm 2 The utilization rate of precious metals is high. At low loading of precious metals, the catalyst still has excellent HER activity and can work efficiently at high current density. -2 At a current density of only 31 mV, the overpotential is only 1 A cm -2 Only 288 mV overpotential was generated at high current density, and at 10 and 500 mA cm -2 and 1A cm -2 Therefore, the preparation method of the present invention is suitable for large-scale industrial production of HER catalytic electrodes for water electrolysis, which can meet the actual working conditions of PEMWE electrolyzers with ampere-level current density, corrosion resistance and long life, and is widely used in electrolyzers and fuel cell applications. Description of the drawings:
[0023] Figure 1 The XRD patterns of Example 1, Example 2, Example 3, Example 4, Example 5 and Example 6 are shown in FIG.
[0024] Figure 2 The SEM images of Example 1, Example 2, Example 3, Example 4, Example 5, and Example 6 are shown;
[0025] Figure 3 LSV diagrams of Example 1, Example 2, Example 3, Example 4, Example 5, and Example 6 in 0.5 mH2SO4;
[0026] Figure 4 The XRD patterns of Example 1, Example 7, Example 8 and Example 9 are shown in FIG.
[0027] Figure 5 The SEM images of Example 1, Example 7, Example 8 and Example 9 are shown;
[0028] Figure 6 LSV diagrams of Example 1, Example 7, Example 8, and Example 9 in 0.5 mH2SO4;
[0029] Figure 7 1 is the SEM image of Example 1, Example 10 and Example 11;
[0030] Figure 8 2 are LSV diagrams of Example 1, Example 10 and Example 11 in 0.5 mH2SO4.
[0031] Fig. 9 1 is the SEM image of Example 1, Example 12 and Example 13;
[0032] Fig.10 LSV diagrams of Example 1, Example 12 and Example 13 in 0.5 mH2SO4;
[0033] Fig.11 1 is the XRD pattern of Example 1, Example 14, Example 15 and raw carbon cloth;
[0034] Fig.12 The SEM images of Example 1, Example 14, Example 15 and the EDS image of Example 1;
[0035] Fig.13 TEM image of Example 1;
[0036] Fig.14 LSV diagrams of Example 1, Example 14 and Example 15 in 0.5 mH2SO4;
[0037] Fig.15 For Example 1 at (a) 10 mA / cm 2 (b) 500mA / cm 2 and (c) 1A / cm 2 Constant current chronopotentiometry CP test diagram under current density;
[0038] Fig.16 Comparison of XRD test patterns before and after HER in Example 1;
[0039] Fig.17 (a) C 1s, (b) O 1s, (c) W 4f, and (d) Ru 3d fine spectra of Example 1;
[0040] Fig.18 (a) Ru 3d fine spectrum comparison of Example 1 and Comparative Example 1, and (b) W 4f fine spectrum comparison of Comparative Example 2;
[0041] Fig.19 Comparison of (a) Ru 3d fine spectrum and (b) W 4f fine spectrum before and after HER in Example 1; Specific implementation method:
[0042] The present invention will be described in detail below with reference to the accompanying drawings and embodiments.
[0043] Embodiment 1, a method for preparing a noble metal-based integrated self-supporting electrode confined by metal carbides, comprising the following steps:
[0044] The first step is to immerse a 1*2.5cm rectangular carbon cloth in a hydrothermal reactor filled with 65% concentrated nitric acid, seal it and keep it at 90°C for 12h, take out the carbon cloth after cooling, ultrasonically treat it with anhydrous ethanol and deionized water, and then vacuum dry it to obtain a pretreated carbon cloth. The pretreated carbon cloth is immersed in a polyethyleneimine solution (4mg / ml) and treated at 60°C for 1h, then the carbon cloth is taken out and rinsed with deionized water and dried.
[0045] The second step is to weigh 0.2 g of phosphotungstic acid and 0.056 g of ruthenium chloride hydrate, mix them in 2 ml of ethanol, take 100 μL of the precursor solution and evenly drop it on the surface of the carbon cloth, immerse it for 30 minutes, and then vacuum dry it for 6 hours.
[0046] The third step is to conduct Joule heating of the dried carbon cloth in a vacuum environment, with a voltage of 65V, a current of 90A, and pulse heating at 1600°C for 10 times, a cycle of 6s, and a pulse heating time of 0.1s each time. After the Joule heating is completed, the carbon-based substrate-supported carbide-confined noble metal-based nanocatalytic electrode Ru-W can be obtained. x C / CC.
[0047] Example 2, a method for preparing a metal carbide confined precious metal-based integrated self-supporting electrode, is the same as Example 1, except for the second step: weigh 0.2g of phosphotungstic acid and 0.03g of ruthenium chloride hydrate, mix them in 2ml of ethanol, take 100μL of the precursor solution and evenly drop it on the surface of the carbon cloth, and then vacuum dry it for 6h.
[0048] Example 3, a method for preparing a metal carbide confined precious metal-based integrated self-supporting electrode, is the same as Example 1, except for the second step: weigh 0.2g of phosphotungstic acid and 0.04g of ruthenium chloride hydrate, mix them in 2ml of ethanol, take 100μL of the precursor solution and evenly drop it on the surface of the carbon cloth, and then vacuum dry it for 6h.
[0049] Example 4, a method for preparing a metal carbide confined precious metal-based integrated self-supporting electrode, is the same as Example 1, except for the second step: weigh 0.2 g of phosphotungstic acid and 0.05 g of ruthenium chloride hydrate, mix them in 2 ml of ethanol, take 100 μL of the precursor solution and evenly drop it on the surface of the carbon cloth, and then vacuum dry it for 6 hours.
[0050] Example 5, a method for preparing a metal carbide confined precious metal-based integrated self-supporting electrode, is the same as Example 1, except for the second step: weigh 0.2g of phosphotungstic acid and 0.06g of ruthenium chloride hydrate, mix them in 2ml of ethanol, take 100μL of the precursor solution and evenly drop it on the surface of the carbon cloth, and then vacuum dry it for 6h.
[0051] Example 6, a method for preparing a metal carbide confined precious metal-based integrated self-supporting electrode, is the same as Example 1, except for the second step: weigh 0.2g of phosphotungstic acid and 0.07g of ruthenium chloride hydrate, mix them in 2ml of ethanol, take 100μL of the precursor solution and evenly drop it on the surface of the carbon cloth, and then vacuum dry it for 6h.
[0052] See also Figure 1 The XRD of the above six embodiments shows the changes in the XRD peaks after changing the concentration of Ru. It is found that the positions of all peaks do not change after changing the concentration, indicating that the crystal structure has not changed, but the peak intensity changes, indicating that the particle size of the material has changed.
[0053] See also Figure 2 The SEM images of the above six examples and Example 1 show that the Ru loading is 0.56 mg / cm 2 The material is dispersed more evenly and the particle size is smaller.
[0054] See also Figure 3 The LSV diagrams of the above six examples in 0.5 mH2SO4 show that the Ru loading is 0.56 mg / cm 2 The lowest overpotential for hydrogen evolution is produced.
[0055] Example 7, a method for preparing a metal carbide confined precious metal-based integrated self-supporting electrode, is the same as Example 1, except for the second step: weigh 0.1g of phosphotungstic acid and 0.056g of ruthenium chloride hydrate, mix them in 2ml of ethanol, take 100μL of the precursor solution and evenly drop it on the surface of the carbon cloth, and then vacuum dry it for 6h.
[0056] Example 8, a method for preparing a metal carbide confined precious metal-based integrated self-supporting electrode, is the same as Example 1, except for the second step: weigh 0.3 g of phosphotungstic acid and 0.056 g of ruthenium chloride hydrate, mix them in 2 ml of ethanol, take 100 μL of the precursor solution and evenly drop it on the surface of the carbon cloth, and then vacuum dry it for 6 hours.
[0057] Example 9, a method for preparing a metal carbide confined precious metal-based integrated self-supporting electrode, is the same as Example 1, except for the second step: weigh 0.4 g of phosphotungstic acid and 0.056 g of ruthenium chloride hydrate, mix them in 2 ml of ethanol, take 100 μL of the precursor solution and evenly drop it on the surface of the carbon cloth, and then vacuum dry it for 6 hours.
[0058] See also Figure 4 The XRD of the above three examples and Example 1 shows the changes of XRD peaks after changing the concentration of HPW. It is found that the positions of all peaks do not change after changing the concentration, indicating that the crystal structure does not change, but the peak intensity changes significantly. After increasing the content of HPW, W x The peak intensity of C increases significantly.
[0059] See also Figure 5 The SEM images of the above three examples and Example 1 show that when the HPW loading is 4 mg / cm 2 When the material is dispersed more evenly, the W on the surface of the carbon cloth increases with the increase of HPW. x The C content increased significantly, which is consistent with the XRD analysis results.
[0060] See also Figure 6 The LSV diagrams of the above three examples and Example 1 in 0.5 mH2SO4 show that the loading amount of HPW is 4 mg / cm 2 The best hydrogen evolution reaction activity is obtained at low current density, while 6 mg / cm 2 It has the best hydrogen evolution reaction activity at high current density.
[0061] Example 10, a method for preparing a noble metal-based integrated self-supporting electrode confined by metal carbides, is the same as Example 1, except that the third step is to perform electric Joule heat treatment in a vacuum environment, wherein the voltage is 70V, the current is 100A, and the pulse heating is performed 10 times at 1800°C, the cycle is 6s, and the pulse heating time for each time is 0.1s.
[0062] Example 11, a method for preparing a noble metal-based integrated self-supporting electrode confined by metal carbides, is the same as Example 1, except that the third step is to perform electric Joule heat treatment in a vacuum environment, wherein the voltage is 55V, the current is 80A, and the pulse heating is performed 10 times at 1400°C, the cycle is 6s, and the pulse heating time for each time is 0.1s.
[0063] See also Figure 7 The SEM images of the above embodiments and embodiment 1 show that the morphological characteristics of the materials change after changing the Joule heat temperature. It is found that the materials are more evenly dispersed at 1600°C.
[0064] See also Figure 8The LSV diagrams of the above two examples and Example 1 in 0.5 mH2SO4 show that they have the best hydrogen evolution activity at 1600°C.
[0065] Example 12, a method for preparing a noble metal-based integrated self-supporting electrode confined by metal carbides, is the same as Example 1, except that the third step is to perform electric Joule heat treatment in a vacuum environment, wherein the voltage is 55V, the current is 80A, and the pulse heating is performed 10 times at 1400°C, the cycle is 6s, and the pulse heating time for each time is 0.5s.
[0066] Example 13, a method for preparing a noble metal-based integrated self-supporting electrode confined by metal carbides, is the same as Example 1, except that the third step is to perform electric Joule heat treatment in a vacuum environment, wherein the voltage is 55V, the current is 80A, and the pulse heating is performed 10 times at 1400°C, the cycle is 6s, and the pulse heating time for each time is 0.3s.
[0067] See also Fig. 9 The SEM of the above-mentioned embodiment and embodiment 1 shows that the morphological characteristics of the materials change after changing the different Joule heating times. It is found that the shorter the Joule heating time, the smaller the particle size, and the morphology does not change.
[0068] See also Fig.10 The LSV diagrams of the above examples and Example 1 in 0.5 mH2SO4 show that they have the best hydrogen evolution reaction activity at 0.1 s.
[0069] Example 14, a method for preparing a metal carbide confined precious metal-based integrated self-supporting electrode, is the same as Example 1, except for the second step: weigh 0.056g of ruthenium chloride hydrate, mix it in 2ml of ethanol, take 100μL of the precursor solution and evenly drop it on the surface of the carbon cloth, and then vacuum dry it for 6h.
[0070] Example 15, a method for preparing a metal carbide confined precious metal-based integrated self-supporting electrode, is the same as Example 1, except for the second step: weigh 0.2 g of phosphotungstic acid, mix it in 2 ml of ethanol, take 100 μL of the precursor solution and evenly drop it on the surface of the carbon cloth, and then vacuum dry it for 6 hours.
[0071] See also Fig.11 , XRD spectrum shows that Ru-W xThe C / CC material includes three strong peaks of WC and W2C, indicating that dual-phase tungsten carbide nanoparticles are generated in the material. The corresponding three strong peaks are (011), (100), (101) and (100), (002), (101). There is a weak Ru diffraction peak in the XRD spectrum, indicating that the Ru content is low and the Ru particle size is small. After adding Ru, the diffraction peak of tungsten carbide is slightly offset, indicating that Ru is successfully doped inside the tungsten carbide lattice. W x After Ru is doped into the C system, W x The diffraction peak intensity of WC and W2C in C is significantly reduced. At the same time, compared with Ru / CC, the diffraction peak intensity of Ru is also greatly reduced, indicating that after the interaction between Ru and WC, the particle size is reduced and the dispersion on the carbon cloth is better.
[0072] See also Fig.12 , SEM images show that Ru-W x The C / CC material presents a nano-island surface morphology on the carbon cloth surface, and the particle size is between 20 and 50 nm. Both SEM and EDS images show that the material and elements are evenly distributed on the carbon cloth surface, and the Ru element is evenly confined inside the tungsten carbide lattice.
[0073] See also Fig.13 , TEM images show that Ru-W x The Ru lattice appears in the C / CC material, and Ru is confined to W. x C inside.
[0074] See also Fig.14 , LSV diagram shows that Ru-W x C / CC materials at 10mAcm -2 、1Acm -2 The overpotentials at the catalytic current density are 31mV and 288mV respectively. x The overpotential of C / CC (218mV, 504mV) is much lower.
[0075] See also Fig.15 , Ru-W x C / CC at 10mA / cm 2 , 500mA / cm 2 and 1A / cm 2 The current density can be stably operated for more than 100 hours. After the electrolyte is updated, the voltage will decrease and the catalyst will become more stable.
[0076] See also Fig.16 , Ru-W x Comparison of the XRD test patterns before and after C / CCHER shows that after 100 hours of HER testing, the XRD peak position has basically not changed, indicating that the catalyst has good stability.
[0077] See also Fig.17 , Fig.18 and Fig.19 , Ru-W x The Ru 3d nuclear electron energy spectrum of C / CC shows that after adding HPW to the precursor, the binding energy of the high-valent Ru species gradually moves to the lower binding energy direction, indicating that the valence of Ru decreases, and the binding energy of the low-valent Ru increases slightly, and the valence of Ru is between 0 and +4. The 4f nuclear electron energy spectrum of W shows that Ru-W x C / CC exists W 6+ and W 2 + , W 6+ The existence of W 4+ The oxidation of W is caused by Ru doping. After Ru doping, the binding energy of W with a valence of +6 moves to a low binding energy, indicating that the valence state of W in a high valence state decreases, and Ru doping inhibits the oxidation of W. The binding energy of W with a valence of +2 in a low valence state moves to a high binding energy, indicating that W in a low valence state loses electrons and transfers electrons to Ru species; therefore, there is a charge transfer between Ru and W, and the valence state of W is slightly increased to prevent the oxidation of Ru species. There is a strong electronic interaction between W and Ru. After the HER test, Ru is slightly oxidized, and the valence state of Ru gradually increases, all changing to a high valence state of +4. The valence state of W decreases, W gradually decreases from +6, the low valence state of W disappears, and the valence state of W is between +2 and +6.
[0078] Table 1 is a comparison of HER performance of all embodiments and comparative examples:
[0079] <![CDATA[HPW / mg / cm 2 ]]> Ru:HPW η10 / mV η1000 / mV Tafel / mV / dec Example 1 4 3.6:1 31 288 46.64 Example 2 4 6.67:1 69 390 58.51 Example 3 4 5:1 53 378 55.19 Example 4 4 4:1 38 370 56.93 Example 5 4 3.3:1 44 353 51.83 Example 6 4 2.8:1 44 350 53.23 Example 7 2 1.8:1 41 300 51.66 Example 8 6 5.4:1 35 264 44.59 Example 9 8 7.2:1 39 330 45.49 Example 10 4 3.6:1 45 338 58.05 Embodiment 11 4 3.6:1 33 - 44.28 Example 12 4 3.6:1 101 - 72.17 Example 13 4 3.6:1 95 - 62.18 Embodiment 14 - - 67 - 146.89 Embodiment 15 4 - 218 504 80.5
[0080] In summary, Example 1 of the present invention is the best embodiment. The obtained self-supporting integrated electrode has a high specific surface area and a porous structure, increases the active sites, the Ru sites supported by tungsten carbide are evenly dispersed, and the synergistic effect of metal elements greatly increases the activity and stability of the catalyst, can achieve stable hydrogen evolution in ampere-level acidic water electrolysis, and has a low amount of precious metals, which can be commercially applied.
[0081] The above are only specific embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a noble metal-based integrated self-supporting electrode confined by metal carbides, characterized in that: The following steps are involved: The first step is to immerse the pretreated carbon-based substrate material in a polyethyleneimine solution and treat it at 60-70°C for 1-2 hours, take out the carbon-based substrate material, rinse it with deionized water, and dry it; Step 2: weigh polyoxometalate and noble metal salt hydrate, mix them in ethanol solution and stir evenly to obtain a uniformly dispersed precursor solution; take a certain amount of the precursor solution and evenly drop it on the surface of the carbon-based substrate and immerse it for 30 to 40 minutes; put the carbon-based substrate into a vacuum oven and dry it for 6 to 8 hours; The third step is to subject the dried carbon-based substrate to Joule heat treatment in an inert atmosphere, and perform 10 pulse reactions at 1400-1800°C, with each pulse lasting 0.1-0.5s, to obtain a carbide-confined precious metal-based nanocatalytic electrode supported on a carbon-based substrate.
2. The method for preparing a metal carbide confined noble metal-based integrated self-supporting electrode according to claim 1, characterized in that: The pretreatment of step 1 is to immerse the carbon-based substrate material in a hydrothermal reactor filled with 65% concentrated nitric acid, seal it and keep it at 80-100° C. for 12-15 hours, take out the carbon cloth after cooling, ultrasonically treat it with anhydrous ethanol and deionized water, and then vacuum dry it to obtain a pretreated carbon-based substrate.
3. The method for preparing a metal carbide confined noble metal-based integrated self-supporting electrode according to claim 1, characterized in that: The carbon-based substrate is selected from one or more carbon-based substrates such as carbon cloth, carbon paper, and carbon felt.
4. The method for preparing a metal carbide confined noble metal-based integrated self-supporting electrode according to claim 1, characterized in that: In the suspension of step 2, the concentration of polyoxometalate is 0.05-0.2 g / ml, and the concentration of noble metal is 0.015-0.035 g / ml.
5. The method for preparing a metal carbide confined noble metal-based integrated self-supporting electrode according to claim 1, characterized in that: The polyoxometalate in step 2 is selected from one or more of phosphotungstic acid, silicotungstic acid and ammonium tungstate.
6. The method for preparing a metal carbide confined noble metal-based integrated self-supporting electrode according to claim 1, characterized in that: The noble metal salt hydrate in step 2 is selected from one or more of ruthenium chloride hydrate, iridium chloride hydrate and palladium chloride hydrate.
7. The method for preparing a metal carbide confined noble metal-based integrated self-supporting electrode according to claim 1, characterized in that: The inert atmosphere in step three is one of vacuum environment, argon or helium.
8. The method for preparing a metal carbide confined noble metal-based integrated self-supporting electrode according to claim 1, characterized in that: In the step three, the Joule heat heating voltage is 40 to 70 V, and the current is 50 to 100 A.
9. A metal carbide-confined noble metal-based integrated self-supporting electrode obtained by the preparation method according to claim 1.