Polarization-maintaining gain fiber and preparation method thereof

By using Er, Yb, P co-doped quartz core layer and Cl doped quartz cladding in polarized erbium ytterbium co-doped optical fiber, combined with the non-circular stress zone design, the existing fiber core core large and low absorption rate are solved. The problem of improving the beam quality and output efficiency.

CN118938388APending Publication Date: 2024-11-12YANGTZE OPTICAL FIBRE & CABLE CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410853712.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-28
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing bias-maintaining erbium-ytterbium co-doped optical fibers have large core pore diameters, poor beam quality, high hole drilling and low absorption rate, which limits the fiber output power and pump absorption efficiency.

Method used

Using the structure of a quartz core layer co-doped by Er, Yb, and P, a Cl-doped quartz first cladding and a F-containing polyacrylic resin second cladding, it is deposited by chemical vapor deposition method and melted into an optical fiber at high temperature. Rods, process symmetrically distributed stress through holes, reduce interfacial stress and increase refractive index, avoid deposition of Ge/P co-doped base layer, and form non-circular stress regions to improve absorption efficiency.

Benefits of technology

It reduces the difficulty of core drilling, improves beam quality and pump light binding ability, enhances signal light output efficiency, and avoids core rupture and fiber output power limitation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118938388A_ABST
    Figure CN118938388A_ABST
Patent Text Reader

Abstract

The invention discloses a polarization-maintaining gain optical fiber. The optical fiber sequentially comprises a core layer, a first cladding layer and a second cladding layer from inside to outside, the fiber core is a quartz layer co-doped with Er, Yb and P; the first wrapping layer is a Cl-doped quartz layer; the second cladding is made of F-containing polyacrylic resin; wherein the refractive index n1 of the core layer, the refractive index n2 of the first cladding layer and the refractive index n3 of the second cladding layer are in step distribution, and the relationship that n1 > n2 > n3 is satisfied. A P and Ge co-doped base layer can be prevented from being deposited near a core layer, the punching difficulty of a stress area is reduced, meanwhile, good light beam quality and higher pump light binding capacity are guaranteed, and the pump light absorption efficiency is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of optical fiber products, and more specifically to a polarization-maintaining gain optical fiber and a method for preparing the polarization-maintaining gain optical fiber. Background Art

[0002] The research and application scenarios of polarization-maintaining Er-Yb co-doped optical fibers for linear polarization output are becoming increasingly important, especially as technologies such as fiber-optic LiDAR and laser weapons are advancing by leaps and bounds. High-precision LiDAR detection systems are expected to output linear polarization characteristics with better performance.

[0003] In order to achieve high-power output, the existing polarization-maintaining erbium-ytterbium co-doped optical fiber heavily dopes the core with ytterbium ions with a larger absorption cross section, so that it can act as a sensitizer to transfer power to the erbium ions. At the same time, the heavily doped rare earth ions need to be doped with a high concentration of phosphorus to prevent crystallization. However, the heavy doping of each element will inevitably lead to a very high numerical aperture of the core, resulting in too many modes of signal light and poor beam quality; and because the core is heavily doped with P and Yb elements, the stress generated at its interface is large, making it more difficult to drill holes in the polarization-maintaining erbium-ytterbium optical fiber than in general polarization-maintaining core rods, which can easily lead to the problem of core breakage during drilling. The current existing solution is to deposit a layer of P and Ge co-doped base layer on the edge of the core layer. The preparation of the base layer reduces the relative refractive index of the core layer and ensures the quality of the core layer beam. However, the base layer is also heavily doped with P and Ge, which further increases the stress in the core layer and its surrounding areas, further increasing the difficulty of drilling holes in the stress area.

[0004] At the same time, the absorption rate of the existing polarization-maintaining erbium-ytterbium co-doped optical fiber is not high, which results in the optical fiber being used for too long, which will cause the optical fiber output power to be limited and nonlinear effects to occur. Therefore, the optical fiber pump absorption efficiency is also a problem that needs to be addressed. Summary of the invention

[0005] In view of the above defects or improvement needs of the prior art, the present invention proposes a polarization-maintaining gain optical fiber and a preparation method thereof, which can avoid depositing a P and Ge co-doped base layer near the core layer, reduce the difficulty of drilling holes in the stress area, and ensure good beam quality and higher pump light binding ability, as well as improve the pump light absorption efficiency.

[0006] To achieve the above-mentioned purpose, an embodiment of the present invention provides a polarization-maintaining gain optical fiber, which includes a core layer, a first cladding layer, and a second cladding layer from the inside to the outside; the core is a quartz layer co-doped with Er, Yb, and P; the first cladding layer is a quartz layer doped with Cl; the second cladding layer is a polyacrylic resin containing F; wherein the refractive index n1 of the core layer, the refractive index n2 of the first cladding layer, and the refractive index n3 of the second cladding layer are step-distributed and satisfy the relationship n1>n2>n3.

[0007] In one embodiment of the present invention, the refractive index of the first cladding is in the range of 1.47 to 1.473; and / or the difference in refractive index between the core layer and the first cladding is in the range of 0.0025 to 0.0045; and / or the difference in refractive index between the first cladding and the second cladding is greater than 0.084.

[0008] In one embodiment of the present invention, two non-circular stress regions are symmetrically distributed in the first cladding with the fiber core as the center.

[0009] In one embodiment of the present invention, the difference in refractive index between the stress region and the first cladding layer ranges from -0.0247 to -0.0297.

[0010] In one embodiment of the present invention, the ratio of the distance from the center of the stress region to the center of the fiber core to the radius of the fiber core is in the range of 7-14.

[0011] In one embodiment of the present invention, the Cl concentration doped in the first cladding layer is 10-18 wt %.

[0012] In one embodiment of the present invention, the first cladding layer comprises a first Cl-doped layer close to the core layer and a second Cl-doped layer close to the second cladding layer, wherein the Cl concentration in the first Cl-doped layer is greater than that in the second Cl-doped layer.

[0013] In one embodiment of the present invention, the core layer is doped with Er2O3 at a concentration of 0.05-0.1 mol%, Yb2O3 at a concentration of 0.9-2 mol%, and P2O5 at a concentration of 10-17 mol%.

[0014] In addition, an embodiment of the present invention proposes a method for preparing a polarization-maintaining gain optical fiber as described in any of the above embodiments, comprising: depositing a Cl-doped liner tube by chemical vapor deposition; depositing a core layer in the Cl-containing liner tube by chemical vapor deposition, and melting and shrinking it into an optical fiber preform rod at high temperature after the deposition is completed; processing symmetrically distributed stress through holes on the optical fiber preform rod; preparing a B-doped stress rod, assembling it with the processed optical fiber preform rod, and using a drawing tower to draw it into a polarization-maintaining gain optical fiber of a target size.

[0015] In one embodiment of the present invention, before processing the symmetrically distributed stress through holes on the optical fiber preform, it also includes: processing a Cl-doped sleeve by chemical vapor deposition according to the size of the optical fiber preform, and inserting the optical fiber preform into the sleeve of corresponding size to pull or melt to obtain the required diameter ratio of the cladding and the core layer.

[0016] In general, the above technical solutions conceived by the present invention have at least one or more of the following beneficial effects compared with the prior art:

[0017] (1) The polarization-maintaining gain optical fiber provided has better material uniformity of the first cladding by doping Cl in the first cladding, thereby eliminating the interface stress of the first cladding caused by multi-layer doping, and also reducing the interface stress between the pure silica cladding and the core layer, making it easy to drill holes in the polarization-maintaining erbium-ytterbium co-doped optical fiber to avoid core breakage, and the Cl-doped first cladding increases the refractive index, and also ensures a small relative refractive index between the core layer and the first cladding, thereby reducing the numerical aperture of the core layer, making the signal light mode less or outputting a single mode, ensuring the beam quality, and avoiding the method of depositing a Ge / P co-doped base layer around the core to reduce the relative refractive index between the core layer and the first cladding, thereby reducing the size of the core layer and its vicinity, and further reducing the difficulty of optical fiber drilling;

[0018] (2) The refractive index of the first cladding is increased by doping with Cl, thereby also increasing the relative refractive index between the first cladding and the second cladding, making the pump light more confining and further avoiding the leakage of the cladding pump light;

[0019] (3) By setting the shape of the stress zone to be non-circular, compared with the circular stress zone, the non-circular stress zone has a better effect on breaking the pump helical light, which can further increase the absorption coefficient of the cladding and improve the signal light output efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 A schematic structural diagram of a polarization-maintaining gain optical fiber provided in an embodiment of the present invention;

[0021] Figure 2 A schematic structural diagram of another polarization-maintaining gain optical fiber provided in an embodiment of the present invention;

[0022] Figure 3 The present invention provides a flowchart of a method for preparing a polarization-maintaining gain optical fiber. DETAILED DESCRIPTION

[0023] It should be noted that, in the absence of conflict, the embodiments of the present invention and the features in the embodiments can be combined with each other. The present invention will be described below with reference to the accompanying drawings and in combination with the embodiments.

[0024] In order to enable ordinary technicians in the field to better understand the technical solution of the present invention, the technical solution in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments, and all should belong to the protection scope of the present invention.

[0025] It should be noted that the terms "first", "second", etc. in the specification and claims of the present invention and the above-mentioned drawings are applicable to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the terms used in this way can be interchangeable where appropriate, so that the embodiments of the present invention described herein can be implemented in an order other than those illustrated or described herein. In addition. The terms "including" and "having" and any variations thereof are intended to cover non-exclusive inclusions, for example, a process, method, system, product or device that includes a series of steps or units is not necessarily limited to those steps or units that are clearly listed, but may include other steps or units that are not clearly listed or are proprietary to these processes, methods, products or devices.

[0026] like Figure 1 As shown, an embodiment of the present invention proposes a polarization-maintaining gain optical fiber, for example, including a core layer, a first cladding layer, and a second cladding layer from the inside to the outside, wherein the refractive index n1 of the core is greater than the refractive index n2 of the first cladding layer, and the refractive index n2 of the first cladding layer is greater than the refractive index n3 of the second cladding layer, presenting a step-type distribution. The core layer matrix is ​​quartz, and its doping includes three elements: Er, Yb, and P. The first cladding layer is also a quartz matrix, and its doping element is Cl. The second cladding layer is a polyacrylic resin containing F. The refractive index refers to the ratio of the propagation speed of light in a certain medium to that in a vacuum. The relative refractive index of two media is the ratio of the propagation speed of light in the two media. For example, the relative refractive index expression of the core layer and the first cladding layer is n 21 =n2 / n1=sinr / sinβ, n2 is the refractive index of the core layer, n1 is the refractive index of the first cladding layer, r and β are the incident angle and refraction angle of light entering the first cladding layer from the core layer, respectively.

[0027] Furthermore, two stress zones are symmetrically distributed along the core in the first cladding, and the doping elements of the stress zones are B and P. As is known to all, the larger the size of the core layer and its vicinity, the higher the concentration of elements with large linear expansion coefficients such as Ge\P, the greater the internal stress of the core layer and its vicinity, and the difficulty of drilling holes in the stress zone will be very great. The present invention makes the material uniformity of the first cladding better by doping Cl in the first cladding, eliminates the interface stress of the first cladding caused by multi-layer doping, and also reduces the interface stress between the pure silicon cladding and the core layer, which can facilitate the drilling of optical fibers and avoid core rupture. In addition, the Cl-doped first cladding increases the refractive index, so that the core layer and the first cladding have a smaller relative refractive index, thereby reducing the numerical aperture of the core layer, making the signal light mode less or single-mode output, ensuring the beam quality, and avoiding the use of the prior art of depositing a Ge / P co-doped base layer around the core to reduce the relative refractive index between the core layer and the first cladding, thereby reducing the size of the core layer and its vicinity, and further reducing the difficulty of drilling holes.

[0028] Preferably, the refractive index of the first cladding is in the range of 1.47 to 1.473, and the difference in refractive index between the core layer and the first cladding is in the range of 0.0025 to 0.0045, which can achieve single-mode output of optical fiber with excellent beam quality and facilitate drilling of stress areas.

[0029] Furthermore, the refractive index difference between the first cladding and the second cladding is greater than 0.084. By increasing the refractive index of the first cladding, the relative refractive index between the first cladding and the second cladding is increased, so that the binding ability of the pump light is better and the leakage of the cladding pump light is further avoided.

[0030] Furthermore, two non-circular stress zones are symmetrically distributed in the first cladding with the core as the center. The shape of the stress zone is non-circular. Compared with the circular stress zone, when the area of ​​the non-circular stress zone is consistent with the area of ​​the circular stress zone, the effect of breaking the pump spiral light is better, and the cladding absorption coefficient is further increased, and the signal light output is improved. In addition, since the first cladding is doped with Cl, the difficulty of drilling the stress zone is reduced, which further promotes the processing of the non-circular stress zone.

[0031] It should be noted that the non-circular stress area can be Figure 1 The square shown in Figure 2 The octagon shown in FIG. 1 is not limited to this application.

[0032] Preferably, the difference in refractive index between the stress zone and the first cladding is in the range of -0.0247 to -0.0297. In one embodiment, the diameter of the core is between 4 and 50 μm, the diameter of the first cladding is between 125 and 700 μm, and the thickness of the F-doped second cladding is between 20 and 40 μm. The ratio of the distance from the center of the non-circular stress zone to the center of the core to the core radius is 7 to 14, which can avoid the stress zone being too close to the core to affect the fiber loss and the breakage of the erbium-doped core, and at the same time avoid the stress zone being too far from the core to reduce the core stress, thereby affecting the polarization maintaining performance. The area of ​​the non-circular stress zone is 785 to 26700 μm 2 The cross section of the first cladding is circular.

[0033] Preferably, the Cl concentration doped in the first cladding is 10-18wt%, which can achieve good beam quality and effectively reduce the difficulty of drilling holes in the stress zone. In particular, the first cladding can be doped with Cl at a uniform concentration or a non-uniform concentration. In one embodiment, the first cladding doped with Cl at a non-uniform concentration includes a first Cl-doped layer close to the core layer and a second Cl-doped layer close to the second cladding, wherein the Cl concentration doped in the first Cl-doped layer is greater than that in the second Cl-doped layer. A small relative refractive index between the core layer and the first Cl-doped layer can be ensured, thereby ensuring the beam quality. At the same time, the second Cl-doped layer has a lower Cl-doping concentration, which is more conducive to drilling holes in the stress zone.

[0034] In one embodiment, the Er2O3 concentration doped in the core layer is 0.05-0.1mol%, the Yb2O3 concentration is 0.9-2mol%, and the P2O5 concentration is 10-17mol%. The core is heavily doped with ytterbium ions with a larger absorption cross-section, so that it can transfer its ability to erbium ions as a sensitizer. At the same time, the heavy doping of rare earth ions requires the simultaneous doping of high concentrations of phosphorus elements to prevent crystallization from occurring and avoid affecting fiber loss and power output. However, the heavy doping of each element will inevitably lead to a very high numerical aperture of the core, resulting in too many modes of signal light and poor beam quality. The above-mentioned polarization-maintaining gain fiber proposed in this embodiment is suitable for solving this technical problem. The specific structure of the polarization-maintaining gain fiber and the functions it realizes are as described above and will not be described in detail here.

[0035] In addition, if Figure 3 As shown, an embodiment of the present invention further proposes a method for preparing a polarization-maintaining gain optical fiber, for example, comprising: step S1, depositing a Cl-doped liner tube by chemical vapor deposition; step S2, depositing a core layer in a Cl-containing liner tube by chemical vapor deposition, and melting and shrinking the core layer into an optical fiber preform rod at high temperature after the deposition is completed; step S3, processing symmetrically distributed stress through holes on the optical fiber preform rod; step S4, preparing a B-doped stress rod, assembling the rod with the processed optical fiber preform rod, and drawing the rod into a polarization-maintaining gain optical fiber of a target size by using a drawing tower.

[0036] Specifically, the Cl-doped first cladding is divided into two parts, the liner and the sleeve, or only the Cl-doped liner can be prepared according to the size of the optical fiber. In step S1, whether it is a Cl-doped liner or a sleeve for supplementing the cladding area, the preparation method adopted is the same, and the doping concentration is also the same. The blank is deposited by external vapor deposition, the blank is polished, and then stretched to the liner or sleeve of the target size through a stretching device. The liner and sleeve can be prepared in batches and retained for later use.

[0037] In step S2, the core layer may be deposited in the liner tube containing Cl by an in-tube vapor deposition method, including a plasma vapor deposition method and an improved chemical vapor deposition method.

[0038] In one embodiment, it can be selected whether to coat a Cl-doped sleeve outside the Cl-doped liner by stretching or melting according to the size of the optical fiber to ensure the diameter ratio of the cladding layer to the core layer.

[0039] In step S3, a B-doped stress rod is prepared by an in-tube vapor deposition method, including a plasma vapor deposition method and an improved chemical vapor deposition method, and then the pure silicon cladding is removed by polishing, etching and other methods. The core rod coated with the sleeve is then processed with stress through holes, and the stress is symmetrically distributed along the core. The stress through holes have various non-circular structures, such as octagonal, hexagonal, plum blossom, square or D-shaped. Finally, the stress rod is assembled with the processed sleeve and drawn into a polarization-maintaining gain fiber of the target size using a drawing tower. The polarization-maintaining gain fiber and its preparation method are described in detail below through specific embodiments:

[0040] Embodiment 1:

[0041] The polarization-maintaining gain optical fiber includes a core layer, a first cladding layer, and a second cladding layer from the inside to the outside, wherein the first cladding layer is a Cl-doped quartz layer, and the second cladding layer contains F-containing polyacrylic resin. The refractive indexes of the core, the first cladding layer, and the second cladding layer decrease in sequence and present a step-refractive index distribution. For example, the Er2O3 concentration of the core layer is set to 0.05mol%, the Yb2O3 concentration is set to 0.9mol%, the P2O5 concentration is set to 10mol%, and the Cl doping concentration in the cladding layer is set to 10wt%. The doping of the core layer and the cladding layer ensures that the refractive index of the first cladding layer is 1.47, the refractive index difference between the core layer and the first cladding layer is 0.0025, the refractive index difference between the first cladding layer and the second cladding layer is 0.084, the refractive index difference between the stress zone and the first cladding layer is -0.0247, the ratio of the distance from the center of the stress zone to the center of the core to the core radius is 14, and the area of ​​the stress zone is 785μm 2 The stress zone is square in shape. The core diameter is 4μm, and the first cladding diameter is 125μm.

[0042] Embodiment 2:

[0043] The polarization-maintaining gain optical fiber includes a core layer, a first cladding layer, and a second cladding layer from the inside to the outside, wherein the first cladding layer is a Cl-doped quartz layer, and the second cladding layer contains F-containing polyacrylic resin. The refractive indexes of the core, the first cladding layer, and the second cladding layer decrease in sequence and present a step-refractive index distribution. For example, the Er2O3 concentration of the core layer is set to 0.08 mol%, the Yb2O3 concentration is set to 1.1 mol%, the P2O5 concentration is set to 15 mol%, the Cl doping concentration in the cladding layer is set to 12 wt%, the doping of the core layer and the cladding layer ensures that the refractive index of the cladding layer is 1.472, the refractive index difference between the core layer and the first cladding layer is 0.003, the refractive index difference between the first cladding layer and the second cladding layer is 0.085, the refractive index difference between the stress zone and the first cladding layer is -0.0297, the ratio of the distance from the center of the stress zone to the center of the core to the core radius is 7, and the area of ​​the stress zone is 3140 μm2 The stress zone is square in shape. The core diameter is 25μm, and the first cladding diameter is 250μm.

[0044] Embodiment 3:

[0045] The polarization-maintaining gain optical fiber includes a core layer, a first cladding layer, and a second cladding layer from the inside to the outside, wherein the first cladding layer is a Cl-doped quartz layer, and the second cladding layer contains F-containing polyacrylic resin. The refractive indexes of the core, the first cladding layer, and the second cladding layer decrease in sequence and present a step-refractive index distribution. For example, the Er2O3 concentration of the core layer is set to 0.08 mol%, the Yb2O3 concentration is set to 1.2 mol%, the P2O5 concentration is set to 17 mol%, the Cl concentration doped in the cladding layer is set to 18 wt%, the doping of the core layer and the cladding layer ensures that the refractive index of the cladding layer is 1.473, the refractive index difference between the core layer and the first cladding layer is 0.0045, the refractive index difference between the first cladding layer and the second cladding layer is 0.085, the refractive index difference between the stress zone and the first cladding layer is -0.0297, the ratio of the distance from the center of the stress zone to the center of the core to the core radius is 7, and the area of ​​the stress zone is 785 μm 2 The stress zone is octagonal in shape. The core diameter is 10 μm, and the first cladding diameter is 125 μm.

[0046] Embodiment 4:

[0047] The polarization-maintaining gain optical fiber includes a core layer, a first cladding layer, and a second cladding layer from the inside to the outside, wherein the first cladding layer is a Cl-doped quartz layer, and the second cladding layer contains F-containing polyacrylic resin. The refractive indexes of the core, the first cladding layer, and the second cladding layer decrease in sequence and present a step-refractive index distribution. For example, the Er2O3 concentration in the core layer is set to 0.08 mol%, the Yb2O3 concentration is set to 1.1 mol%, the P2O5 concentration is set to 15 mol%, the Cl concentration doped in the cladding layer is set to 12 wt%, the doping of the core layer and the cladding layer ensures that the refractive index of the cladding layer is 1.472, the refractive index difference between the core layer and the first cladding layer is 0.003, the refractive index difference between the first cladding layer and the second cladding layer is 0.085, the refractive index difference between the stress zone and the first cladding layer is -0.0297, the ratio of the distance from the center of the stress zone to the center of the core to the core radius is 7, and the area of ​​the stress zone is 26700 μm 2 The stress zone is hexagonal in shape. The core diameter is 50μm, and the first cladding diameter is 700μm.

[0048] Embodiment 5:

[0049] The polarization-maintaining gain optical fiber includes a core layer, a first cladding layer, and a second cladding layer from the inside to the outside, wherein the first cladding layer is a non-uniformly Cl-doped quartz layer, and the second cladding layer contains F-containing polyacrylic resin. For example, the core Er2O3 concentration is set to 0.08 mol%, the Yb2O3 concentration is 1.1 mol%, and the P2O5 concentration is 15 mol%. The first cladding layer contains two Cl-doped layers, the first layer has a Cl doping concentration of 18 wt%, and the second layer has a Cl doping concentration of 10 wt%. The doping of the core layer and the cladding ensures that the refractive index of the cladding layer is 1.472, the refractive index difference between the core layer and the first cladding layer is 0.003, the refractive index difference between the first cladding layer and the second cladding layer is 0.085, the refractive index difference between the stress zone and the first cladding layer is -0.0267, the ratio of the distance from the center of the stress zone to the center of the core to the core radius is 7, and the area of ​​the stress zone is 785 μm 2 The stress zone is square in shape. The core diameter is 10μm, the first cladding layer has a diameter of 25μm, and the second cladding layer has a diameter of 125μm.

[0050] The polarization-maintaining gain optical fiber designed above is prepared as follows:

[0051] Step 1: Install the cleaned target rod on the synchronous chuck of the horizontal OVD lathe, heat and deposit the target rod with an oxyhydrogen flame, control the hydrogen flow rate of the oxyhydrogen flame to 80-160slm, control the oxygen flow rate to 45-120slm, and control the ratio of hydrogen to oxygen to 1.5:1-2:1. After the target rod is deposited, SiCl4 is introduced for hydrolysis to produce powder rods, with a deposition rate of 100-200g / min and a target rod rotation speed of 5-10rpm / min. After the powder rod is cooled, the powder rod is extracted from the target rod and dehydrated, and 1-1.5L / min SiCl4 and 0.5-1L / min He are introduced for dehydration, with a dehydration temperature of 1050-1100℃, and then sintered at 1400℃-1600℃ to form a transparent chlorine-containing insulating glass. The insulating glass is then stretched and cold-processed into a Cl-containing sleeve or liner of target size and doping concentration.

[0052] Step 2: Select the Cl-doped liner tube of the corresponding size in step 1, install it on the MCVD lathe for core layer deposition, use the chelate vapor deposition method, transfer the rare earth raw materials of the chelate to the deposition tube after high-temperature evaporation, and introduce the corresponding phosphorus oxychloride, silicon tetrachloride, oxygen, helium and other gases to participate in the reaction, forming a multi-doped, highly doped core layer deposition layer. The flow rate of phosphorus oxychloride is 200sccm, oxygen is 1000sccm, helium is 500sccm, rare earth chelate is 400-600sccm, aluminum chloride is 10-50sccm, the temperature is 1400-1600℃, and the main lamp speed is 120mm / min.

[0053] Step 3: After the core layer is deposited, it is melted and shrunk at a high temperature of 1900-2100°C to melt the hollow deposition tube into a solid preform rod;

[0054] Step 4: insert the optical fiber preform into a chlorine-containing casing of target size for melting and shrinking to meet the target core-to-shell ratio. The chlorine content of the casing and the liner can be the same or different.

[0055] Step 5: Process the combined rod in step 4 with a double symmetrical circular base hole on the outside of the core rod along the axial direction of the optical fiber mother rod, and then carve out stress zone shapes of different shapes based on the base hole, which can be square, hexagonal, etc.

[0056] Step six: Install a conventional liner on a PCVD deposition lathe to prepare stress rods, with a deposition rate of 0.5-2.5 g / min, a boron chloride flow rate of 50-500 sccm, phosphorus oxychloride of 50-250 sccm, an oxygen-silicon ratio of 3-4, a resonant cavity power of 1500-4500 W, and then sinter at high temperature to form a glass rod containing a B and P core. The glass rod is then subjected to external cylindrical grinding to remove the pure silicon cladding, leaving only the glass core containing B and P.

[0057] Step 7: Combine the punched combination rod from step 5 with the circular stress rod from step 6, and perform high-temperature drawing. When the high-temperature furnace of the drawing tower is heated, the stress rod will melt first and fill the entire non-circular through hole due to its low melting point. During the drawing process, a second cladding layer will be coated, and the target polarization-maintaining gain fiber will be finally drawn.

[0058] Typical examples and comparative examples are summarized in the following table:

[0059]

[0060]

[0061] It can be seen from the embodiments and comparative examples in the table that the optical fiber without Cl-doped first cladding will result in a large refractive difference between the core layer and the first cladding, the optical fiber is no longer a single-mode optical fiber, the beam quality will deteriorate rapidly, the stress zone will be circular, and the cladding absorption coefficient will be smaller than that of Example 2.

[0062] In summary, the polarization-maintaining gain optical fiber and its preparation method proposed in the embodiment of the present application dope Cl in the first cladding to make the material uniformity of the first cladding better, eliminate the interface stress of the first cladding caused by multi-layer doping, and also reduce the interface stress between the pure silicon cladding and the core layer, which can avoid depositing a thick highly doped Ge / P co-doped base layer around the core to reduce the relative refractive index of the core layer, thereby reducing the size of the core layer and its vicinity, greatly reducing the difficulty of drilling, and the Cl-doped first cladding increases the refractive index, and also ensures a small relative refractive index of the core layer, reduces the numerical aperture of the core layer, and can make the signal light mode less or single-mode output, thereby ensuring the beam quality; by doping Cl to increase the refractive index of the first cladding, thereby also increasing the relative refractive index difference between the first cladding and the second cladding, so that the binding ability of the pump light is better, and the leakage of the cladding pump light is further avoided; by setting the shape of the stress zone to be non-circular, compared with the circular stress zone, the non-circular stress zone has a better effect on breaking the pump spiral light, which can further increase the absorption coefficient of the cladding and improve the signal light output efficiency.

[0063] The above is only an exemplary embodiment of the present disclosure, and the scope of the present disclosure cannot be limited thereto. That is, any equivalent changes and modifications made according to the teachings of the present disclosure are still within the scope of the present disclosure. After considering the specification and practicing the disclosure here, those skilled in the art will easily think of the implementation scheme of the present disclosure. The present invention is intended to cover any variation, use or adaptive change of the present disclosure, which follows the general principles of the present disclosure and includes common knowledge or customary technical means in the technical field not recorded in the present disclosure. The description and examples are regarded as exemplary only, and the scope and spirit of the present disclosure are defined by the claims.

[0064] The technical features of the above embodiments may be combined arbitrarily. To make the description concise, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0065] It will be easily understood by those skilled in the art that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A polarization-maintaining gain optical fiber, characterized in that: The optical fiber includes a core layer, a first cladding layer, and a second cladding layer from the inside to the outside; The fiber core is a quartz layer co-doped with Er, Yb and P; The first cladding layer is a Cl-doped quartz layer; The second cladding layer is a polyacrylic acid resin containing F; The refractive index n1 of the core layer, the refractive index n2 of the first cladding layer, and the refractive index n3 of the second cladding layer are in step distribution and satisfy the relationship n1>n2>n3.

2. The polarization-maintaining gain optical fiber according to claim 1, characterized in that: The refractive index of the first cladding is in the range of 1.47 to 1.473; and / or the refractive index difference between the core layer and the first cladding is in the range of 0.0025 to 0.0045; and / or the refractive index difference between the first cladding and the second cladding is greater than 0.

084.

3. The polarization-maintaining gain optical fiber according to claim 1, characterized in that: Two non-circular stress regions are symmetrically distributed in the first cladding with the fiber core as the center.

4. The polarization-maintaining gain optical fiber according to claim 3, characterized in that: The difference in refractive index between the stress region and the first cladding layer ranges from -0.0247 to -0.0297.

5. The polarization-maintaining gain optical fiber according to claim 3, characterized in that: The ratio of the distance from the center of the stress area to the center of the fiber core to the radius of the fiber core is in the range of 7-14.

6. The polarization-maintaining gain optical fiber according to claim 1, characterized in that: The Cl concentration doped in the first cladding layer is 10-18 wt%.

7. The polarization-maintaining gain optical fiber according to claim 6, characterized in that: The first cladding layer comprises a first Cl-doped layer close to the core layer and a second Cl-doped layer close to the second cladding layer, wherein the Cl concentration in the first Cl-doped layer is greater than that in the second Cl-doped layer.

8. The polarization-maintaining gain optical fiber according to claim 1, characterized in that: The core layer is doped with Er2O3 at a concentration of 0.05-0.1 mol%, Yb2O3 at a concentration of 0.9-2 mol%, and P2O5 at a concentration of 10-17 mol%.

9. A method for preparing a polarization-maintaining gain optical fiber according to any one of claims 1 to 8, characterized in that: include: The Cl-doped liner was deposited by chemical vapor deposition; The core layer is deposited in a Cl-containing liner by chemical vapor deposition, and after the deposition is completed, it is melted and shrunk at high temperature to form an optical fiber preform; Processing symmetrically distributed stress through holes on the optical fiber preform; A B-doped stress rod is prepared and assembled with the processed optical fiber preform rod, and then drawn into the polarization-maintaining gain optical fiber of target size by using a drawing tower.

10. The method for preparing a polarization-maintaining gain optical fiber according to claim 9, characterized in that: Before processing the symmetrically distributed stress through holes on the optical fiber preform, the method further comprises: According to the size of the optical fiber preform, a Cl-doped sleeve is processed by chemical vapor deposition, and the optical fiber preform is inserted into the sleeve of corresponding size for stretching or melting to obtain the required diameter ratio of the cladding layer to the core layer.