High-air-permeability bending-resistant carbon fiber paper as well as preparation method and application thereof

By combining wet molding and impregnation with alcohol-soluble resin solution with carbonization treatment, high air permeability and bending resistance carbon fiber paper is prepared, which solves the problems of low toughness and low porosity of carbon paper. It is suitable for gas diffusion layers of fuel cells and improves the performance of fuel cells.

CN118932783AActive Publication Date: 2024-11-12SOUTH CHINA UNIV OF TECH
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202310513305.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-09
Publication Date
2024-11-12
Estimated Expiration
2043-05-09

AI Technical Summary

Technical Problem

Existing carbon paper is insufficient in terms of toughness and durability, is prone to breakage, and has low porosity, which affects the performance of fuel cells.

Method used

Highly breathable and resistant to bending carbon fiber paper is prepared by using a wet molding process combined with impregnation and carbonization of alcohol-soluble resin solution. The durability and breathability are improved by forming good connections between the carbon fibers.

Benefits of technology

The prepared carbon fiber paper has high air permeability and can withstand multiple 90° bends without breaking. It is suitable for the gas diffusion layer of fuel cells and improves the water-gas transmission performance of fuel cells.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004218094570000041
    Figure BDA0004218094570000041
  • Figure BDA0004218094570000051
    Figure BDA0004218094570000051
  • Figure HDA0004218094580000011
    Figure HDA0004218094580000011
Patent Text Reader

Abstract

The invention belongs to the technical field of fuel cell gas diffusion layers, and particularly discloses high-air-permeability bending-resistant carbon fiber paper and a preparation method and application thereof.The preparation method comprises the following steps that 1, carbon fibers, binding fibers and a dispersing agent are subjected to a wet forming process to obtain carbon fiber base paper; (2) dissolving alcohol-soluble resin in ethanol to prepare a stable ethanol-resin solution, then pouring the ethanol-resin solution into water, and uniformly stirring to obtain a suspension; (3) soaking carbon fiber raw paper in the suspension, taking out the carbon fiber raw paper, and performing pre-curing treatment to obtain gummed paper; and (4) carrying out carbonization treatment on the impregnated paper in a protective atmosphere to obtain the high-air-permeability bending-resistant carbon fiber paper. The tensile modulus of the carbon fiber paper can reach 2000 MPa, the air permeability is about 3250 mm / s, the conductivity is about 40 s / cm, the carbon fiber paper can resist 90-degree direct bending for tens of times, and the carbon fiber paper has good durability and high air permeability; and the method is simple in process and low in cost.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of fuel cell gas diffusion layers, and in particular to a method for preparing high-porosity and bending-resistant carbon paper. Background Art

[0002] Fuel cells are not affected by the Carnot cycle and are an important direction for the development of new energy. Among them, carbon paper, as an important component of the gas diffusion layer, participates in water vapor management and current transmission, so it has high requirements for the air permeability, conductivity and durability of carbon paper. The current industrial production of carbon paper has a low degree of domestic independence, and is obviously insufficient in toughness and durability. In the known literature, carbon paper is mainly prepared by the process of wet molding-resin impregnation-hot pressing curing-high temperature carbonization. After high-temperature carbonization, the resin bonds the carbon fiber into a whole in the form of resin carbon. However, resin carbon exhibits greater brittleness, which makes carbon paper prone to direct fracture when subjected to external force. And after hot pressing carbonization, the resin is distributed in the carbon paper network structure in the form of flakes, which seriously reduces the porosity of the carbon paper.

[0003] Invention patent CN108914681A discloses a method for preparing carbon fiber paper: polyacrylonitrile-based carbon fiber and mesophase asphalt-based carbon fiber are mixed in a certain proportion, impregnated with a thermosetting phenolic resin-ethanol solution, and then carbonized and graphitized to obtain carbon fiber paper. Although the obtained carbon fiber paper has excellent electrical and thermal conductivity, the preparation process is relatively complicated, and the carbon fiber paper is brittle and easily broken when subjected to external force.

[0004] Invention patent CN113066995A discloses a PEM fuel cell, high-toughness porous carbon paper and its preparation method, which is to perform carbon deposition on pretreated metal fibers, then prepare a porous carbon paper embryo with polyvinyl alcohol acetal, impregnate N-methylpyrrolidone solution containing bisphenol A phthalonitrile, and obtain high-toughness porous carbon paper after high-temperature carbonization. This preparation method is relatively complicated, and the weight of the carbon paper is relatively high due to the addition of metal fibers. Summary of the invention

[0005] In view of the shortcomings of the prior art, the purpose of the present invention is to improve the durability and air permeability of carbon paper and avoid the problems of easy breakage and low porosity of carbon paper caused by resin carbon. The present invention adopts a resin impregnation method to achieve good connection between carbon fibers, while making it have good bending resistance and high air permeability.

[0006] According to tests, the carbon fiber paper prepared by the present invention has an air permeability of 3250 mm / s and can be bent directly at 90 degrees for dozens of times without breaking.

[0007] In order to achieve the above technical objectives, the present invention is implemented through the following technical solutions.

[0008] A method for preparing high-air-permeability and fold-resistant carbon fiber paper comprises the following steps:

[0009] (1) carbon fiber, bonding fiber and dispersant are wet-formed to obtain carbon fiber base paper;

[0010] (2) dissolving an alcohol-soluble resin in ethanol to obtain a stable ethanol-resin solution, then pouring the ethanol-resin solution into water and stirring to obtain a suspension;

[0011] (3) soaking the carbon fiber base paper in the suspension, taking it out and performing a pre-curing treatment to obtain the impregnated paper;

[0012] (4) The impregnated paper is carbonized under a protective atmosphere to obtain a carbon fiber paper with high air permeability and bending resistance.

[0013] Preferably, the carbon fiber in step (1) is one or more of PAN-based and asphalt-based carbon fibers, and has a length of 2 to 12 mm.

[0014] Preferably, the alcohol-soluble resin in step (2) is a resin with a relatively high residual carbon rate.

[0015] Preferably, the alcohol-soluble resin is one or more of furan resin, phenolic resin and asphalt resin.

[0016] Preferably, the concentration of the ethanol-resin solution is 5% to 60% by weight, and the concentration of the alcohol-soluble resin in the suspension is 0.2% to 20%.

[0017] Preferably, the concentration of the ethanol-resin solution is 5% to 10 wt%, and the concentration of the alcohol-soluble resin in the suspension is 0.5% to 3.0%.

[0018] Preferably, the pre-curing conditions in step (3) are a temperature of 60 to 150°C and a holding time of 30 to 120 min; the carbonization conditions in step (4) are a temperature of 900 to 1400°C, a heating rate of 2 to 15°C / min, and a carbonization treatment time of 30 to 180 min.

[0019] Preferably, the soaking time in step (4) is 30 to 90 seconds. After the soaking, the excess soaking liquid is scraped off, the mixture is dried, and the mixture is turned over every 5 to 30 minutes.

[0020] The high-permeability and bending-resistant carbon fiber paper prepared by the above method can be used in the gas diffusion layer of fuel cells.

[0021] Compared with the prior art, the present invention has the following advantages and beneficial effects:

[0022] (1) The carbon fiber paper prepared by the present invention has a simple process, requires only a small amount of resin as a binder, has a low cost, and is easy to achieve industrial promotion.

[0023] (2) The carbon fiber paper obtained by the method of the present invention has high air permeability, which facilitates the water vapor transmission in the gas diffusion layer.

[0024] (3) The carbon fiber paper obtained by the method of the present invention has good bending resistance and can withstand 90° bending without direct breakage, and has good durability. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 This is a photo of the high air permeability and bending-resistant carbon fiber paper prepared in Example 1.

[0026] Figure 2 This is the SEM image of the high air permeability and bending resistance carbon fiber paper prepared in Example 1.

[0027] Figure 3 This is a SEM image of the cross-sectional morphology of the high air permeability and bending-resistant carbon fiber paper prepared in Example 1.

[0028] Figure 4 This is the SEM image of the high air permeability and bending resistance carbon fiber paper prepared in Example 2.

[0029] Figure 5 This is the SEM image of the carbon fiber paper prepared in Comparative Example 1.

[0030] Figure 6 This is the SEM image of the carbon fiber paper prepared in Comparative Example 2. DETAILED DESCRIPTION

[0031] The present invention is further described in detail below in conjunction with specific embodiments, but the embodiments of the present invention are not limited thereto. For process parameters not particularly noted, conventional techniques may be used.

[0032] Example 1

[0033] (1) 6.28 g of carbon fiber, 50,000 parts of polyethylene oxide and 10% of polyvinyl alcohol fiber are dispersed in a deflaking machine, and a carbon fiber base paper is obtained by wet forming;

[0034] (2) Dissolve 12.64 g of phenolic resin in 200 ml of anhydrous ethanol to form an ethanol-resin solution with a concentration of 6.32%. Take 40 ml of the ethanol-resin solution and inject it into 200 ml of water and stir evenly.

[0035] (3) After soaking the carbon fiber base paper in the impregnation solution in step (2) for 30 seconds, take it out, scrape off the excess impregnation solution, spread it flat until dry, and turn it over every 15 minutes;

[0036] (4) placing the impregnated paper in a high temperature oven and pre-curing it at 80°C for 30 min, 100°C for 30 min, and 140°C for 60 min;

[0037] (5) Place the pre-cured paper in step (4) on N 2 The carbonization treatment was carried out under atmosphere, the temperature was increased to 1400°C at a heating rate of 10°C / min, and the temperature was kept for 60 min to obtain carbon fiber paper.

[0038] Example 2

[0039] (1) 6.28 g of carbon fiber, 50,000 parts of polyethylene oxide and 10% of polyvinyl alcohol fiber are dispersed in a deflaking machine, and a carbon fiber base paper is obtained by wet forming;

[0040] (2) Dissolve 18.97 g of furan resin in 200 ml of anhydrous ethanol to form an ethanol-resin solution with a concentration of 9.5%. Take 50 ml of the ethanol-resin solution and inject it into 200 ml of water and stir evenly.

[0041] (3) After soaking the carbon fiber base paper in the impregnation solution in step (2) for 60 seconds, take it out, scrape off the excess impregnation solution, spread it flat until dry, and turn it over every 20 minutes;

[0042] (4) placing the impregnated paper in a high temperature oven and keeping it at 80°C for 60 minutes and 140°C for 60 minutes for pre-curing treatment;

[0043] (5) Place the pre-cured paper in step (4) on N 2 The carbonization treatment was carried out under atmosphere, the temperature was increased to 1400°C at a heating rate of 10°C / min, and the temperature was kept for 60 min to obtain carbon fiber paper.

[0044] Example 3

[0045] (1) 6.28 g of carbon fiber, 50,000 parts of polyethylene oxide and 10% of polyvinyl alcohol fiber are dispersed in a deflaking machine, and a carbon fiber base paper is obtained by wet forming;

[0046] (2) Dissolve 18.97 g of furan resin in 200 ml of anhydrous ethanol to form an ethanol-resin solution with a concentration of 9.5%. Take 20 ml of the ethanol-resin solution and inject it into 200 ml of water and stir evenly.

[0047] (3) After soaking the carbon fiber base paper in the impregnation solution in step (2) for 60 seconds, take it out, scrape off the excess impregnation solution, spread it flat until dry, and turn it over every 20 minutes;

[0048] (4) placing the impregnated paper in a high temperature oven and keeping it at 80°C for 60 minutes and 140°C for 60 minutes for pre-curing treatment;

[0049] (5) Place the pre-cured paper in step (4) on N 2 The carbonization treatment was carried out under atmosphere, the temperature was increased to 1400°C at a heating rate of 10°C / min, and the temperature was kept for 60 min to obtain carbon fiber paper.

[0050] Example 4

[0051] (1) 6.28 g of carbon fiber, 50,000 parts of polyethylene oxide and 10% of polyvinyl alcohol fiber are dispersed in a deflaking machine, and a carbon fiber base paper is obtained by wet forming;

[0052] (2) Dissolve 18.97 g of phenolic resin in 200 ml of anhydrous ethanol to form an ethanol-resin solution with a concentration of 9.5%. Take 40 ml of the ethanol-resin solution and inject it into 200 ml of water and stir evenly.

[0053] (3) After soaking the carbon fiber base paper in the impregnation solution in step (2) for 60 seconds, take it out, scrape off the excess impregnation solution, spread it flat until dry, and turn it over every 20 minutes;

[0054] (4) placing the impregnated paper in a high temperature oven and keeping it at 80°C for 60 minutes and 140°C for 60 minutes for pre-curing treatment;

[0055] (5) Place the pre-cured paper in step (4) on N 2 The carbonization treatment was carried out under atmosphere, the temperature was increased to 1300°C at a heating rate of 5°C / min, and the temperature was kept for 90 min to obtain carbon fiber paper.

[0056] Comparative Example 1

[0057] The difference between this embodiment and embodiment 1 is that the carbon fiber base paper is directly impregnated in the 6.32% by mass ethanol-resin solution. The air permeability, electrical conductivity and folding endurance of the obtained carbon fiber paper are shown in Table 1.

[0058] Comparative Example 2

[0059] The difference between this embodiment and embodiment 3 is that the carbon fiber base paper is directly impregnated in the 9.5% by mass ethanol-resin solution. The air permeability, electrical conductivity and folding endurance of the obtained carbon fiber paper are shown in Table 1.

[0060] As shown in Table 1, the carbon fiber paper obtained in Examples 1-4 has excellent air permeability and bending resistance. The ethanol-resin solution of Comparative Examples 1 and 2 is not dispersed in water to form a suspension, and the resin carbon is mostly distributed in the carbon fiber grid structure in the form of flakes after carbonization, resulting in poor air permeability and poor bending resistance. Figure 5 , 6 It can be seen that the porosity of the carbon paper in Comparative Examples 1 and 2 is relatively low; while the porosity of the carbon paper of the present invention is significantly improved ( Figure 2-4 ).

[0061] Table 1

[0062]

[0063]

[0064] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.

Claims

1. A method for preparing high-permeability, bending-resistant carbon fiber paper, characterized in that: The following steps are involved: (1) carbon fiber, bonding fiber and dispersant are wet-formed to obtain carbon fiber base paper; (2) dissolving an alcohol-soluble resin in ethanol to prepare an ethanol-resin solution, then pouring the ethanol-resin solution into water and stirring uniformly to obtain a suspension; (3) soaking the carbon fiber base paper in the suspension, taking it out and performing a pre-curing treatment to obtain the impregnated paper; (4) The impregnated paper is carbonized under a protective atmosphere to obtain a carbon fiber paper with high air permeability and bending resistance.

2. The preparation method according to claim 1, characterized in that The carbon fiber in step (1) is one or more of PAN-based and asphalt-based carbon fibers, and has a length of 2 to 12 mm.

3. The preparation method according to claim 1, characterized in that The alcohol-soluble resin in step (2) is a resin with a relatively high residual carbon rate.

4. The preparation method according to claim 1, characterized in that The alcohol-soluble resin is one or more of furan resin, phenolic resin and asphalt resin.

5. The preparation method according to claim 1, 2, 3 or 4, characterized in that: The concentration of the ethanol-resin solution is 5% to 60% by weight, and the concentration of the alcohol-soluble resin in the suspension is 0.2% to 20%.

6. The preparation method according to claim 5, characterized in that The concentration of the ethanol-resin solution is 5% to 10% by weight, and the concentration of the alcohol-soluble resin in the suspension is 0.5% to 3.0%.

7. The preparation method according to claim 6, characterized in that The pre-curing conditions in step (3) are a temperature of 60 to 150° C. and a holding time of 30 to 120 min; the carbonization conditions in step (4) are a temperature of 900 to 1400° C., a heating rate of 2 to 15° C. / min, and a carbonization treatment time of 30 to 180 min.

8. The preparation method according to claim 7, characterized in that The soaking time in step (4) is 30 to 90 seconds. After the soaking is completed, the excess soaking liquid is scraped off and the mixture is dried. The mixture is turned over every 5 to 30 minutes.

9. The high-permeability and bending-resistant carbon fiber paper prepared by the method according to any one of claims 1 to 8.

10. Use of the carbon fiber paper according to claim 9 in a gas diffusion layer of a fuel cell.

Citation Information

Patent Citations

  • Method for preparing carbon fiber paper for gas diffusion layer of fuel cell

    CN101613982A

  • Carbon fiber paper and preparation method thereof

    CN115613390A

  • A carbon paper used in gas diffusion layer of fuel cell and a method of manufacturing thereof

    KR102436335B1

  • Cyber storage system of preserving and distributing private cultural assets

    KR102501263B1