Method and device for measuring high-temperature resistance curve of iron alloy furnace burden
By designing a high-temperature resistance measurement device including large crucibles and graphite rods, the problem of measuring resistance of complex-shaped ferroalloy furnaces is solved, and the accurate measurement of high-temperature resistance and furnace temperature control is achieved, meeting the needs of the ferroalloy industry.
Patent Information
- Application Number
- CN202411060192.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-11-12
AI Technical Summary
The prior art is difficult to accurately measure the resistance of ferroalloy furnace charges of complex shapes under high temperature conditions, and the existing devices are complex in structure and high in cost, which cannot meet the demand for ferroalloy industry for the measurement of resistance of complex furnace charges.
A high-temperature resistance measurement device including a large crucible, an alumina sheet, a graphite sheet, a graphite rod, a metal wire and a heating element is designed to provide pressure stability by setting the furnace material to be tested in the large crucible and using the graphite rod and alumina sheet. , combined with a resistance tester to perform heating and cooling control, and determine the high-temperature resistance curve of the ferroalloy furnace material.
Accurate measurement of the high-temperature resistance of complex ferroalloy furnace materials is achieved, manual operation workload is reduced, measurement accuracy is improved, and the high-temperature resistance change pattern is studied by adjusting the furnace material ratio, which improves the temperature control and thermal efficiency of the electric furnace furnace.
Smart Images

Figure CN118937414A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of high temperature resistance testing, in particular to a method and a device for measuring a high temperature resistance curve of a ferroalloy furnace charge. Background Art
[0002] At present, the ferroalloy industry usually adopts electric furnace smelting to obtain high-carbon ferroalloys, such as high-carbon ferrochrome. The high-temperature smelting process of ferrochrome pellets, coke, silica, dolomite and other furnace materials in the smelting of high-carbon ferrochrome involves complex chemical reactions. Basic physical parameters such as resistance are extremely complex and unstable. In addition, since the furnace charge is in the form of complex shapes and composites, it is a percolation structure, that is, since the furnace charge is a variety of materials, after different particle sizes are mixed together, there will be different gaps, and the material with a small particle size will partially fill the larger gap. Different materials have different matching methods, and the form of their gaps is that there are many kinds. In addition, due to the different types of furnace charges, the overall resistance is also relatively complicated. This is not the measurement of the resistance of a single material, but the measurement of the resistance of this specific structural form of material in the furnace to form a relatively stable overall structure. In addition, under high temperature conditions, there will be complex chemical reactions between the materials, and the gaps are constantly changing. Therefore, these complex changes lead to great difficulties in measuring the resistance of this type of percolation structure under high temperature conditions. Measuring the high-temperature resistance of complex charges will play a very important guiding role in optimizing the charge ratio and improving the furnace temperature control and thermal efficiency of the electric furnace. Therefore, how to measure the high-temperature resistance of such complex charges has become an urgent problem to be solved in the ferroalloy industry.
[0003] The Chinese utility model patent announcement text with announcement number CN210269985U discloses a device for measuring the high-temperature resistance of insulating materials under high voltage. The sample to be tested is heated to different temperatures by adjusting the temperature of the high-temperature furnace cavity, and then the resistance of the sample to be tested is tested using an megohmmeter to obtain the high-temperature resistance of the sample to be tested under high voltage. However, the sample measured by the device is a single regular-shaped solid material, and the resistance of irregular composite furnace materials cannot be measured. The measured resistance is the resistance value obtained when the sample to be tested is reduced by one temperature interval. The manual operation workload is large and the results are inaccurate.
[0004] The Chinese invention patent announcement text with announcement number CN103675454B discloses a resistance testing device, which can measure high-temperature resistance by contact testing of resistance through a four-probe resistance testing device. However, although the measurement accuracy of the measuring device is high, its structure is relatively complex and it is unable to measure solid and irregularly shaped composite furnace charges. At the same time, its relatively high cost makes it unsuitable for resistance measurement of complex furnace charges in the ferroalloy industry. Summary of the invention
[0005] The technical problem to be solved by the present invention is to provide a high temperature resistance measuring device and method capable of measuring the relationship between the resistance and temperature of complex ferroalloy furnace materials in view of the deficiencies of the prior art.
[0006] The specific implementation is through the following technical solutions:
[0007] A device for measuring the high temperature resistance curve of an iron alloy furnace charge comprises a furnace body, a large crucible, an alumina sheet, an upper graphite sheet, a lower graphite sheet, a pad brick, a first graphite rod, a second graphite rod, a small crucible, a first metal wire, a second metal wire, a first lead wire, a second lead wire, a first wiring port, a heating element and a second wiring port.
[0008] The pad brick is arranged at the inner bottom of the furnace body, a groove is opened at a non-edge position of the pad brick, the small crucible is arranged in the groove, and the first graphite rod is vertically arranged in the small crucible.
[0009] The large crucible is arranged on the upper part of the cushion brick, and the outer bottom wall of the large crucible is in contact with the top wall of the cushion brick. A lower graphite sheet, a charge to be tested, an upper graphite sheet and an alumina sheet are arranged in sequence from bottom to top in the large crucible. The second graphite rod passes through the alumina sheet and is vertically arranged with the top protruding from the alumina sheet. A bottom hole is opened on the bottom wall of the large crucible. The diameter or equivalent diameter of the bottom hole is greater than or equal to the diameter or equivalent diameter of the second graphite rod. The top end of the first graphite rod passes through the bottom hole and contacts the bottom end of the lower graphite sheet.
[0010] One end of the first metal wire is connected to the lower graphite sheet, and the other end of the first metal wire is connected to the first lead wire arranged in the furnace body; one end of the second metal wire is connected to the second graphite rod, and the other end of the second metal wire is connected to the second lead wire arranged in the furnace body.
[0011] The first connecting wire is connected to the first wiring port arranged outside the furnace body, the second connecting wire is connected to the second wiring port arranged outside the furnace body, and the first wiring port and the second wiring port are respectively connected to the positive and negative electrodes of the resistance tester arranged outside the furnace body.
[0012] The heating element for heating the interior of the furnace body is arranged in the furnace body.
[0013] Preferably, the total mass of the alumina sheet, the upper graphite sheet and the second graphite rod is G, the average diameter of the coke in the ferroalloy charge is d, the volume of the space formed between the upper graphite sheet and the lower graphite sheet in the large crucible is v, and 5 (g / mm) ≤ G / d ≤ 78 (g / mm) and / or 0.9 (g / cm 3 )≤G / v≤9.5(g / cm 3 ).
[0014] Preferably, the device for measuring the high temperature resistance of the ferroalloy charge also includes a resistance tester.
[0015] Preferably, the alumina sheet is provided with a through hole, the second graphite rod passes through the through hole, and the bottom end of the second graphite rod is in contact with the top end of the upper graphite sheet.
[0016] Preferably, the furnace body is a box-type furnace body with a temperature control accuracy of ±1°C and a temperature range of 800-1700°C;
[0017] Preferably, the resistance tester is a DC low resistance tester, the test resistance range is 0.1 μΩ to 110 MΩ, and the test accuracy is 0.01%.
[0018] Preferably, the large crucible and the small crucible are both alumina crucibles.
[0019] Preferably, the large crucible and the small crucible are both cylindrical crucibles.
[0020] Preferably, the alumina sheet, the upper graphite sheet and the lower graphite sheet are all circular sheet structures with equal diameters.
[0021] Preferably, the aluminum oxide sheet is one sheet or multiple sheets are stacked.
[0022] Preferably, the diameters of the alumina sheet, the upper graphite sheet and the lower graphite sheet are less than or equal to or substantially equal to the inner diameter of the large crucible.
[0023] Preferably, the pad brick is a rectangular parallelepiped, a cube, a truncated cone or a square cone with the groove provided at the center.
[0024] Preferably, the material of the pad brick is alumina;
[0025] Preferably, the heating element is a silicon molybdenum rod.
[0026] Preferably, the first metal wire and the second metal wire are both molybdenum wires or platinum-rhodium wires; the first connecting wire and the second connecting wire are both platinum-rhodium wires.
[0027] Preferably, the first graphite rod and the second graphite rod are round rods or polygonal rods.
[0028] A method for measuring the high temperature resistance curve of an iron alloy charge, the method being carried out using the above-mentioned measuring device, comprising the following steps:
[0029] S1. Place a small crucible in the groove of the pad brick, and vertically place the first graphite rod in the small crucible.
[0030] S2. Place a large crucible on top of a cushion brick, with the outer bottom wall of the large crucible in contact with the top wall of the cushion brick, pass the top end of the first graphite rod through the bottom hole of the large crucible, and place a lower graphite sheet, a charge to be tested, an upper graphite sheet and an alumina sheet in the large crucible from bottom to top, so that the top end of the first graphite rod is in contact with the bottom end of the lower graphite sheet, and pass the second graphite rod through the alumina sheet and set it vertically with the top protruding from the alumina sheet.
[0031] S3. Clamp one end of the first metal wire between the lower graphite sheet and the first graphite rod, and connect the other end of the first metal wire to the first lead wire disposed in the furnace body; connect one end of the second metal wire to the second graphite rod, and connect the other end of the second metal wire to the second lead wire disposed in the furnace body.
[0032] S4, closing the furnace door of the furnace body (101), starting the heating element (112) to heat the furnace body, and simultaneously starting the resistance tester, and controlling the temperature in the furnace by the heating element (112) to be 0°C to the first insulation threshold, the heating rate is 3 to 6.8°C / min, and the insulation time of the first insulation threshold is 18 to 23 minutes; the heating rate is 4.8 to 8.2°C / min from the first insulation threshold to the second insulation threshold, and the insulation time of the second insulation threshold is 19 to 22 minutes; the heating rate is 2.1 to 5.0°C / min from the second insulation threshold to the third insulation threshold, and the insulation time of the third insulation threshold is 28 to 32 minutes; the cooling rate is 2.2 to 3.6°C / min from the third insulation threshold to the fourth insulation threshold n, the insulation time at the fourth insulation threshold is 18 to 22 hours; the cooling rate from the fourth insulation threshold to the fifth insulation threshold is 2.0 to 4.5°C / min, and the insulation time of the fifth insulation threshold is 18 to 22 minutes; the cooling rate from the fifth insulation threshold to the final temperature threshold is 3.9 to 5.8°C / min, and the insulation time of the final temperature threshold is 16 to 21 minutes, and then the cooling rate is controlled to be 3 to 6°C / min to room temperature or 0°C; wherein the first insulation threshold is 240 to 265°C, the second insulation threshold is 930 to 980°C, the third insulation threshold is 1350 to 1550°C, the fourth insulation threshold is 1180 to 1250°C, the fifth insulation threshold is 880 to 920°C, and the final temperature threshold is 385 to 420°C.
[0033] S5. The high-temperature resistance of the ferroalloy charge is measured by a resistance tester at the end of the first insulation threshold insulation time, the end of the second insulation threshold insulation time, the end of the third insulation threshold insulation time, the end of the fourth insulation threshold insulation time, the end of the fifth insulation threshold insulation time, the end of the sixth insulation threshold insulation time and the end of the final insulation threshold insulation time to form a high-temperature resistance curve of the ferroalloy charge.
[0034] Preferably, the ferroalloy charge includes pellets, coke and silica, and the average particle size of the pellets: the average particle size of the coke: the average particle size of the silica is (10-30): (5-40): (5-25).
[0035] Further preferably, due to the use of an open writing method, within this range, in addition to the above-mentioned main charges, dolomite can also be optionally included, and the particle size ratio of dolomite to the above-mentioned charge components is 5-20, that is, the average particle size of the pellet ore: the average particle size of the coke: the average particle size of the silica: the average particle size of the dolomite is (10~30): (5~40): (5~25): (5-20).
[0036] The “inner diameter”, “outer diameter”, etc. referred to in the present invention are all “diameters”.
[0037] The technical effects of the present invention are:
[0038] 1. The present invention places a large crucible in a furnace body, places a charge to be tested with a complex structure and composition between an upper graphite sheet and a lower graphite sheet in the large crucible, and arranges an alumina sheet and a second graphite rod on the upper part of the upper graphite sheet to stabilize the pressure of the charge to be tested. The position of the charge is limited by the large crucible (i.e., forming an integral material with a volume) and the relative relationship between the mass of the upper components such as the upper graphite sheet and the alumina sheet and the average diameter of the coke is limited (as well as the relative relationship between the mass and the effective volume), so that in the specific heating process set by the present invention, it is possible to ensure that the charge in the large crucible has a certain pressure so that its structure remains relatively stable, and it is possible to simulate the situation that the gaps in the charge in the early stage of real smelting become slightly smaller due to gravity through complex chemical changes during the heating process, and the gaps are not too compressed and distorted due to the existence of excessive pressure on the charge, so that the change in the resistance of the charge under specific high temperature conditions can be more realistically measured.
[0039] 2. By arranging a small crucible in the pad brick and arranging a first graphite rod in the small crucible, the lower graphite sheet and the first graphite rod are tightly matched by gravity, so that the first metal wire can be in contact with the lower graphite sheet more stably, thereby enhancing the data stability during resistance measurement; before conducting a high-temperature resistance test, the charge is tested at room temperature to reduce the resistance difference caused by the different placement positions of the raw materials in the crucible. At the same time, the present invention can change the charge ratio, and then study the influence of the change of one or several charges on the high-temperature resistance of complex charges.
[0040] 3. The present invention limits the temperature thresholds of heating and cooling, and sets different heating rates or cooling rates and insulation time, so that the actual resistance change of the charge in the early stage of smelting can be measured more fully and truly. Since the heating process of the electric furnace is achieved by arc discharge, rather than the temperature control of an ordinary resistance furnace, the temperature change of the heating process of the electric furnace cannot be controlled in real time by humans, and the measurement of conventional high-temperature resistance curves is not exactly the same as the actual heating process of the electric furnace. The present invention has found that the furnace is cold at the beginning of heating and needs to absorb a lot of heat. The present invention sets the heating rate of this stage to a specific relatively high heating rate in stages. When the temperature reaches a certain temperature, each charge will undergo a certain chemical reaction. Setting a relatively low heating rate can match the actual reaction in the electric furnace. During the cooling process, it is mainly used for reverse verification. Due to certain chemical reactions, the void structure also undergoes slight changes. The present invention reasonably sets the cooling rate to form a matching relationship with the heating stage, so that the resistance of each temperature stage can be more reasonably measured in a verification manner, and the overall setting makes the high-temperature resistance measurement more accurate. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] Figure 1 This is a perspective structural schematic diagram of a measuring device according to an embodiment of the present invention.
[0042] Figure 2 The figure is a schematic structural diagram of a resistance tester according to an embodiment of the present invention.
[0043] Figure 3 Schematic diagram for comparison of charge configurations according to an embodiment of the present invention.
[0044] Figure 4 This is a schematic diagram of a high temperature resistance curve obtained according to an embodiment of the present invention.
[0045] Figure 5 This is a schematic diagram of a high temperature resistance curve obtained according to another embodiment of the present invention.
[0046] Among them, 101-furnace body; 102-large crucible; 103-alumina sheet; 104-upper graphite sheet; 105-lower graphite sheet; 106-pad brick; 107-groove; 108-second graphite rod; 109-small crucible; 110-first metal wire; 111-first lead wire; 112-heating element; 113-first graphite rod, 114-second metal wire, 115-second lead wire, 116-first wiring port; 117-second wiring port; 118-furnace charge to be tested;
[0047] 200-display screen; 201-negative pole; 202-positive pole; 203-U disk socket.
[0048] Figure 3 Among them, (a) is ferrochrome pellets; (b) is coke; (c) is dolomite; and (d) is silica. DETAILED DESCRIPTION
[0049] In order to make the purpose, technical solution and advantages of the embodiment of the present invention clearer, the technical solution in the embodiment of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiment of the present invention. Obviously, the described embodiment is a part of the embodiment of the present invention, not all of the embodiments. At the same time, the terms such as "upper", "lower", "front", "back", "middle" and the like involved in this specification are based on the orientation of the normal operation of the present invention, and do not limit the orientation during storage and transportation. They only represent relative positional relationships, not absolute positional relationships, and are only for the convenience of description, rather than for limiting the scope of the implementation of the present invention. Changes or adjustments in their relative relationships should also be regarded as the scope of the implementation of the present invention without substantial changes in the technical content. Specific implementation methods Unless otherwise specified, each feature is only an example of a series of equivalent or similar features. It is only to help understand the present invention. Those skilled in the art should understand that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0050] Example 1
[0051] like Figure 1 As shown, the high temperature resistance measuring device of this embodiment includes a furnace body 101, a large crucible 102 made of alumina, an alumina sheet 103, an upper graphite sheet 104, a lower graphite sheet 105, a spacer brick 106, a first graphite rod 108, a second graphite rod 113, a small crucible 109 made of alumina, a first metal wire 110, a second metal wire 114, a first lead wire 111, a second lead wire 115, a first connection port 116, a heating element 112, and a second connection port 117. The measuring device of the present invention also includes the following: Figure 2 Resistance tester shown.
[0052] like Figure 1 As shown, the pad brick 106 is a rectangular parallelepiped structure, which is arranged at the inner bottom of the furnace body 101. A groove 107 is opened at the center of the pad brick 106. The small crucible 109 is arranged in the groove 107, and the first graphite rod 108 is vertically arranged in the small crucible 109.
[0053] The large crucible 102 is arranged on the upper part of the pad brick 106, and the outer bottom wall of the large crucible 102 is in contact with the top wall of the pad brick 106. The lower graphite sheet 105, the furnace charge 118 to be tested, the upper graphite sheet 104 and the alumina sheet 103 are arranged in sequence from bottom to top in the large crucible 102. The alumina sheet 103 is provided with a through hole, and the second graphite rod 113 passes through the through hole, and the bottom end of the second graphite rod 113 contacts the top end of the upper graphite sheet 104, and the top end or upper part of the second graphite rod 113 contacts the second metal wire 114. The bottom wall of the large crucible 102 is provided with a bottom hole, and the diameter or equivalent diameter of the bottom hole is greater than or equal to the diameter or equivalent diameter of the second graphite rod, and the top end of the first graphite rod 108 passes through the bottom hole and contacts the bottom end of the lower graphite sheet 105. The first graphite rod and the second graphite rod in this embodiment are both round rods.
[0054] One end of the first metal wire 110 is connected to the lower graphite sheet 105, and the other end of the first metal wire 110 is connected to the first lead wire 111 arranged in the furnace body 101; one end of the second metal wire 114 is connected to the second graphite rod 113, and the other end of the second metal wire 114 is connected to the second lead wire 115 arranged in the furnace body 101.
[0055] The first connecting wire 111 is connected to a first wiring port 116 disposed outside the furnace body 101, and the second connecting wire 115 is connected to a second wiring port 117 disposed outside the furnace body 101. The first wiring port 116 and the second wiring port 117 are respectively connected to the positive and negative poles of a resistance tester disposed outside the furnace body 101.
[0056] The heating element 112 for heating the interior of the furnace body 101 is arranged inside the furnace body 101 .
[0057] The furnace body described in this embodiment is a box-type furnace, model KF1700, with a temperature control accuracy of ±1°C and a temperature range of 800 to 1700°C.
[0058] The resistance tester in this embodiment is a DC low resistance tester, model RK2514N, with a test resistance range of 0.1 μΩ-110 MΩ and a test accuracy of 0.01%.
[0059] like Figure 2 As shown, the resistance tester includes a display screen 200, a cathode 201, a cathode 202, and a USB flash drive socket 203. In this embodiment, the cathode 201 is connected to the second wiring port 117 through a wire, the cathode 202 is connected to the first wiring port 116 through a wire, the display screen 200 is used to display data, and the USB flash drive socket 203 is used to connect a USB flash drive storing data.
[0060] The pad bricks in this embodiment are made of alumina, the first metal wire and the second metal wire are both platinum-rhodium wires, the first lead wire and the second lead wire are both platinum-rhodium wires, and the heating element is a 1800-type silicon-molybdenum rod. The alumina sheet, the upper graphite sheet and the lower graphite sheet are all disc structures with equal diameters.
[0061] Example 2
[0062] This embodiment is a method for measuring the high temperature resistance curve of a specific furnace charge using the device of embodiment 1. The furnace charge to be measured in this embodiment is as follows: Figure 3 The furnace charge is formed by randomly mixing 298.5 g of chromite pellets with a particle size of 10 to 30 mm, 63.5 g of coke with a particle size of 5 to 40 mm (average particle size of 29.2 mm), 21.5 g of dolomite with a particle size of 5 to 20 mm, and 35.1 g of silica with a particle size of 15 to 25 mm, wherein the coke accounts for 63.5 / 418.6=15.16%, and the total volume of the large alumina crucible of this embodiment is 617 cm 3 , and the volume v of the charge storage part is 445.32cm 3 The total weight G of all alumina sheets, upper graphite sheets and upper graphite rods is 767 g, that is, G / d = 26.27 (g / mm), which is within the range of 5 to 78 (g / mm), meeting the requirement of 5 (g / mm) ≤ G / d ≤ 78 (g / mm), and G / v = 1.73, which also meets the requirement of 0.9 (g / cm 3 )≤G / v≤9.5(g / cm 3 ), the determination method comprises the following steps:
[0063] S1. Place a small crucible 109 in the groove 107 of the pad brick 106 , and vertically place a first graphite rod 108 in the small crucible 109 .
[0064] S2. Place the large crucible 102 (the outer diameter of the large crucible in this embodiment is 100 mm and the height is 100 mm) on the upper part of the pad brick 106, and the outer bottom wall of the large crucible 102 is in contact with the top wall of the pad brick 106. Place the lower graphite sheet 105, the charge 118 to be tested, the upper graphite sheet 104 and the alumina sheet 103 in order from bottom to top inside the large crucible 102. The alumina sheet 103 is provided with a through hole, and the second graphite rod 113 passes through the through hole, and the bottom end of the second graphite rod 113 is in contact with the top end of the upper graphite sheet 104. The bottom wall of the large crucible 102 is provided with a bottom hole, and the diameter or equivalent diameter of the bottom hole is greater than or equal to the diameter or equivalent diameter of the second graphite rod 113. The top end of the first graphite rod 108 passes through the bottom hole and contacts the bottom end of the lower graphite sheet 105. The first graphite rod and the second graphite rod in this embodiment are both round rods.
[0065] S3. Connect one end of the first metal wire 110 to the lower graphite sheet 105, and the other end of the first metal wire 110 to the first lead wire 111 disposed in the furnace body 101; connect one end of the second metal wire 114 to the upper graphite sheet 104, and the other end of the second metal wire 114 to the second lead wire 115 disposed in the furnace body.
[0066] S4, close the furnace door of the furnace body 101, insert the USB flash drive into the USB flash drive socket of the resistance tester, start the heating element 112 to heat the furnace body, and start the resistance tester at the same time, and control the temperature in the furnace by the heating element 112. Figure 4 The heating and cooling curves shown are used for heating and cooling, specifically 0-255°C, heating rate 5°C / min, heating time 51min, 255°C insulation for 20min; 255-950°C, heating rate 5°C / min, heating time 139min, 950°C insulation for 20min; 950-1400°C, heating rate 3°C / min, heating time 150min, 1400°C insulation for 30min; 1400- 1200℃, cooling rate 3℃ / min, cooling time 70min, keep at 1200℃ for 20min; 1200-900℃, cooling rate 3℃ / min, cooling time 100min, keep at 900℃ for 20min; 900-400℃, cooling rate 5℃ / min, cooling time 100min, keep at 400℃ for 20min; 400-0℃, cooling rate 5℃ / min, cooling time 80min.
[0067] S5, using a resistance tester to measure the high temperature resistance of the ferroalloy charge at the end of the first insulation threshold insulation time, the end of the second insulation threshold insulation time, the end of the third insulation threshold insulation time, the end of the fourth insulation threshold insulation time, the end of the fifth insulation threshold insulation time, the end of the sixth insulation threshold insulation time and the end of the final insulation time, to form a high temperature resistance curve of the ferroalloy charge as shown in Figure 4 shown.
[0068] The coke content in this embodiment is about 15 wt.%. Figure 4 It can be concluded that: (1) When the temperature is 0-500℃, the resistance value of the charge is maintained at a low level, and as the temperature gradually rises, this is mainly due to the volatilization of moisture in the charge.
[0069] (2) When the temperature is 500-1160℃, the resistance value of the charge shows a fluctuating trend with the increase of temperature; this phenomenon is attributed to a variety of complex physical and chemical processes, including but not limited to the volatilization of coke, the transformation of silica crystal form, the decomposition of specific compounds, and the possible interaction between different charges. These processes intricately affect the conductive structure inside the charge, resulting in a fluctuating growth pattern of the resistance value with the increase of temperature.
[0070] (3) When the temperature is 1160-1285℃, the resistance value of the charge increases sharply with the increase of temperature and then decreases sharply. As the temperature increases, the resistance value rises sharply. This is basically due to the complex chemical reaction of the charge, which generates molten oxide with high resistivity (the total weight G of the alumina sheet, upper graphite sheet and upper graphite rod is the most stringent requirement at this stage). However, when the temperature continues to rise, the melting process of the chromite pellets accelerates, the liquid phase ratio increases significantly, and the reduction reaction proceeds, which promotes the formation of metal phases. These conductive phases cover the surface of the pellets, greatly enhancing the conductivity of the charge. It was found through thermodynamic calculations that primary slag was formed in this temperature range. These reasons caused the resistance value to drop sharply in a short period of time.
[0071] (4) When the temperature is 1285-1400°C, the resistance value of the charge shows good stability and hardly changes with the increase of temperature, indicating that the resistance value of the charge structure of this embodiment tends to be stable. The setting of the temperature threshold range of the present invention matches this characteristic, and the resistance of the charge within this temperature range is maintained at a relatively constant level.
[0072] Example 3
[0073] The other configurations of this embodiment are the same as those of embodiment 2, except that 283g of ferrochrome pellets, 83.72g of coke, 20g of dolomite, and 31.8g of silica. The proportion of coke is 83.72 / 418.52=20%, that is, 20% of coke is added, and the high temperature resistance curve is as follows: Figure 5 shown.
[0074] The coke ratio in this embodiment is 20wt.%, Figure 5 It can be obtained that: (1) When the temperature is 0-400℃, the resistance value of the charge increases slowly with the increase of temperature, which is mainly due to the volatilization of moisture in the charge.
[0075] (2) When the temperature is 400-700℃, the resistance of the charge increases sharply and then decreases rapidly. This is basically due to the volatilization of the coke, which makes the coke loose and increases the resistivity of the charge. As the temperature rises, the ferrochrome pellets in the charge undergo a reduction reaction to generate metal phases, which adhere to the surface of the pellets and effectively reduce the resistivity of the entire charge.
[0076] (3) When the temperature is 700-900℃, the resistance of the charge decreases in a fluctuating manner. This is mainly due to the decomposition of dolomite, the crystal transformation of silica and the reduction reaction in the ferrochrome pellets.
[0077] (4) When the temperature is 900-1400℃, the resistance of the charge fluctuates continuously within a relatively low range. At this stage, a relatively stable metal phase structure has been formed inside the charge, providing a stable path for conduction. However, the high temperature environment still promotes the continued crystal transformation of silica, which may be accompanied by the formation of primary slag. Although these processes are not drastic, they are enough to cause slight fluctuations in the resistance value of the charge.
[0078] That is, the device and method provided by the present invention can accurately measure the high temperature resistance curves of furnace materials with different components.
[0079] Comparative Example 1
[0080] The other configurations of this comparative example are the same as those of Example 2, except that the total weight G of all the alumina sheets, the upper graphite sheet, and the upper graphite rod is set to 2508 g (and the effective volume v of the large crucible is also increased to 515.22 cm 3 ), the average diameter of the coke in the ferroalloy charge was determined to be 28.5 mm, wherein G / d=88, which does not meet the requirement of 5 (g / mm)≤G / d≤78 (g / mm). After the same steps as in Example 2, the heating and cooling processes were carried out, and it was found that after the end, the height of the ferroalloy charge dropped by about 18%. This is because the relatively large pressure causes some normal voids therein to be compressed during the high temperature process, thereby destroying the form of the original percolation structure, resulting in inaccurate determination of the high temperature resistance curve.
[0081] The technical principle of the present invention is described above in conjunction with specific embodiments. These descriptions are only for explaining the principles of the present invention and cannot be interpreted in any way as limiting the scope of protection of the present invention. The present invention provides a method and device for measuring the high-temperature resistance curve of an iron alloy furnace charge. There are many methods and ways to implement the technical solution. The above is only a preferred embodiment of the present invention. The part without comparison means that the effect can be explained by using text description. It should be pointed out that for ordinary technicians in this technical field, without departing from the principle of the present invention, several improvements and modifications can be made, and these improvements and modifications should also be regarded as the scope of protection of the present invention. All components not specified in this embodiment can be implemented using existing technologies.
Claims
1. A device for measuring the high temperature resistance curve of ferroalloy charge, characterized in that: The invention comprises a furnace body (101), a large crucible (102), an alumina sheet (103), an upper graphite sheet (104), a lower graphite sheet (105), a pad brick (106), a first graphite rod (108), a second graphite rod (113), a small crucible (109), a first metal wire (110), a second metal wire (114), a first lead wire (111), a second lead wire (115), a first connection port (116), a heating element (112) and a second connection port (117); The cushion brick (106) is arranged at the inner bottom of the furnace body (101); a groove (107) is provided at a non-edge position of the cushion brick (106); the small crucible (109) is arranged in the groove (107); and the first graphite rod (108) is vertically arranged in the small crucible (109); The large crucible (102) is arranged on the upper part of the cushion brick (106), and the outer bottom wall of the large crucible (102) is in contact with the top wall of the cushion brick (106). A lower graphite sheet (105), a furnace charge to be tested (118), an upper graphite sheet (104) and an alumina sheet (103) are arranged in sequence from bottom to top in the large crucible (102). The second graphite rod (113) passes through the alumina sheet and is vertically arranged with its top protruding from the alumina sheet (103). A bottom hole is opened on the bottom wall of the large crucible (102). The diameter or equivalent diameter of the bottom hole is greater than or equal to the diameter or equivalent diameter of the second graphite rod. The top end of the first graphite rod (108) passes through the bottom hole and is in contact with the bottom end of the lower graphite sheet (105). One end of the first metal wire (110) is connected to the lower graphite sheet (105), and the other end of the first metal wire (110) is connected to the first lead wire (111) disposed in the furnace body (101); one end of the second metal wire (114) is connected to the second graphite rod (113), and the other end of the second metal wire (114) is connected to the second lead wire (115) disposed in the furnace body (101); The first lead wire (111) is connected to a first wiring port (116) arranged outside the furnace body (101), the second lead wire (115) is connected to a second wiring port (117) arranged outside the furnace body (101), and the first wiring port (116) and the second wiring port (117) are respectively connected to a positive electrode and a negative electrode of a resistance tester arranged outside the furnace body (101); The heating element (112) for heating the interior of the furnace body (101) is arranged inside the furnace body (101).
2. The device for measuring the high temperature resistance curve of ferroalloy charge according to claim 1, characterized in that: The total mass of the alumina sheet (103), the upper graphite sheet (104) and the second graphite rod (113) is G, the average diameter of the coke in the ferroalloy charge is d, the volume of the space formed between the upper graphite sheet (104) and the lower graphite sheet (105) in the large crucible (102) is v, and 5 (g / mm) ≤ G / d ≤ 78 (g / mm) and / or 0.9 (g / cm 3 )≤G / v≤9.5(g / cm 3 ).
3. The device for measuring the high temperature resistance curve of ferroalloy charge according to claim 1, characterized in that: The device for measuring the high temperature resistance of the ferroalloy furnace charge also includes a resistance tester.
4. The device for measuring the high temperature resistance curve of ferroalloy charge according to claim 1, characterized in that: The alumina sheet (103) is provided with a through hole, the second graphite rod (113) passes through the through hole, and the bottom end of the second graphite rod (113) is in contact with the top end of the upper graphite sheet (104).
5. The device for measuring the high temperature resistance curve of ferroalloy charge according to claim 1 or 3, characterized in that: The furnace body (101) is a box-type furnace body with a temperature control accuracy of ±1°C and a temperature range of 800-1700°C; The resistance tester is a DC low resistance tester, the test resistance range is 0.1μΩ~110MΩ, and the test accuracy is 0.01%; The large crucible (102) and the small crucible (109) are both alumina crucibles; The large crucible (102) and the small crucible (109) are both cylindrical crucibles; The aluminum oxide sheet (103), the upper graphite sheet (104) and the lower graphite sheet (105) are all circular sheet structures with equal diameters; The aluminum oxide sheet (103) is one sheet or a plurality of sheets stacked together; The diameters of the alumina sheet (103), the upper graphite sheet (104) and the lower graphite sheet (105) are less than or equal to or substantially equal to the inner diameter of the large crucible (102); The pad brick (106) is a rectangular parallelepiped, a cube, a truncated cone or a square cone structure with the groove (107) provided at the center.
6. The device for measuring the high temperature resistance curve of ferroalloy charge according to claim 1, characterized in that: The material of the pad brick (106) is alumina; The heating element (112) is a silicon-molybdenum rod.
7. The device for measuring the high temperature resistance curve of ferroalloy charge according to claim 1, characterized in that: The first metal wire (110) and the second metal wire (114) are both molybdenum wires or platinum-rhodium wires; the first connecting wire (111) and the second connecting wire (115) are both platinum-rhodium wires.
8. The device for measuring the high temperature resistance curve of ferroalloy charge according to claim 1, characterized in that: The first graphite rod (108) and the second graphite rod (113) are round rods or polygonal rods.
9. A method for measuring the high temperature resistance curve of ferroalloy charge, characterized in that: The measuring method is carried out using the measuring device according to any one of claims 1 to 8, comprising the following steps: S1, placing a small crucible (109) in the groove (107) of the pad brick (106), and vertically placing a first graphite rod (108) in the small crucible (109); S2, placing the large crucible (102) on the upper part of the pad brick (106), with the outer bottom wall of the large crucible (102) in contact with the top wall of the pad brick (106), passing the top end of the first graphite rod (108) through the bottom hole of the large crucible (102), placing the lower graphite sheet (105), the charge to be tested (118), the upper graphite sheet (104) and the alumina sheet (103) in the large crucible (102) from bottom to top, so that the top end of the first graphite rod (108) is in contact with the bottom end of the lower graphite sheet (105), and passing the second graphite rod (113) through the alumina sheet and arranged vertically with the top protruding from the alumina sheet (103); S3, clamping one end of the first metal wire (110) between the lower graphite sheet (105) and the first graphite rod (108), and connecting the other end of the first metal wire (110) to a first lead wire (111) disposed in the furnace body (101); connecting one end of the second metal wire (114) to the second graphite rod (113), and connecting the other end of the second metal wire (114) to a second lead wire (115) disposed in the furnace body (101); S4, closing the furnace door of the furnace body (101), starting the heating element (112) to heat the furnace body, and simultaneously starting the resistance tester, and controlling the temperature in the furnace by the heating element (112) to be 0°C to the first insulation threshold, the heating rate is 3 to 6.8°C / min, and the insulation time of the first insulation threshold is 18 to 23 minutes; the heating rate is 4.8 to 8.2°C / min from the first insulation threshold to the second insulation threshold, and the insulation time of the second insulation threshold is 19 to 22 minutes; the heating rate is 2.1 to 5.0°C / min from the second insulation threshold to the third insulation threshold, and the insulation time of the third insulation threshold is 28 to 32 minutes; the cooling rate is 2.2 to 3.6°C / min from the third insulation threshold to the fourth insulation threshold n, the insulation time at the fourth insulation threshold is 18 to 22 hours; the cooling rate from the fourth insulation threshold to the fifth insulation threshold is 2.0 to 4.5°C / min, and the insulation time of the fifth insulation threshold is 18 to 22 minutes; the cooling rate from the fifth insulation threshold to the final temperature threshold is 3.9 to 5.8°C / min, and the insulation time of the final temperature threshold is 16 to 21 minutes, and then the cooling rate is controlled to be 3 to 6°C / min to room temperature or 0°C; wherein the first insulation threshold is 240 to 265°C, the second insulation threshold is 930 to 980°C, the third insulation threshold is 1350 to 1550°C, the fourth insulation threshold is 1180 to 1250°C, the fifth insulation threshold is 880 to 920°C, and the final temperature threshold is 385 to 420°C; S5. The high-temperature resistance of the ferroalloy charge is measured by a resistance tester at the end of the first insulation threshold insulation time, the end of the second insulation threshold insulation time, the end of the third insulation threshold insulation time, the end of the fourth insulation threshold insulation time, the end of the fifth insulation threshold insulation time, the end of the sixth insulation threshold insulation time and the end of the final insulation threshold insulation time to form a high-temperature resistance curve of the ferroalloy charge.
10. The method for measuring the high temperature resistance curve of ferroalloy charge according to claim 9, characterized in that: The ferroalloy furnace charge includes pellets, coke and silica, and the average particle size of the pellets: the average particle size of the coke: the particle size of the silica is (10-30): (5-40): (5-25).
Citation Information
Patent Citations
Resistance testing device
CN103675454B
Device for measuring high-temperature resistance of insulating material under high voltage
CN210269985U