Production device and method of sound-absorbing material
Through the combination of dispersing tanks, high-speed dispersing tanks and molding and drying integrated device, the dimensional stability and resilience problems in the production of sound absorbing materials are solved, the production efficiency and drying uniformity are improved, and the efficient preparation of sound absorbing materials is achieved.
Patent Information
- Application Number
- CN202411030306.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-11-12
AI Technical Summary
The existing sound-absorbing material production technology is difficult to efficiently prepare sound-absorbing materials with stable size and high resilience, and separation of molding and drying processes leads to low production efficiency.
Using a production device including a removable tank, a high-speed dispersion tank and a molding and drying integrated device, the removable fiber slurry is dispersed at high speed through a centrifugal pump, and heated and pneumatically controlled in the molding and drying integrated device to realize the forming of materials. and dry.
The stability and high rebound rate of material size are achieved, the production process is simplified, the production efficiency is improved, and the drying is more uniform and efficient.
Smart Images

Figure CN118932775A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a device and method for producing a sound-absorbing material, belonging to the technical field of light industry. Background Art
[0002] Noise pollution is considered to be a type of physical environmental pollution that has a great impact on people's daily lives. It not only affects people's physical health, but also affects their quality of life. Nowadays, noise pollution mainly comes from transportation, and cars are an important means of transportation for people in their daily lives.
[0003] At present, sound-absorbing cotton boards are usually made of polyester fiber, acrylic fiber, glass fiber and other materials. These materials have the characteristics of light weight, softness, heat preservation, heat insulation, water resistance, fire resistance, UV resistance, etc., and also have good sound absorption effect.
[0004] With the development of society, people have attached other functions to sound-absorbing cotton besides sound insulation, such as light weight and high resilience. The light weight makes it more convenient during installation and use. Compared with traditional heavy sound insulation materials, this material can greatly reduce installation and maintenance costs; the high resilience makes it have a shock-absorbing effect when subjected to external impact, and can quickly restore its shape, thereby effectively absorbing and dispersing the impact force, protecting internal equipment and personnel from harm. Summary of the invention
[0005] The technical problem to be solved by the present invention is to provide a production device and a production method for a sound absorbing material.
[0006] In order to solve the above problems, the present invention provides a production device for sound-absorbing materials, which includes a deflaking tank for deflaking slurry, the discharge port of the deflaking tank is connected to a high-speed dispersion tank for fiber dispersion through a centrifugal pump; the discharge port of the high-speed dispersion tank is connected to a plurality of integrated molding and drying devices for slurry molding and drying through a centrifugal pump.
[0007] Preferably, the integrated molding and drying device includes an inner cavity with an upper end plate inserted at the top, a heating rod passes through the upper end plate and is arranged in the inner cavity, and holes for inserting the heating rod are evenly distributed on the upper end plate; an electric heating probe for detecting temperature is also provided in the inner cavity, and both sides of the upper end plate are connected to a pneumatic element that can move up and down.
[0008] Preferably, the number of the heating rods is 20 to 40, and the length is 3 to 8 mm.
[0009] Preferably, the surface of the heating rod is coated with Teflon for preventing fiber adhesion.
[0010] Preferably, the control pressure of the pneumatic element is not greater than 0.4 MPa; and the adjustment height of the inner cavity is not higher than 100 mm.
[0011] Preferably, the integrated molding and drying device is externally provided with a scale for controlling the slurry molding height.
[0012] The present invention also provides a method for producing a sound-absorbing material: placing fiber slurry into a deflaking tank for deflaking, the deflaked fiber slurry enters a high-speed dispersion tank through a centrifugal pump, and then an adhesive, a waterproofing agent, and an oil-proofing agent are respectively added for high-speed dispersion to form a porous slurry; the porous slurry enters a molding and drying integrated device through a centrifugal pump for molding and drying to obtain the sound-absorbing material.
[0013] Preferably, the fiber pulp is any one or more of coniferous wood pulp, broadleaf wood pulp, and grass pulp plant fiber pulp.
[0014] Preferably, the dispersion time is 0.5h to 2h, the frequency is 2000 to 20000 rpm; the molding drying temperature is not higher than 150°C, the time is 0.5h to 2h, and the molding height is not higher than 100mm; the pneumatic component control pressure is not greater than 0.4MPa.
[0015] Compared with the prior art, the present invention has the following beneficial effects:
[0016] 1. The sound-absorbing material is prepared by using an integrated molding and drying device. The material has good dimensional stability, and the molding temperature and pressure are adjustable and controllable, and products of different heights can be prepared.
[0017] 2. The integrated molding and drying device has both molding and drying functions, which saves the time for materials to enter the drying equipment after molding, and can greatly improve the production capacity of sound-absorbing materials;
[0018] 3. The integrated forming and drying device evenly arranges several heating rods in the inner cavity of the device. The even arrangement allows the material to be dried evenly and the material is dried inside, which improves the drying efficiency. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 A schematic diagram of the structure of a production device for the sound-absorbing material provided by the present invention;
[0020] Figure 2 It is a schematic diagram of the integrated molding and drying device;
[0021] Figure 3 The present invention provides a process flow chart of the method for producing the sound-absorbing material. DETAILED DESCRIPTION
[0022] In order to make the present invention more clearly understood, preferred embodiments are described in detail below with reference to the accompanying drawings.
[0023] like Figure 1As shown, it is a schematic diagram of the structure of the production device of the sound-absorbing material provided by the present invention, which includes a decomposition tank 1 for decomposing the slurry, and the discharge port of the decomposition tank 1 is connected to a high-speed dispersion tank 2 for fiber dispersion through a centrifugal pump; the discharge port of the high-speed dispersion tank 2 is connected to a plurality of integrated molding and drying devices 3 for slurry molding and drying through a centrifugal pump.
[0024] like Figure 2 As shown, the molding and drying integrated device includes an inner cavity 3-4 with an upper end plate 3-2 inserted at the top, a heating rod 3-3 passing through the upper end plate 3-2 and arranged in the inner cavity 3-4, and the upper end plate 3-2 is evenly distributed with holes for inserting the heating rod 3-3; the inner cavity 3-4 is also provided with an electric heating probe 3-1 for detecting temperature, and the two sides of the upper end plate 3-2 are connected with a pneumatic element 3-5 that can move up and down; the pneumatic element 3-5 is a prior art, and all commercially available products are applicable. The number of the heating rods 3-3 is 20 to 40, and the length is 3 to 8 mm. The surface of the heating rod 3-3 is coated with Teflon for preventing fiber adhesion. The bottom of the inner cavity 3-4 is provided with a bottom support, and the bottom support is provided with a hole for taking out the sample. The molding and drying integrated device is provided with a scale for controlling the slurry molding height. The control pressure of the pneumatic element 3-5 is not greater than 0.4MPa; the adjustment height of the inner cavity 3-4 is not higher than 100mm.
[0025] The present invention provides a method for producing a sound-absorbing material, using the above-mentioned production device, and the specific steps are:
[0026] The fiber slurry A is placed in the deflaking tank 1 for deflaking. The deflaked fiber slurry A enters the high-speed dispersion tank 2 through a centrifugal pump, and then an adhesive B, a waterproofing agent C, and an oil-proofing agent D are respectively added for high-speed dispersion to form a porous slurry. The porous slurry enters the molding and drying integrated device 3 through a centrifugal pump for molding and drying to obtain the sound-absorbing material E.
[0027] The fiber pulp is any one or more of coniferous wood pulp, broadleaf wood pulp, and grass pulp plant fiber pulp.
[0028] The dispersion time is 0.5h to 2h, the frequency is 2000 to 20000 rpm; the molding drying temperature is not higher than 150°C, the time is 0.5h to 2h, and the molding height is not higher than 100mm; the pneumatic component control pressure is not greater than 0.4MPa.
[0029] Example 1
[0030] A method for producing a sound-absorbing material, comprising the following specific steps:
[0031] Fiber pulp (bleached kraft softwood pulp) with a mass fraction of 3% is put into the decompression tank for decompression for 30 minutes. The decompressed pulp enters the high-speed dispersion tank through a centrifugal pump, and 0.5% of the mass of the pulp is added with adhesive, 0.1% of the waterproof agent, and 0.1% of the oil repellent agent. High-speed dispersion is performed for 30 minutes to form a porous pulp. The porous pulp enters a molding and drying integrated device through a centrifugal pump for molding and drying. The molding and drying integrated device sets the molding temperature to 150°C, the molding time to 2h, the molding height to 50mm, and the pneumatic component controls the pressure to 0.4MPa, thereby obtaining a sound-absorbing material. Under the static pressure of 2kg, the material can rebound to 35mm, and the rebound rate can reach 70%.
[0032] Example 2
[0033] A method for producing a sound-absorbing material, comprising the following specific steps:
[0034] The fiber pulp (bleached kraft softwood pulp) with a mass fraction of 3% is put into the decomposition tank for decomposition for 30 minutes. The decomposition pulp enters the high-speed dispersion tank through a centrifugal pump, and 0.5% of the mass of the pulp adhesive, 0.1% of the waterproof agent, and 0.1% of the oil repellent are added, and high-speed dispersion is carried out for 30 minutes to form a porous pulp. The porous pulp enters a forming and drying mold through a centrifugal pump for forming and drying. The forming and drying integrated device sets the forming temperature to 150°C, the forming time to 2h, the forming height to 50mm, and the pneumatic component controls the pressure to 0.2MPa, thereby obtaining a sound-absorbing material. Under the static pressure of 2kg, the material can rebound to 40mm, and the rebound rate can reach 80%.
[0035] Example 3
[0036] A method for producing a sound-absorbing material, comprising the following specific steps:
[0037] The fiber pulp (bleached kraft softwood pulp) with a mass fraction of 3% is put into the decomposition tank for decomposition for 30 minutes. The decomposition pulp enters the high-speed dispersion tank through a centrifugal pump, and 0.5% of the mass of the pulp is added with adhesive, 0.1% of the waterproof agent, and 0.1% of the oil repellent agent. High-speed dispersion is carried out for 30 minutes to form a porous pulp. The porous pulp enters a forming and drying mold through a centrifugal pump for forming and drying. The forming and drying integrated device sets the forming temperature to 150°C, the forming time to 2h, the forming height to 100mm, and the pneumatic component controls the pressure to 0.2MPa, thereby obtaining a sound-absorbing material. Under the static pressure of 2kg, the material can rebound to 80mm, and the rebound rate can reach 80%.
[0038] Example 4
[0039] A method for producing a sound-absorbing material, comprising the following specific steps:
[0040] The fiber pulp (bleached kraft softwood pulp) with a mass fraction of 4% is put into the decomposition tank for decomposition for 30 minutes. The decomposition pulp enters the high-speed dispersion tank through a centrifugal pump, and 0.5% of the mass of the pulp is added with adhesive, 0.1% of the waterproof agent, and 0.1% of the oil repellent agent. It is dispersed at high speed for 30 minutes to form a porous pulp. The porous pulp enters a forming and drying mold through a centrifugal pump for forming and drying. The forming and drying integrated device sets the forming temperature to 150°C, the forming time to 2h, the forming height to 100mm, and the pneumatic component controls the pressure to 0.2MPa, thereby obtaining a sound-absorbing material. Under the static pressure of 2kg, the material can rebound to 75mm, and the rebound rate can reach 75%.
Claims
1. A device for producing sound-absorbing material, characterized in that: The invention comprises a decomposition tank (1) for decomposing pulp, wherein the discharge port of the decomposition tank (1) is connected to a high-speed dispersion tank (2) for fiber dispersion via a centrifugal pump; and the discharge port of the high-speed dispersion tank (2) is connected to a plurality of integrated forming and drying devices (3) for pulp forming and drying via a centrifugal pump.
2. The device for producing sound-absorbing material according to claim 1, characterized in that: The integrated molding and drying device comprises an inner cavity (3-4) with an upper end plate (3-2) inserted at the top, a heating rod (3-3) passing through the upper end plate (3-2) and arranged in the inner cavity (3-4), and holes for inserting the heating rod (3-3) are evenly distributed on the upper end plate (3-2); an electric heating probe (3-1) for detecting temperature is also arranged in the inner cavity (3-4), and both sides of the upper end plate (3-2) are connected to a pneumatic element (3-5) that can move up and down.
3. The device for producing a sound-absorbing material according to claim 1, characterized in that: The number of the heating rods (3-3) is 20 to 40, and the length is 3 to 8 mm.
4. The device for producing a sound-absorbing material according to claim 1, characterized in that: The surface of the heating rod (3-3) is coated with Teflon for preventing fibers from sticking.
5. The device for producing a sound-absorbing material according to claim 1, characterized in that: The control pressure of the pneumatic element (3-5) is not greater than 0.4 MPa; and the adjustment height of the inner cavity (3-4) is not higher than 100 mm.
6. The device for producing a sound absorbing material according to claim 1, characterized in that: A bottom support is provided at the bottom of the inner cavity (3-4), and a hole for taking out the sample is provided on the bottom support.
7. The device for producing a sound absorbing material according to claim 1, characterized in that: The molding and drying integrated device is provided with a scale for controlling the slurry molding height.
8. A method for producing a sound-absorbing material, characterized in that: The production device of the sound-absorbing material according to any one of claims 1 to 7 is used to put the fiber slurry into a deflaking tank for deflaking, the deflaked fiber slurry enters a high-speed dispersion tank through a centrifugal pump, and then an adhesive, a waterproofing agent, and an oil-proofing agent are respectively added for high-speed dispersion to form a porous slurry; the porous slurry enters a molding and drying integrated device through a centrifugal pump for molding and drying, and the sound-absorbing material is obtained.
9. The method for producing a sound absorbing material according to claim 8, characterized in that: The fiber pulp is any one or more of coniferous wood pulp, broadleaf wood pulp, and grass pulp plant fiber pulp.
10. The method for producing a sound absorbing material according to claim 8, characterized in that: The dispersion time is 0.5h to 2h, the frequency is 2000 to 20000 rpm; the molding drying temperature is not higher than 150°C, the time is 0.5h to 2h, and the molding height is not higher than 100mm; the pneumatic component control pressure is not greater than 0.4MPa.
Citation Information
Patent Citations
A sound-absorbing paper material and its manufacturing method
CN102277788A
High strength filter paper and preparation method thereof
CN107304534A
Preparation method of halogen-free sound absorption anti-flaming paper
CN110318286A
Soft soil foundation treatment device
CN113605363A
Movable feed cylinder desicator
CN207825268U