Photoresist for C-HJT battery manufacturing process

By using ternary photosensitive styrene-maleic anhydride-styrene sulfonate modified resin as a photoresist for polymer adhesive, the problem of low preparation accuracy of copper gate electrodes in C-HJT batteries was solved, and the problem of low production accuracy of copper gate electrodes in C-HJT batteries was achieved. The fast development speed, good curing rate and good electroplating resistance improve production efficiency and reduce costs.

CN118938602APending Publication Date: 2024-11-12SHIMING (LIAONING) NEW MATERIAL CO LTD +1
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411037196.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

During the preparation process of copper gate electrodes in C-HJT batteries, the dry film cost is high and the preparation accuracy is low, resulting in low production efficiency and yield. A photoresist that is fast cured and developed is needed to replace the dry film and improve the copper gate. Preparation accuracy of electrodes.

Method used

A photolithography used for C-HJT battery process was prepared by using polymeric binder as ternary photosensitive styrene-maleic anhydride-styrene sulfonate modified resin, combined with photopolymerization monomer and photoinitiator. The glue has the characteristics of strong hydrophilicity, fast development speed and good curing rate, and improves the performance of permeability.

Benefits of technology

The development speed is improved, the exposure energy demand is reduced, and the production efficiency is improved. The penetration resistance plating performance in the copper electroplating process is improved through high Tg monomers, solving the problem of high raw material costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004971412530000031
    Figure BDA0004971412530000031
  • Figure BDA0004971412530000061
    Figure BDA0004971412530000061
  • Figure FDA0004971412520000011
    Figure FDA0004971412520000011
Patent Text Reader

Abstract

The invention discloses a photoresist for a C-HJT battery manufacturing process, which comprises the following components in parts by weight: 50-80 parts of a polymer adhesive, 20-40 parts of a photopolymerization monomer and 3-5 parts of a photoinitiator, the photopolymerization monomer has an acryloyloxy unsaturated functional group, and the polymer adhesive is a ternary photosensitive styrene-maleic anhydride-sodium p-styrenesulfonate modified resin or a mixture containing the ternary photosensitive styrene-maleic anhydride-sodium p-styrenesulfonate modified resin. The photoresist has the characteristics of high hydrophilicity, high developing speed, good curing rate and the like, and the diffusion plating resistance in a copper electroplating process after exposure can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of photoresists for batteries, and in particular to a photoresist used in a C-HJT battery manufacturing process. Background Art

[0002] HJT cells, also known as heterojunction cells, are a type of N-type cells. They are a high-efficiency crystalline silicon solar cell structure, which is made of crystalline silicon substrates and amorphous silicon thin films, that is, a layer of non-doped (intrinsic) hydrogenated amorphous silicon thin film is added between P-type hydrogenated amorphous silicon and N-type hydrogenated amorphous silicon and the N-type silicon substrate. Heterojunction cells are a new type of cell based on the photovoltaic effect. Due to their unique double-sided symmetrical structure and excellent passivation effect of the amorphous silicon layer, they have the advantages of high conversion efficiency, high bifaciality, almost no light-induced degradation, good temperature characteristics, the use of thin silicon wafers, and the ability to stack perovskites. At the same time, their manufacturing process is relatively short and will be more popular in the future. After the application of heterojunction cell technology in the photovoltaic field, the conversion efficiency of photovoltaic cells has increased from 22.3% to 28%, that is, the annual power generation of power stations with the same floor area has increased by about 7.6%. At the same time, heterojunction technology not only has excellent conversion efficiency, but also has relatively simple production process steps.

[0003] Heterojunction solar cells generally use resin-type low-temperature curing silver paste as the metal electrode, which has high resistivity and poor conductivity. In order to improve the conductivity, the width or height of the metal electrode needs to be increased, which in turn leads to an increase in the silver paste consumption of the battery. The silver consumption of a single piece is 2.62 times that of the previous PERC battery. With the emergence of the C-HJT (copper grid heterojunction battery) process, copper grid electrodes are used to replace traditional silver grid electrodes, thereby achieving the purpose of reducing costs. However, the preparation of copper grids currently usually uses dry films, and the dry films are formed into electrode grids through lamination, exposure, tearing, development, and electroplating. The cost of dry films is high, and the precision of the prepared grid lines is low. Therefore, there is an urgent need for a fast-curing and fast-developing photoresist to replace the dry film and carry out the C-HJT copper grid electrode process, effectively improving the preparation precision of the grid lines, thereby improving the production efficiency and yield of heterojunction solar cells. Summary of the invention

[0004] In order to solve the above technical problems, the purpose of the present invention is to provide a photoresist for C-HJT battery process, which has the characteristics of strong hydrophilicity, fast development speed, good curing rate, etc., and can improve the resistance to permeation plating in the copper electroplating process after exposure.

[0005] In order to achieve the above technical objectives and the above technical effects, the present invention is implemented through the following technical solutions:

[0006] A photoresist for C-HJT battery process comprises the following components in parts by weight: 50-80 parts of polymer adhesive, 20-40 parts of photopolymer monomer, and 3-5 parts of photoinitiator; the photopolymer monomer has an acryloxy type unsaturated functional group, and the polymer adhesive is a ternary photosensitive styrene-maleic anhydride-sodium styrene sulfonate modified resin.

[0007] Furthermore, the weight average molecular weight of the ternary photosensitive styrene-maleic anhydride-sodium styrene sulfonate modified resin is 5000-20000.

[0008] Furthermore, the ternary photosensitive styrene-maleic anhydride-sodium styrene sulfonate modified resin is one of the following structural formulas:

[0009]

[0010] Wherein, m, n, and p are integers between 1 and 100, and R is H or CH3. Specifically, the resin structure is one of poly(styrene-maleic anhydride-sodium styrene sulfonate) grafted with hydroxyethyl (meth)acrylate, pentaerythritol tri(meth)acrylate, and dipentaerythritol penta(meth)acrylate.

[0011] The preparation method of the polymer modified by terphenylethylene, maleic anhydride and sodium styrene sulfonate is as follows:

[0012] Dissolve three monomers (200 parts in total) of styrene / maleic anhydride / sodium 4-vinylbenzenesulfonate in 100 parts of propylene glycol methyl ether acetate (PMA) to prepare a monomer solution, add 3-5% initiator of the total weight of the monomer to the monomer solution, and the initiator is mainly selected from azobisisobutylnitrile or benzoyl peroxide. Prime with 100 parts of PMA solvent, control the reaction temperature at 80-100°C, drip the monomer for 2-3 hours, keep warm for 1 hour, add esterification catalyst triphenylphosphine 1% (total monomer amount) and 0.1% methoxyphenol (inhibitor, total monomer amount), add one of (meth) hydroxyethyl acrylate, pentaerythritol tri(meth) acrylate, dipentaerythritol penta(meth) acrylate within 10 minutes, the molar ratio of the molar number to maleic anhydride is 1.05:1, the reaction time is 5-6 hours, the temperature is maintained at 80-90°C, and after the reaction is completed, cool down to room temperature under stirring to obtain a photoresist resin solution.

[0013] Furthermore, the photopolymerizable monomer includes at least one of pentaerythritol tetraacrylate, di-trimethylolpropane tetraacrylate, and dipentaerythritol hexaacrylate.

[0014] Furthermore, the photoinitiator is one or a combination of two or more of α-hydroxyketone derivatives (1173, 184), α-aminoketone derivatives (907, 369), and thioxanthone derivatives (ITX).

[0015] Furthermore, the photoresist also contains one or more of a crosslinking agent, a leveling agent, a surfactant, an inhibitor, a stabilizer, a dispersant, a plasticizer, and a dye.

[0016] The beneficial effects of the present invention are:

[0017] The present invention adopts a photosensitive terpolymer of styrene-maleic anhydride-sodium styrene sulfonate as a polymer binder. The sodium styrene sulfonate contains a sodium sulfonate group and exhibits excellent hydrophilicity, which can improve the development speed of the non-exposed area of ​​the photoresist. The anhydride group of the maleic anhydride can be ring-opened with a hydroxyl-containing photosensitive monomer to obtain a photosensitive group by grafting. The styrene monomer has a relatively high Tg, which can improve the anti-plating performance of the exposed area in the copper electroplating process after exposure.

[0018] The present invention adopts photosensitive terphenylene-maleic anhydride-sodium styrene sulfonate modified polymer as polymer adhesive, and can control the monomer ratio and polymerization degree during copolymerization of terphenylene-maleic anhydride-sodium styrene sulfonate, so as to realize the regulation of development speed under different acid values. In the photosensitive terphenylene-maleic anhydride-sodium styrene sulfonate modified polymer, terphenylene-maleic anhydride-sodium styrene sulfonate is grafted with photosensitive groups (the number of photosensitive groups can also be regulated), and a photopolymerization monomer containing a multifunctional group is matched at the same time, so that the exposure speed is excellent during the curing process, the exposure energy requirement is extremely low, and the production efficiency is improved while saving energy. The presence of carboxyl and sulfonate groups in the polymer can improve the development speed and resolution, and on the other hand, the presence of high Tg monomer styrene improves the resistance to permeation plating in the copper electroplating process after exposure; the main monomers used in the present invention are styrene, maleic anhydride, and sodium styrene sulfonate, and the three monomers have high cost performance, which solves the problem of cost reduction of raw materials in the photovoltaic cell market that is currently the most urgent to be solved. DETAILED DESCRIPTION

[0019] The technical solutions in the present invention will be described clearly and completely below in conjunction with specific embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0020] The present invention provides a photoresist for C-HJT battery process, which comprises the following components in parts by weight: 50-80 parts of a polymer binder, 20-40 parts of a photopolymerizable monomer, and 3-5 parts of a photoinitiator; the photopolymerizable monomer has an acryloxy-type unsaturated functional group, and the polymer binder is a ternary photosensitive styrene-maleic anhydride-sodium styrene sulfonate modified resin or a mixture containing the ternary photosensitive styrene-maleic anhydride-sodium styrene sulfonate modified resin.

[0021] The weight average molecular weight of the ternary photosensitive styrene-maleic anhydride-sodium styrene sulfonate modified resin is 5000-20000.

[0022] The ternary photosensitive styrene-maleic anhydride-sodium styrene sulfonate modified resin is one of the following structural formulas:

[0023]

[0024] Wherein, m, n, and p are integers between 1 and 100, and R is H or CH3. Specifically, the resin structure is one of poly(styrene-maleic anhydride-sodium styrene sulfonate) grafted with hydroxyethyl (meth)acrylate, pentaerythritol tri(meth)acrylate, and dipentaerythritol penta(meth)acrylate.

[0025] The preparation method of the polymer modified by terphenylethylene, maleic anhydride and sodium styrene sulfonate is as follows:

[0026] Dissolve three monomers (200 parts in total) of styrene / maleic anhydride / sodium 4-vinylbenzenesulfonate in 100 parts of propylene glycol methyl ether acetate (PMA) to prepare a monomer solution, add 3-5% initiator of the total weight of the monomer to the monomer solution, and the initiator is mainly selected from azobisisobutylnitrile or benzoyl peroxide. Prime with 100 parts of PMA solvent, control the reaction temperature at 80-100°C, drip the monomer for 2-3 hours, keep warm for 1 hour, add esterification catalyst triphenylphosphine 1% (total monomer amount) and 0.1% methoxyphenol (inhibitor, total monomer amount), add one of (meth) hydroxyethyl acrylate, pentaerythritol tri(meth) acrylate, dipentaerythritol penta(meth) acrylate within 10 minutes, the molar ratio of the molar number to maleic anhydride is 1.05:1, the reaction time is 5-6 hours, the temperature is maintained at 80-90°C, and after the reaction is completed, cool down to room temperature under stirring to obtain a photoresist resin solution.

[0027] The photopolymerizable monomer includes at least one of pentaerythritol tetraacrylate, di-trimethylolpropane tetraacrylate and dipentaerythritol hexaacrylate.

[0028] The photoinitiator is preferably one or a combination of two or more of α-hydroxyketone derivatives (1173, 184), α-aminoketone derivatives (907, 369), and thioxanthone derivatives (ITX).

[0029] The photoresist further comprises one or more of a crosslinking agent, a leveling agent, a surfactant, an inhibitor, a stabilizer, a dispersant, a plasticizer, and a dye.

[0030] The present invention is further described in detail below through specific examples.

[0031] Example 1

[0032] 1. Preparation of polymer adhesive

[0033] 50g of styrene, 50g of maleic anhydride, 100g of sodium 4-vinylbenzenesulfonate, and 6g of azobisisobutyronitrile were added to 100g of propylene glycol methyl ether acetate (PMA), and stirred for 1 hour to prepare a monomer solution. 100g of PMA was added to a three-necked flask, and the temperature was raised to 80°C. The monomer solution was added dropwise, and the dropping rate was controlled to be completed within 2 hours. The mixture was kept warm for 1 hour, and 2g of triphenylphosphine and 0.2g of 0.1% methoxyphenol were added. Subsequently, 62g of hydroxyethyl acrylate was added within 10 minutes. The mixture was reacted at 80°C for 5 hours, and stirred and cooled to room temperature to obtain a polymer adhesive A1.

[0034] 2. Preparation of photoresist for C-HJT cell process

[0035] 150 g of A1, 80 g of pentaerythritol tetraacrylate, 6 g of photoinitiator 907, 4 g of ITX, 1 g of silane coupling agent, and 2 g of polymerization inhibitor pyrogallol were mixed and stirred evenly, and filtered through a 0.5 μm filter to obtain photoresist A-1.

[0036] Example 2.

[0037] 1. Preparation of polymer adhesive

[0038] 50g of styrene, 50g of maleic anhydride, 100g of sodium 4-vinylbenzenesulfonate, and 6g of azobisisobutyronitrile were added to 100g of propylene glycol methyl ether acetate (PMA), and stirred for 1 hour to prepare a monomer solution. 100g of PMA was added to a three-necked flask, and the temperature was raised to 80°C. The monomer solution was added dropwise, and the dropping rate was controlled to be completed within 2 hours. The mixture was kept warm for 1 hour, and 2g of triphenylphosphine and 0.2g of 0.1% methoxyphenol were added. Subsequently, 159.6g of pentaerythritol triacrylate was added within 10 minutes. The mixture was reacted at 80°C for 5 hours, and stirred and cooled to room temperature to obtain a polymer adhesive A2.

[0039] 2. Preparation of photoresist for C-HJT cell process

[0040] 160 g of A2, 80 g of di-trimethylolpropane tetraacrylate, 10 g of initiator 184, 1 g of silane coupling agent, and 2 g of inhibitor p-cresol were mixed and stirred evenly, and filtered through a 0.5 μm filter to obtain photoresist A-2.

[0041] Example 3.

[0042] 1. Preparation of polymer adhesive

[0043] 50g of styrene, 50g of maleic anhydride, 100g of sodium 4-vinylbenzenesulfonate, and 6g of azobisisobutyronitrile were added to 100g of propylene glycol methyl ether acetate (PMA), and stirred for 1 hour to prepare a monomer solution. 100g of PMA was added to a three-necked flask, and the temperature was raised to 80°C. The monomer solution was added dropwise, and the dropping rate was controlled to be completed within 2 hours. The mixture was kept warm for 1 hour, and 2g of triphenylphosphine and 0.2g of 0.1% methoxyphenol were added. Subsequently, 280g of dipentaerythritol pentaacrylate was added within 10 minutes, and the mixture was reacted at 80°C for 5 hours. The mixture was stirred and cooled to room temperature to obtain a polymer adhesive A3.

[0044] 2. Preparation of photoresist for C-HJT cell process

[0045] 150 g A3, 80 g dipentaerythritol hexaacrylate, 6 g photoinitiator 369, 4 g ITX, 1 g silane coupling agent, and 2 g pyrogallol were mixed and stirred evenly, and filtered through a 0.5 μm filter to obtain photoresist A-3.

[0046] Comparative Example 1

[0047] 100 g of commercially available modified acrylic resin (ETERCURE 6071 from Changxing Chemical, molecular weight 7000), 80 g of pentaerythritol tetraacrylate, 10 g of acetophenone, 1 g of silane coupling agent, and 2 g of pyrogallol were mixed and stirred uniformly, and filtered using a 0.5 μm filter to obtain photoresist B-1.

[0048] The above-mentioned photoresist was processed as follows to make C-HJT cell samples A-1, A-2, A-3, and B for performance testing.

[0049] Production of battery samples: The photoresist was coated on the C-HJT battery substrate with the copper seed layer by an automatic screen printing coater, and the coating thickness was controlled to be 13μm. The coated battery was put into an oven at 90℃ for 3 minutes. After drying, the battery substrates A-1, A-2, A-3, and B were tested for the following performances:

[0050] ① High sensitivity and developability: Place a 21-level light gradient ruler on the substrate and expose it with an LDI exposure machine at 20mJ energy. After exposure, use a conventional developing method (the developer is a 1% sodium carbonate aqueous solution, the developing temperature is 30°C, and the spray pressure of the developer is 1.2kg / cm2) to develop for one minute. Clean the substrate with deionized water and blow dry with hot air. Visually inspect the number of photoresist grids left on the light gradient ruler on the substrate. If seven grids are full, it means that the photoresist is completely cured at 20mJ energy. At the same time, judge the developability of the photoresist.

[0051] Evaluation criteria: seven or more photoresist grids indicate high sensitivity; clean exposed copper seed layer indicates good quality; slight white haze on the copper seed layer indicates poor quality. The results are listed in Table 1.

[0052] ② High resolution: Use LDI exposure machine (Xingji Micro Exposure Machine) at 20mJ energy to produce a 15μm opening grid line image, then develop it, and observe whether the opening grid line is clear after development.

[0053] Evaluation criteria: clear opening lines are excellent; slight burrs on the opening edges are good; unclear opening lines are poor; the results are listed in Table 1.

[0054] ③Electroplating resistance: The battery substrate for the gate line is horizontally plated, and the plating layer on the open gate line should reach a thickness of 15-20μm. After plating, observe whether the photoresist layer in the unplated area is corroded by the plating solution.

[0055] The test results are shown in Table 1:

[0056] Table 1

[0057] Battery substrate Substrate A-1 Substrate A-2 Substrate A-3 Substrate B Exposure energy mJ 5 grid 6 grid 7 grid 3 grids Development excellent excellent excellent Difference Development time 30S 50S 75S 120S Resolution / μm 15 15 20 35 Resistant to electroplating good excellent excellent Difference

[0058] From the above, it can be seen that the photoresist of the present invention has a fast developing speed, a good curing rate and good electroplating resistance.

[0059] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above and that the present invention can be implemented in other specific forms without departing from the spirit or essential features of the present invention. Therefore, the embodiments should be considered exemplary and non-restrictive in all respects, and the scope of the present invention is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims be included in the present invention.

[0060] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.

Claims

1. A photoresist for C-HJT battery process, characterized in that: The invention comprises the following components in parts by weight: 50-80 parts of polymer adhesive, 20-40 parts of photopolymerizable monomer and 3-5 parts of photoinitiator; the photopolymerizable monomer has an acryloxy-type unsaturated functional group, and the polymer adhesive is a ternary photosensitive styrene-maleic anhydride-sodium styrene sulfonate modified resin.

2. A photoresist for C-HJT battery process according to claim 1, characterized in that: The weight average molecular weight of the ternary photosensitive styrene-maleic anhydride-sodium styrene sulfonate modified resin is 5000-20000.

3. The photoresist for C-HJT battery process according to claim 1, characterized in that: The structure of the ternary photosensitive styrene-maleic anhydride-sodium styrene sulfonate modified resin is one of poly(styrene-maleic anhydride-sodium styrene sulfonate) grafted with hydroxyethyl (meth)acrylate, pentaerythritol tri(meth)acrylate, and dipentaerythritol penta(meth)acrylate, which is one of the following general structural formulas: Wherein, m, n, and p are integers between 1 and 100, and R is H or CH3.

4. The photoresist for C-HJT battery process according to claim 1, characterized in that: The photopolymerizable monomer includes at least one of pentaerythritol tetraacrylate, di-trimethylolpropane tetraacrylate and dipentaerythritol hexaacrylate.

5. The photoresist for C-HJT battery process according to claim 1, characterized in that: The photoinitiator is at least one of α-hydroxyketone derivatives, α-aminoketone derivatives and thioxanthone derivatives.

6. The photoresist for C-HJT battery process according to claim 1, characterized in that: It also contains one or more of a cross-linking agent, a leveling agent, a surfactant, an inhibitor, a stabilizer, a dispersant, a plasticizer, and a colorant.

Citation Information

Cited By

  • High-resolution photoresist composition and preparation method thereof

    CN122043865A