Organic semiconductor / reduced graphene oxide composite film, preparation method and application

Organic semiconductor/reduced graphene oxide films were prepared by combining pyrrolopyrrole dione or perylene diimide derivatives with graphene oxide, which solved the problems of low efficiency and poor selectivity of existing CO2 reduction technologies. This enabled efficient and low-cost CO2 reduction to methanol, avoiding metal pollution and promoting the use of clean energy.

CN118932408APending Publication Date: 2024-11-12SOUTHWEAT UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411227293.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-03
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Existing CO2 reduction technologies are inefficient and have poor selectivity, and suffer from metal pollution. Photocatalysts are difficult to recycle and reuse, electrocatalysis has high energy consumption, and metal-based and inorganic semiconductor catalysts are expensive, making it difficult to control product selectivity.

Method used

Organic semiconductor/reduced graphene oxide composite films were prepared by combining pyrrolopyrrole dione or perylene diimide derivatives with graphene oxide. The films formed a layered structure through π-π stacking and were used for photoelectrocatalytic CO2 reduction. The films were prepared by combining electrodeposition technology.

Benefits of technology

It improves CO2 reduction efficiency and selectivity, reduces catalyst costs, avoids metal contamination, and produces liquid methanol that is easy to separate and store, thereby reducing energy consumption and promoting the use of clean energy.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118932408A_ABST
    Figure CN118932408A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of renewable energy utilization and carbon circulation, and particularly relates to an organic semiconductor / reduced graphene oxide composite material film, a preparation method and application. A preparation method of an organic semiconductor / reduced graphene oxide composite film comprises the following steps: S1, dissolving graphene oxide in a solvent to obtain a graphene oxide solution, adjusting the pH value, respectively adding an organic semiconductor and zinc powder into the graphene oxide solution, mixing to obtain a mixed solution, carrying out ultrasonic treatment, removing unreacted zinc powder, washing and filtering to obtain a graphene oxide solution; performing vacuum freeze drying on the filter cake to obtain an organic semiconductor / reduced graphene oxide composite material; and S2, adding the organic semiconductor / reduced graphene oxide composite material obtained in the S1 and I2 into acetone, performing ultrasonic cleaning to obtain an electro-deposition solution, cleaning and drying conductive glass, putting the conductive glass into the electro-deposition solution, and performing deposition to obtain the organic semiconductor / reduced graphene oxide composite material film.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of renewable energy utilization and carbon cycle, and specifically relates to an organic semiconductor / reduced graphene oxide composite film, a preparation method and application thereof. Background Art

[0002] Greenhouse gas CO2 comes from fossil fuels such as coal, oil and natural gas. If it is not controlled, it will endanger human survival and development in the future. Therefore, eliminating greenhouse gas CO2 and realizing energy utilization are two major problems that people urgently need to solve. One of the solutions is to use clean solar energy and its derived electricity to convert CO2 into energy fuel, thereby realizing clean energy utilization and carbon cycle.

[0003] Carbon dioxide reduction (CO2RR) technology can convert CO2 into usable chemical fuels such as CO, HCOOH, CH4, and methanol. At present, CO2RR technologies using clean energy can be divided into two categories: photocatalysis and electrocatalysis. Although photocatalytic reduction of CO2 technology is energy-saving, its efficiency and selectivity are poor, and most photocatalysts are powder materials, which limits the recycling of catalysts; although electrocatalytic reduction of CO2 technology is efficient, it requires excessively high voltages, consumes too much energy, and is mainly based on metal-based and non-electrode semiconductors, with poor selectivity. Photoelectrocatalytic technology can not only use light energy to reduce energy loss, but also improve the separation and transmission efficiency of photogenerated carriers in semiconductors by applying a certain bias voltage; especially in organic semiconductors, re-excitation of the reduced or oxidized state can be achieved to achieve the ultra-low reduction or oxidation potential required for CO2RR. Therefore, the use of thin-film photoelectrocatalytic technology to reduce carbon dioxide is of great significance to the energy utilization and market development of greenhouse gas CO2.

[0004] Methanol, as one of the liquid products of carbon dioxide reduction, is easier to separate, store and transport than gaseous products. The newly developed methanol fuel engine is already in the trial operation stage, and has huge market potential in the future. In addition, methanol is also a basic organic chemical raw material, which is widely used in industries such as pesticides, leather, dyes, medicines and rubber, and has huge market demand.

[0005] Pyrrolopyrrole dione and perylene diimide derivatives have good chemical inertness, corrosion resistance and photostability, and are widely used in fluorescent probes, organic semiconductors, organic electroluminescence, molecular self-assembly, catalysis and other fields. The present invention uses pyrrolopyrrole dione or perylene diimide derivatives and graphene to perform π-π stacking to prepare a composite film with a layered structure, promote electron transfer, and improve the photoelectric catalytic performance of the composite material. There are currently no relevant literature reports on the composite preparation method of pyrrolopyrrole dione derivatives and perylene diimide derivatives with redox graphene, and for CO2 reduction. In addition, the CO2 reduction technology that has been reported in the patent uses metal-based or inorganic semiconductor catalysts, which has high cost and energy consumption, and the product selectivity is difficult to control, and it will bring subsequent metal pollution. Therefore, the technology of CO2 catalytic reduction to produce methanol based on organic semiconductor composite film has great academic, practical and market value, so there is an urgent need for an organic semiconductor / reduced graphene oxide composite film, preparation method and application. Summary of the invention

[0006] In view of the problems and shortcomings of the prior art, the present invention provides a method for preparing an organic semiconductor / reduced graphene oxide composite film, comprising the following steps:

[0007] S1: dissolving graphene oxide in a solvent to obtain a graphene oxide solution, adjusting the pH, adding an organic semiconductor and zinc powder to the graphene oxide solution to obtain a mixed solution, performing ultrasound to remove unreacted zinc powder, washing and filtering to obtain a filter cake, and performing vacuum freeze drying to obtain an organic semiconductor / reduced graphene oxide composite material;

[0008] S2: The organic semiconductor / reduced graphene oxide composite material obtained in S1 and I2 are added to acetone, and an electrodeposition solution is obtained after ultrasonic cleaning. The conductive glass is cleaned and dried, and placed in the electrodeposition solution to obtain an organic semiconductor / reduced graphene oxide composite material film by deposition.

[0009] Furthermore, the mass ratio of the graphene oxide, the organic semiconductor and the zinc powder described in S1 is 2:1 to 3:4.

[0010] Furthermore, the organic semiconductor described in S1 is any one of a diketopyrrolopyrrole derivative and a perylene diimide derivative.

[0011] Furthermore, the pH described in S1 is 2, the ultrasonic time is 1 min, and the vacuum freeze-drying time is 48 h.

[0012] Furthermore, the mass ratio of I2 to the organic semiconductor / reduced graphene oxide composite material described in S2 is 1-3:2-5.

[0013] Furthermore, the ultrasonic cleaning time described in S2 is 30 minutes, the drying time is 2 hours, and the drying temperature is 50°C.

[0014] Furthermore, in the electrodeposition process in S2, the electrodeposition time is 10 to 25 s and the constant voltage is 30V.

[0015] An organic semiconductor / reduced graphene oxide composite film, wherein the bottom layer of the organic semiconductor / reduced graphene oxide composite film is reduced graphene oxide, the surface of the reduced graphene oxide has a two-dimensional sheet structure with nano-scale wrinkles, and PDPP nanosheets are evenly distributed on the reduced graphene oxide layer.

[0016] An application of an organic semiconductor / reduced graphene oxide composite film, wherein the organic semiconductor / reduced graphene oxide composite film is applied in preparing an electrode for photoelectrocatalytic reduction of CO2.

[0017] Technical Effects

[0018] (1) The organic semiconductor / reduced graphene oxide composite film provided by the present invention can utilize electrical energy and light energy simultaneously, and the photoelectric synergistic catalysis improves the separation and transmission of carriers, thereby improving the CO2RR catalytic performance (efficiency and selectivity), and the stability under catalytic conditions is >24h, which is much better than other organic materials.

[0019] (2) The present invention provides a method for preparing an organic semiconductor / reduced graphene oxide composite film. The method adopts an organic semiconductor as a catalytic material and can greatly reduce the catalyst cost and avoid metal pollution compared with metal-based and inorganic semiconductor catalysts. The film-forming method has a fast film-forming rate, a dense and complete film structure, good adhesion to the substrate, strong controllability of the film-forming area and the film thickness, and is simple and easy to operate. The method is low in cost and easy to mass produce, and the thin film catalyst is easy to recover.

[0020] (3) Through the application of the method for preparing an organic semiconductor / reduced graphene oxide composite film provided by the present invention, by using the organic semiconductor / reduced graphene oxide composite film as an electrode for photoelectrocatalytic reduction of CO2, the product methanol is the only liquid product, and the separation cost is greatly reduced compared with the mixed product; and the product methanol is a liquid product, without gaseous reduction products, which is easier to store and transport than gaseous products such as CO and CH4, and can be easily extracted from the reaction liquid; while the gaseous products will be mixed with CO2 and the by-product H2, making separation more difficult; and the CO2 catalytic reduction technology, which uses sunlight and its derived electricity, can reduce fossil energy consumption, promote the use of clean energy, and avoid environmental pollution; and compared with thermal catalytic technology, it has better product and process controllability. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] In order to more clearly illustrate the technical solutions of the exemplary embodiments of the present invention, the following is a brief introduction to the drawings required for use in the embodiments. It should be understood that the following drawings only illustrate certain embodiments of the present invention and should not be regarded as limiting the scope. For ordinary technicians in this field, other relevant drawings can be obtained based on these drawings without creative work.

[0022] Figure 1 is the molecular structure formula of the organic semiconductor PDPP in Example 1 of the present invention;

[0023] Figure 2 This is a transmission electron microscope image of the organic semiconductor rGO composite material in Example 1 of the present invention;

[0024] Figure 3 Scanning electron microscope image of the thin film sample in Example 1 of the present invention;

[0025] Figure 4 This is an optical image of the organic semiconductor composite thin film in Example 1 of the present invention;

[0026] Figure 5 This is a diagram showing changes in the organic semiconductor film during the catalytic reaction process in Example 1 of the present invention;

[0027] Figure 6 The LSV curve of the composite material and the precursor film in Example 1 of the present invention in a CO2 solution;

[0028] Figure 7 This is a graph showing the chopping photoelectric response characteristics of the composite material and the precursor film in Example 1 of the present invention;

[0029] Figure 8 Stability diagram of the composite material and precursor film catalyzed CO2 reduction reaction in Example 1 of the present invention;

[0030] Fig. 9 The liquid product methanol of the CO2 reduction reaction catalyzed by the composite film in Example 1 of the present invention 1 H-NMR spectrum. DETAILED DESCRIPTION

[0031] The following will be combined with the embodiments 1-2 and the attached Figures 1 to 9 , the technical solution of the present invention is clearly and completely described. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0032] Example 1

[0033] S1: First, ultrasonically treat 100 mg of graphene oxide (GO) in 100 mL of ultrapure water for 2 hours to make it evenly dispersed; use 12 mol / L HCL to adjust the solution pH to 2 to obtain a solution; then quickly place 50 mg of pyrrolopyrrole diketo derivative PDPP and 200 mg of zinc powder into the solution at the same time and immediately ultrasonicate for 1 minute. After the ultrasonication, add 5 mL of 12 mol / L HCL to remove excess zinc powder. Wash with a large amount of deionized water through a suction filtration device, and after washing, vacuum freeze-dry the obtained filter cake for 48 hours. After drying, an organic semiconductor PDPP / reduced graphene oxide (rGO) composite material is obtained;

[0034] S2: 10 mg I2 and 20 mg organic semiconductor / reduced graphene oxide (rGO) composite material were added to 40 mL acetone and treated with ultrasound at room temperature for 2 hours to prepare the electrodeposition solution; the conductive glass (FTO) was ultrasonically cleaned in ethanol for 30 minutes and dried at 50°C for 2 hours for use; a two-electrode system was adopted, with FTO serving as both the working electrode and the counter electrode; the FTO was placed in the electrodeposition solution, and an organic semiconductor / reduced graphene oxide (rGO) composite film was deposited on the FTO at a constant voltage of 30 V for 10 seconds.

[0035] from Figure 1 It can be known that the molecular formula of PDPP is Figure 2 It can be seen that the two-dimensional rGO sheet structure with nanoscale wrinkles can be clearly observed from TEM, and the PDPP nanosheets are evenly distributed on the rGO layer. The two form a tight two-dimensional interface bond through π-π stacking and van der Waals force. Figure 3 It can be seen that the scanning electron microscope image of the film sample clearly shows the two-dimensional plane of rGO, the surface of the film is smooth and flat, and the PDPP nanosheets and rGO sheets are uniformly formed into a composite material without phase separation and aggregation structure. Figure 4 The optical image of the prepared film can be seen.

[0036] The film prepared in Example 1 was dried at 50°C for 6 h, and then an organic semiconductor / reduced graphene oxide (rGO) composite film electrode was used as a working electrode, a platinum mesh was used as a counter electrode, and Ag / AgCl was used as a reference electrode. An H-type electrolytic cell N117 type proton exchange membrane was used to separate the anode and cathode, and 0.3M KHCO3 was used as an electrolyte solution to form a three-electrode system. The reaction was carried out at a constant potential of -0.50 V (vs Ag / AgCl) for 2 h. Figure 5 As shown, the optical images of the working electrode before and during the catalytic reaction can be seen.

[0037] CO2 gas was continuously introduced into the electrolyte, and a xenon lamp was used as the light source at 100 mW / cm 2 The working electrode is irradiated with visible light. Figure 6 A comparison of the linear voltammetric curves of organic semiconductor / reduced graphene oxide (rGO) composite film electrodes in a CO2 atmosphere is shown. It can be concluded from the figure that the photocathode current of the composite film increases in a CO2 atmosphere. Figure 7 It shows that under the same bias voltage applied to the photocathode, the photocurrent density of the composite material is significantly improved, and the catalytic stability is greater than 2h.

[0038] from Figure 8 It can be seen that the composite material and the precursor film catalyze the CO2 reduction reaction stably, and the gas phase products detected by gas chromatography do not contain any gas phase products such as CO, CH4, H2, etc. The liquid products in the solution after the reaction were quantitatively analyzed by the internal standard method of nuclear magnetic resonance hydrogen spectrum, and only methanol ( Fig. 9 ), and the concentration of methanol is 0.16mmol / L.

[0039] Example 2

[0040] S1: 80 mg of graphene oxide (GO) was ultrasonically treated in 100 mL of ultrapure water for 2 h to make it evenly dispersed. 12 mol / L HCL was used to adjust the solution pH to 2; 30 mg of perylene diimide derivative PDCD and 100 mg of zinc powder were quickly placed in the solution at the same time and ultrasonicated for 1 min immediately; after the ultrasonication, 5 mL of 12 mol / L HCL was added to remove the excess zinc powder; and then washed with a large amount of deionized water through a suction filtration device, and after washing, the obtained filter cake was vacuum freeze-dried for 36 h, and after drying, an organic semiconductor PDCD / reduced graphene oxide (rGO) composite material was obtained;

[0041] S2: 15mg I2 and 25mg organic semiconductor / reduced graphene oxide (rGO) composite material were added to 20mL acetone and treated with ultrasound at room temperature for 2 hours as the electrodeposition solution; the conductive glass (FTO) was ultrasonically cleaned in ethanol for 30min and dried at 80℃ for 2h for standby use. In the dual-electrode system, FTO was used as both the working electrode and the counter electrode; FTO was placed in the electrodeposition solution, and the organic semiconductor / reduced graphene oxide (rGO) composite material was deposited on FTO under a constant voltage of 50V for 25s.

[0042] The film obtained in Example 2 was dried at 50°C for 6 h, CO2 gas was continuously introduced into the electrolyte, and a xenon lamp was used as the light source at 100 mW / cm 2The working electrode was illuminated by visible light. The organic semiconductor PDCD / reduced graphene oxide (rGO) composite film electrode was used as the working electrode, the platinum mesh was used as the counter electrode, and the Ag / AgCl was used as the reference electrode. The H-type electrolytic cell N117 type proton exchange membrane was used to connect the anode and cathode, and 0.4MKHCO3 was used as the electrolyte solution to form a three-electrode system, which was reacted at a constant potential of -0.60V (vs Ag / AgCl) for 2h.

[0043] The gas phase products were detected by gas chromatography, and no gas phase products such as CO, CH4, H2, etc. The liquid products in the solution after the reaction were quantitatively analyzed by the internal standard method of nuclear magnetic resonance hydrogen spectrum, and only methanol was detected, and the concentration of methanol was 1.4mmol / L.

[0044] The organic semiconductor / reduced graphene oxide composite film provided by the present invention has a two-dimensional rGO sheet structure with nanometer-level wrinkles, and PDPP nanosheets are evenly distributed on the rGO layer. The two form a tight two-dimensional interface bond through π-π stacking and van der Waals force. The film surface is smooth and flat, and the PDPP nanosheets and rGO sheets are evenly formed into a film in the form of a composite material without phase separation and aggregation structure. In addition, as a working electrode, it can simultaneously utilize electrical energy and light energy, and photoelectric synergistic catalysis improves the separation and transmission of carriers, thereby improving the CO2RR catalytic performance. In addition, the film has good stability under catalytic conditions, which is much better than other organic materials.

[0045] The present invention provides a method for preparing an organic semiconductor / reduced graphene oxide composite film. The method adopts an organic semiconductor as a catalytic material. Compared with metal-based and inorganic semiconductor catalysts in the prior art, the method has the advantages of low cost, is greener, and avoids metal pollution. The film-forming method in the preparation method has a fast film-forming rate, a dense and complete structure, and good adhesion to the substrate. The film-forming area is large, the film thickness is highly controllable, and the method is simple and easy to operate. Due to the low cost, the method is easy to mass produce, and the thin film catalyst is also easy to recycle.

[0046] Through the application of the preparation method of an organic semiconductor / reduced graphene oxide composite film provided by the present invention, the organic semiconductor / reduced graphene oxide composite film is used as an electrode to photoelectrocatalytically reduce CO2, methanol is the only liquid product in the product, and the separation cost is greatly reduced compared with the mixed product; and there is no gaseous reduction product, which is easier to store and transport, and is easy to extract from the reaction liquid. In the process of CO2 catalytic reduction, sunlight and its derived electric energy are used to reduce fossil energy consumption, promote the use of clean energy, and avoid environmental pollution; and compared with thermal catalytic technology, it has better product and process controllability.

Claims

1. A method for preparing an organic semiconductor / reduced graphene oxide composite film, characterized in that: The following steps are involved: S1: dissolving graphene oxide in a solvent to obtain a graphene oxide solution, adjusting the pH, adding an organic semiconductor and zinc powder to the graphene oxide solution to obtain a mixed solution, performing ultrasound to remove unreacted zinc powder, washing and filtering to obtain a filter cake, and performing vacuum freeze drying to obtain an organic semiconductor / reduced graphene oxide composite material; S2: The organic semiconductor / reduced graphene oxide composite material obtained in S1 and I2 are added to acetone, and an electrodeposition solution is obtained after ultrasonic cleaning. The conductive glass is cleaned and dried, and placed in the electrodeposition solution to obtain an organic semiconductor / reduced graphene oxide composite material film by deposition.

2. The method for preparing an organic semiconductor / reduced graphene oxide composite film according to claim 1, characterized in that: The mass ratio of graphene oxide, organic semiconductor and zinc powder described in S1 is 2:1 to 3:

4.

3. The method for preparing an organic semiconductor / reduced graphene oxide composite film according to claim 1, characterized in that: The organic semiconductor described in S1 is any one of a diketopyrrolopyrrole derivative and a perylene diimide derivative.

4. The method for preparing an organic semiconductor / reduced graphene oxide composite film according to claim 1, characterized in that: The pH described in S1 was 2, the ultrasonic time was 1 min, and the vacuum freeze-drying time was 48 h.

5. According to the method for preparing an organic semiconductor / reduced graphene oxide composite film according to claim 1, the mass ratio of I2 to the organic semiconductor / reduced graphene oxide composite material in S2 is 1-3:2-5.

6. The method for preparing an organic semiconductor / reduced graphene oxide composite film according to claim 1, characterized in that: The ultrasonic cleaning time described in S2 is 30 minutes, the drying time is 2 hours, and the drying temperature is 50°C.

7. The method for preparing an organic semiconductor / reduced graphene oxide composite film according to claim 1, characterized in that: During the electrodeposition process in S2, the electrodeposition time is 10 to 25 s and the constant voltage is 30V.

8. An organic semiconductor / reduced graphene oxide composite film obtained by the preparation method according to any one of claims 1 to 7, characterized in that: The bottom layer of the organic semiconductor / reduced graphene oxide composite film is reduced graphene oxide, the surface of the reduced graphene oxide has a two-dimensional sheet structure with nano-scale wrinkles, and PDPP nanosheets are evenly distributed on the reduced graphene oxide layer.

9. The use of an organic semiconductor / reduced graphene oxide composite film according to claim 8, characterized in that: The organic semiconductor / reduced graphene oxide composite film is used in preparing electrodes for photoelectrocatalytic reduction of CO2.