FRP rib reinforced high-ductility concrete bridge deck seamless connecting plate and structural design method
By using a design method of combining high-ductility concrete with FRP ribs in the bridge deck connecting plate, the problem of lack of structural design of the bridge deck connecting plate is solved, and the complete design theory of the bridge deck seamless connecting plate is provided, and the durability of the bridge is improved. and driving comfort, and realize the resource utilization of solid waste.
Patent Information
- Application Number
- CN202410985626.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-11-12
AI Technical Summary
The existing bridge deck connection plate lacks structural design methods and cannot provide a theoretical basis for the bridge deck seamless connection plate, resulting in the bridge being easily damaged when it withstands loads, temperatures and shrinkage deformation, affecting the durability and service life of the bridge.
The high-ductile concrete and FRP ribs are combined with FRP ribs, and the length of the bridge deck seamless connection plate is determined through structural design and numerical simulation methods, and a FRP rib reinforcement seamless connection plate is provided. and structural design methods to ensure the rationality of the design parameters of the bridge deck seamless connection plate.
Through numerical simulation, the stress analysis of the bridge deck seamless connection plate is verified, which provides a complete design theory of the bridge deck seamless connection plate, reduces the number of maintenance, improves the durability and driving comfort of the bridge, and realizes solid waste Resource utilization.
Smart Images

Figure CN118932843A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of bridge design, and in particular to an FRP bar reinforced high-ductility concrete bridge deck seamless connection plate and a structural design method. Background Art
[0002] As a key part of bridge design, steel expansion joint devices are installed between two adjacent spans of simply supported beams or between beam ends and abutments. Their main purpose is to absorb tensile and compressive deformations caused by temperature, shrinkage, creep, etc. After the expansion joint device is installed, a concrete transition zone is poured between the expansion joint and the adjacent concrete pavement layer. Due to the difference in elastic modulus between the steel expansion joint and the concrete in the transition zone, the deformation of the two is inconsistent. Under the action of vehicle loads, the expansion joint or concrete is easily damaged, causing harmful ions to penetrate into the bridge main beam and substructure, resulting in corrosion of reinforced concrete main beams and substructure steel bars, seriously affecting the durability and service life of the bridge, and causing vehicles to jump at the bridge head, affecting driving comfort.
[0003] In response to expansion joint defects, some scholars use bridge deck connection plates to replace expansion joints and prepare bridge deck seamless connection plates to make the entire bridge continuous, flat and seamless. The bridge deck seamless connection plates replace expansion joints. The bridge deck seamless connection plates are located in the negative bending moment area, but the length of the connection plates is not equal to the length of the expansion joints. It is necessary to calculate the length of the bridge deck seamless connection plates, design the reinforcement, and design the bonding and anchoring length of the reinforcement.
[0004] The current patent reports on bridge deck connection plates are shown in Table 1.
[0005] Table 1 Comparison of the research status of bridge deck connection plates in existing patents
[0006]
[0007]
[0008] It can be seen from Table 1 that the existing patents on bridge deck seamless connection plates do not involve specific connection plate structure design methods, and cannot provide a theoretical basis for the promotion of bridge deck seamless connection plates. Summary of the invention
[0009] Aiming at the lack of structural design method for existing bridge deck connection plates, the present invention considers the tensile constitutive relationship of high-ductility concrete, the bending design method of FRP bar reinforced high-ductility concrete bending members, and the calculation of FRP bar bonding anchorage length, integrates theoretical calculation and numerical simulation methods, and provides a FRP bar reinforced high-ductility concrete bridge deck seamless connection plate and structural design method. Through structural design and numerical simulation, design parameters such as bridge deck seamless connection plate length, reinforcement ratio, FRP bar anchorage length, etc. can be determined. It provides a structural design basis for the seamlessness of small and medium-sized reinforced concrete bridges, and can also provide an effective method for solving expansion joint device diseases.
[0010] In order to solve the above technical problems, the technical solution adopted by the present invention is: a FRP bar reinforced high-ductility concrete bridge deck seamless connection plate, which adopts high-ductility concrete with an elastic modulus similar to that of the adjacent concrete pavement layer and with large bending and tensile deformation capacity, selects FRP bars as reinforcing bars, and prepares the bridge deck seamless connection plate with FRP bar reinforced high-ductility concrete; the high-ductility concrete uses 100% coal gangue fine aggregate, and the strength grade of the high-ductility concrete is not less than C40, the ultimate elongation is not less than 1.0%, and the drying shrinkage is not higher than 600με.
[0011] A structural design method for a FRP bar reinforced high-ductility concrete bridge deck seamless connection plate comprises the following steps:
[0012] The first step is to determine the total length of the seamless connection plate based on the load, temperature and concrete shrinkage characteristics of the bridge, assuming the length of the debonding zone of the bridge deck seamless connection plate and the length of the transition zone on both sides, and then determine the total length of the seamless connection plate, which is the length of the debonding zone + 2 times the length of the transition zone;
[0013] In the second step, the FRP reinforcement ratio in the driving direction is calculated according to the maximum crack width in the normal service limit state; the transverse FRP reinforcement ratio is based on the structural reinforcement, that is, the transverse section reinforcement per unit width is not less than 15% of the force-bearing reinforcement per unit width, and the reinforcement ratio is not less than 0.15%;
[0014] Step 3: The bonding anchorage length of the FRP bars in the driving direction is 12 to 22 times the diameter of the FRP bars;
[0015] The fourth step is to obtain the internal forces of high ductility concrete and FRP bars based on numerical simulation, and compare them with the performance of high ductility concrete and FRP bars themselves to verify the rationality of the structural design.
[0016] As a further limitation of the technical solution of the present invention, in the first step, the length of the debonding area of the connecting plate is l dz The specific calculation of is shown in formula (1):
[0017]
[0018] where Δlive-load causes the displacement at the beam end,
[0019] ΔTemperature - deformation caused by temperature difference,
[0020] ΔShrinkage – deformation caused by shrinkage of high ductility concrete itself,
[0021] ε t —Design value of tensile strain for high ductility concrete.
[0022] As a further limitation of the technical solution of the present invention, in the first step, the length of the transition zone is not less than 0.5 m on one side.
[0023] As a further limitation of the technical solution of the present invention, the FRP bar is a BFRP bar or a GFRP bar, or a composite of the two.
[0024] As a further limitation of the technical solution of the present invention, in the second step, the diameter D of the FRP reinforcement in the driving direction is 10-16 mm, and the diameter D of the FRP reinforcement in the transverse direction is 8-10 mm.
[0025] As a further limitation of the technical solution of the present invention, in the second step, the driving direction FRP reinforcement is arranged above the transverse FRP reinforcement, and the thickness of the protective layer of the driving direction FRP reinforcement is not less than 25 mm.
[0026] As a further limitation of the technical solution of the present invention, the maximum crack width calculation method in the second step is shown in formula (2):
[0027]
[0028] Among them, w max —maximum crack width of flexural members;
[0029] ψ—the strain non-uniformity coefficient of the longitudinal tensile FRP reinforcement between cracks, ranging from 0.2 to 1.0;
[0030] σ fk —Stress of FRP tendons under standard combination of load effects;
[0031] E f —Elastic modulus of FRP bars;
[0032] d eq —Equivalent diameter of longitudinal FRP reinforcement in the tension zone (mm);
[0033] C—protective layer thickness (mm), ranging from 20mm to 65mm;
[0034] ρ te —Reinforcement ratio of longitudinal tensile FRP bars calculated based on the effective tensile concrete cross-sectional area.
[0035] As a further limitation of the technical solution of the present invention, in the fourth step, in the numerical simulation, relying on the entire bridge, it is analyzed whether the internal forces in the high-ductility concrete and FRP bars of the bridge deck seamless connection plate, as well as the internal forces of the pavement layer reinforcement and concrete meet the material's own performance requirements under the coupling effects of vehicle load, seasonal temperature difference and shrinkage.
[0036] Compared with the prior art, the present invention has the following beneficial effects:
[0037] 1) In view of the expansion joint disease and the tensile and compressive deformation, the present invention adopts high ductility concrete with a modulus of elasticity similar to that of the adjacent concrete pavement layer and a large bending and tensile deformation capacity, selects FRP bars as reinforcing bars, and uses FRP bars to reinforce high ductility concrete to prepare bridge deck seamless connection plates. The structural design method specifically involves a connection plate length calculation method, a reinforcement design method, a FRP bar bonding anchorage length calculation method, and a numerical simulation verification method. It can provide a complete design theory for the promotion and application of bridge deck seamless connection plates to replace expansion joints.
[0038] 2) Numerical simulation is used to verify the stress analysis of the bridge deck seamless connection plate. The entire bridge is used as the supporting project, and the coupling effects of vehicle loads, seasonal temperature differences and shrinkage on the bridge deck seamless connection plate and pavement concrete are considered. This is consistent with the stress conditions of the bridge deck seamless connection plate in actual engineering applications, and provides a theoretical basis for the engineering application of bridge deck seamless connection plates.
[0039] 3) The bridge deck seamless connection plate adopts corrosion-resistant FRP bars and high-ductility concrete. The material has good durability, which can reduce the number of maintenance times from the perspective of the entire life cycle and reduce economic costs. Coal gangue is used in the preparation of high-ductility concrete to realize the resource utilization of solid waste; reduce the milling noise caused by maintenance, improve the driving comfort of the seamless bridge, and improve people's quality of life. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] Figure 1 The present invention is a flow chart for the design of the bridge deck seamless connection plate structure.
[0041] Figure 2 It is a schematic diagram of the structure of the bridge deck seamless connection plate of the present invention.
[0042] Figure 3 This is the structural design drawing of the seamless connection plate of the bridge deck in Example 1.
[0043] Figure 4 They are the deformation and force diagrams of high ductility concrete in Example 1 respectively.
[0044] Figure 5 They are respectively the deformation and force diagram of the FRP bars in Example 1 (half model).
[0045] Figure 6 This is the structural design drawing of the seamless connection plate of the bridge deck in Example 2.
[0046] Figure 7 They are the deformation and force diagrams of high ductility concrete in Example 2 respectively.
[0047] Figure 8 They are respectively the deformation and force diagram of the FRP bars in Example 2 (half model).
[0048] Fig. 9This is the structural design drawing of the seamless connection plate of the bridge deck in Example 3.
[0049] Fig.10 They are the deformation and force diagrams of high ductility concrete in Example 3 respectively.
[0050] Fig.11 They are respectively the deformation and force diagram of the FRP bars in Example 3 (half model). DETAILED DESCRIPTION
[0051] The present invention is further described below in conjunction with specific embodiments.
[0052] Example 1
[0053] A medium-sized double-span reinforced concrete simply supported beam, with a beam height of 0.95m, a beam width of 1.4m, and a span length of 20m. A 50mm expansion joint is set between the simply supported beams, and a concrete pavement layer is laid on the simply supported beams, with a pavement thickness of 120mm. The highest temperature in the area where the bridge is located is 36℃, the lowest temperature is -5℃, and the annual temperature difference is 41℃. BFRP bars are used to reinforce high-ductility concrete to prepare the bridge deck seamless connection plate, change the original structural design, and cancel the expansion joint.
[0054] High ductility concrete strength grade C45 is used, the ultimate elongation design value is 1.5%, the ultimate tensile strength design value is 5.56MPa, and the shrinkage is 500με. The diameter of the BFRP bar in the driving direction is 14mm, the ultimate tensile strength is 726.3MPa, the ultimate tensile strain is 1.60%, and the elastic modulus is 45.4GPa. The diameter of the transverse BFRP bar is 8mm, the ultimate tensile strength is 683.5MPa, the ultimate tensile strain is 1.56%, and the elastic modulus is 43.8GPa; the diameter of the transverse GFRP bar is 8mm, the ultimate tensile strength is 638.5MPa, the ultimate tensile strain is 1.56%, and the elastic modulus is 40.9GPa. The thickness of the protective layer is 30mm.
[0055] In the first step, it is assumed that the length of the debonding area of the bridge deck seamless connection plate (l dz ) and the length of the transition zone.
[0056] Δactivation=2θ·h=2×0.005×0.95×1000=9.5mm
[0057] ΔTemperature=2×0.00001×20×41=16.4mm
[0058] Δ contraction = 0.5 × 10 -3 × dz
[0059] according to It can be calculated that l dz ≥1.786m, take the length of the debonding area l dzThe length of the transition zone is 1.8m. The length of the transition zone is 0.6m on one side. The total length of the bridge deck seamless connection plate is 3.0m.
[0060] In the second step, the BFRP reinforcement ratio in the driving direction is calculated based on the maximum crack width of the bridge deck seamless connection plate of 0.5mm. The reinforcement in the driving direction is calculated to use 8 BFRP bars with a diameter of 14mm and a spacing of 150mm, that is, 8@150. The bridge deck seamless connection plate in the transverse direction uses 11 BFRP bars with a diameter of 8mm and a spacing of 250mm, that is, 11@250.
[0061] In the third step, the bonding anchorage length of the BFRP reinforcement on the driving direction side is 19 times the diameter, that is, 270mm.
[0062] The fourth step is to use the temperature-load thermal coupling method based on Abaqus software to analyze the stress of the bridge deck seamless connection plate. The maximum tensile strain of high ductility concrete is 0.56%, which is less than the design requirement of 1.5%; the maximum tensile stress is 2.78MPa, which is less than the design requirement of 5.56MPa. The maximum tensile strain of BFRP bars is 0.18%, which is less than the design requirement of 1.60%; the maximum tensile stress is 91.0MPa, which is less than the design requirement of 726.3MPa.
[0063] Example 2
[0064] A small double-span reinforced concrete simply supported beam, with a beam height of 0.8m, a beam width of 1.2m, and a span length of 15m. A 40mm expansion joint is set between the simply supported beams, and a concrete pavement layer is laid on the simply supported beams, with a thickness of 100mm. The highest temperature in the area where the bridge is located is 34℃, the lowest temperature is -2℃, and the annual temperature difference is 36℃. GFRP bars are used to reinforce high-ductility concrete to prepare the bridge deck seamless connection plate, change the original structural design, and cancel the expansion joint.
[0065] High ductility concrete strength grade C40 is used, the ultimate elongation design value is 1%, the ultimate tensile strength design value is 5.62MPa, and the shrinkage is 600με. The diameter of the GFRP bar in the driving direction is 10mm, the ultimate tensile strength is 702.3MPa, the ultimate tensile strain is 1.67%, and the elastic modulus is 42.1GPa. The diameter of the transverse GFRP bar is 8mm, the ultimate tensile strength is 638.5MPa, the ultimate tensile strain is 1.56%, and the elastic modulus is 40.9GPa. The protective layer thickness is 25mm.
[0066] In the first step, it is assumed that the length of the debonding area of the bridge deck seamless connection plate (l dz ) and the length of the transition zone.
[0067] Δactivation=2θ·h=2×0.005×0.8×1000=8mm
[0068] ΔTemperature=2×0.00001×15×1000×36=10.8mm
[0069] Δ contraction = 0.6 × 10 -3 × dz
[0070] according to It can be calculated that l dz ≥2.0m, take the length of the debonding area l dz The length of the transition zone is 2.0m. The length of the transition zone is 0.5m on one side. The total length of the bridge deck seamless connection plate is 3.0m.
[0071] In the second step, the reinforcement ratio of GFRP bars in the driving direction is calculated based on the maximum crack width of the bridge deck seamless connection plate of 0.5mm. The reinforcement calculated in the driving direction is 14 GFRP bars with a diameter of 10mm and a spacing of 90mm, that is, 14@90. The bridge deck seamless connection plate in the transverse direction uses 12 BFRP bars with a diameter of 8mm and a spacing of 250mm, that is, 12@250.
[0072] The third step is that the bonding anchorage length of the GFRP reinforcement on the driving direction side is 12 times the diameter, that is, 120mm.
[0073] The fourth step is to use the temperature-load thermal coupling method based on Abaqus software to analyze the stress of the bridge deck seamless connection plate. The maximum tensile strain of high ductility concrete is 0.55%, which is less than the design requirement of 1.0%; the maximum tensile stress is 2.7MPa, which is less than the design requirement of 5.62MPa. The maximum tensile strain of BFRP bars is 0.19%, which is less than the design requirement of 1.59%; the maximum tensile stress is 93.7MPa, which is less than the design requirement of 701.2MPa.
[0074] Example 3
[0075] A medium-sized double-span reinforced concrete simply supported beam, with a beam height of 1.0m, a beam width of 1.5m, and a span length of 25m. A 60mm expansion joint is set between the simply supported beams, and a concrete pavement layer is laid on the simply supported beams, with a pavement thickness of 120mm. The highest temperature in the area where the bridge is located is 33℃, the lowest temperature is -6℃, and the annual temperature difference is 39℃. BFRP bars and GFRP bars are used to reinforce high-ductility concrete to prepare the bridge deck seamless connection plate, change the original structural design, and cancel the expansion joint.
[0076] High ductility concrete strength grade C50 is used, the ultimate elongation design value is 1.3%, the ultimate tensile strength design value is 5.92MPa, and the shrinkage is 450με. The diameter of BFRP and GFRP bars in the driving direction is 16mm; the ultimate tensile strength of BFRP bars is 734.5MPa, the ultimate tensile strain is 1.59%, and the elastic modulus is 46.2GPa; the ultimate tensile strength of GFRP bars is 722.3MPa, the ultimate tensile strain is 1.64%, and the elastic modulus is 44.1GPa. The diameter of the transverse BFRP bars is 10mm, the ultimate tensile strength is 701.2MPa, the ultimate tensile strain is 1.59%, and the elastic modulus is 44.1GPa. The thickness of the protective layer is 35mm.
[0077] In the first step, it is assumed that the length of the debonding area of the bridge deck seamless connection plate (l dz ) and the length of the transition zone.
[0078] Δactivation=2θ·h=2×0.005×1.0×1000=10mm
[0079] ΔTemperature=2×0.00001×25×1000×39=19.5mm
[0080] Δ contraction = 0.45 × 10 -3 × dz
[0081] according to It can be calculated that l dz ≥2.351m, take the length of the debonding area l dz The length of the transition zone is 2.4m. The length of the transition zone is 0.7m on one side. The total length of the bridge deck seamless connection plate is 3.8m.
[0082] In the second step, the reinforcement ratio of GFRP and BFRP bars in the driving direction is calculated based on the maximum crack width of 0.5mm in the bridge deck seamless connection plate. The reinforcement in the driving direction is calculated as 3 GFRP bars with a diameter of 16mm and 4 BFRP bars. The GFRP and BFRP are arranged at intervals of 200mm, with a total reinforcement of 7@200. The bridge deck seamless connection plate in the transverse direction uses 14 BFRP bars with a diameter of 10mm, with a spacing of 250mm, that is, 14@250.
[0083] In the third step, the bonding anchorage length of the GFRP bars and BFRP bars on the driving direction side is 22 times the diameter, that is, 350mm.
[0084] The fourth step is to use the temperature-load thermal coupling method based on Abaqus software to analyze the stress of the bridge deck seamless connection plate. The maximum tensile strain of high ductility concrete is 0.58%, which is less than the design requirement of 1.3%; the maximum tensile stress is 2.72MPa, which is less than the design requirement of 5.92MPa. The maximum tensile strain of BFRP and GFRP bars is 0.17%, which is less than the design requirement of ultimate tensile strain; the maximum tensile stress is 88.7MPa, which is less than the design requirement of ultimate tensile strength.
[0085] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be thought of by a person skilled in the art within the technical scope disclosed by the present invention without creative work should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope defined in the claims.
Claims
1. A FRP reinforced high ductility concrete bridge deck seamless connection plate, It is characterized in that High-ductility concrete with a similar elastic modulus to that of the adjacent concrete pavement layer and large bending and tensile deformation capacity is used, FRP bars are selected as reinforcing bars, and the high-ductility concrete is reinforced with FRP bars to prepare a bridge deck seamless connection plate; the high-ductility concrete uses 100% coal gangue fine aggregate, the strength grade of the high-ductility concrete is not less than C40, the ultimate elongation is not less than 1.0%, and the drying shrinkage is not higher than 600με.
2. A structural design method for FRP reinforced high ductility concrete bridge deck seamless connection plate, It is characterized in that The following steps are involved: The first step is to determine the total length of the seamless connection plate based on the load, temperature and concrete shrinkage characteristics of the bridge, assuming the length of the debonding zone of the bridge deck seamless connection plate and the length of the transition zone on both sides, and then determine the total length of the seamless connection plate, which is the length of the debonding zone + 2 times the length of the transition zone; In the second step, the FRP reinforcement ratio in the driving direction is calculated according to the maximum crack width in the normal service limit state; the transverse FRP reinforcement ratio is based on the structural reinforcement, that is, the transverse section reinforcement per unit width is not less than 15% of the force-bearing reinforcement per unit width, and the reinforcement ratio is not less than 0.15%; Step 3: The bonding anchorage length of the FRP bars in the driving direction is 12 to 22 times the diameter of the FRP bars; The fourth step is to obtain the internal forces of high ductility concrete and FRP bars based on numerical simulation, and compare them with the performance of high ductility concrete and FRP bars themselves to verify the rationality of the structural design.
3. According to the structural design method of the FRP bar reinforced high ductility concrete bridge deck seamless connection plate of claim 2, It is characterized in that The length of the debonding area of the connecting plate in the first step is l dz The specific calculation of is shown in formula (1): where Δlive-load causes the displacement at the beam end, ΔTemperature - deformation caused by temperature difference, ΔShrinkage – deformation caused by shrinkage of high ductility concrete itself, ε t —Design value of tensile strain for high ductility concrete.
4. According to the structural design method of the FRP bar reinforced high ductility concrete bridge deck seamless connection plate of claim 2, It is characterized in that In the first step, the length of the transition zone is not less than 0.5m on one side.
5. According to the structural design method of the FRP bar reinforced high ductility concrete bridge deck seamless connection plate of claim 2, It is characterized in that The FRP bars are BFRP bars or GFRP bars, or a combination of the two.
6. The structural design method of the FRP bar reinforced high ductility concrete bridge deck seamless connection plate according to claim 2, It is characterized in that In the second step, the diameter D of the FRP reinforcement in the driving direction is 10-16 mm, and the diameter D of the FRP reinforcement in the transverse direction is 8-10 mm.
7. According to the structural design method of the FRP bar reinforced high ductility concrete bridge deck seamless connection plate of claim 1, It is characterized in that In the second step, the driving direction FRP reinforcement is arranged above the transverse FRP reinforcement, and the thickness of the protective layer of the driving direction FRP reinforcement is not less than 25mm.
8. The structural design method of the FRP bar reinforced high ductility concrete bridge deck seamless connection plate according to claim 1, It is characterized in that The calculation method of the maximum crack width in the second step is shown in formula (2): Among them, w max —maximum crack width of flexural members; ψ—the strain non-uniformity coefficient of the longitudinal tensile FRP reinforcement between cracks, ranging from 0.2 to 1.0; σ fk —Stress of FRP tendons under standard combination of load effects; E f —Elastic modulus of FRP bars; d eq —Equivalent diameter of longitudinal FRP reinforcement in the tension zone (mm); C—protective layer thickness (mm), ranging from 20mm to 65mm; ρ te —Reinforcement ratio of longitudinal tensile FRP bars calculated based on the effective tensile concrete cross-sectional area.
9. The structural design method of the FRP bar reinforced high ductility concrete bridge deck seamless connection plate according to claim 1, It is characterized in that In the fourth step, based on the entire bridge, the internal forces in the high-ductility concrete and FRP bars of the bridge deck seamless connection plate, as well as the internal forces in the pavement layer reinforcement and concrete are analyzed in numerical simulation to determine whether they meet the material's own performance requirements under the coupling effects of vehicle load, seasonal temperature difference and shrinkage.