Method and system for manufacturing vertical conductive adhesive for IC (integrated circuit) test

By using multi-layer stacking and silk-printing technology to make vertical conductive adhesives in semiconductor testing, the problems of low efficiency and poor quality of conductive adhesives in the existing technology are solved, and efficient and low-cost conductive adhesive production is achieved, suitable for semiconductor packaging testing. .

CN118942796AInactive Publication Date: 2024-11-12苏州微飞半导体有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411004572.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

In the prior art, the vertical conductive adhesive production process is low and the quality is poor during semiconductor testing, resulting in high costs. Traditional soldering and ACF processes are limited, which cannot effectively solve the problem of large chip size and warping, affecting the packaging test efficiency.

Method used

Using a vertical conductive adhesive production method, by making silk screen templates, including templates No. 1 and No. 2, combined with high elastic special silicone rubber and conductive adhesive, multi-layer stacking and cutting at room temperature is used to form a predetermined thickness. Vertical conductive adhesive layer and polished with glue surface to ensure flatness and connection quality.

Benefits of technology

It improves the quality and efficiency of the conductive adhesive layer, reduces production costs, realizes batch and automated production, simplifies the maintenance and replacement process, and solves the problems of deformation and poor flatness of components to be tested.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118942796A_ABST
    Figure CN118942796A_ABST
Patent Text Reader

Abstract

The invention provides a vertical conductive adhesive manufacturing method and a vertical conductive adhesive manufacturing system for IC (integrated circuit) testing. The vertical conductive adhesive manufacturing method comprises the steps that silk-screen templates are manufactured according to task demand information, and the silk-screen templates comprise the first silk-screen template and the second silk-screen template; laying a basic adhesive film on the operation base station; assembling a first silk-screen template and a conductive adhesive layer and an isolation adhesive film corresponding to the first silk-screen template on the operation base platform on which the basic adhesive film is laid; assembling a second silk-screen template and a conductive adhesive layer and an isolation adhesive film corresponding to the second silk-screen template on the first silk-screen template and the isolation adhesive film corresponding to the first silk-screen template; repeating the steps until a predetermined thickness required in the task demand information is reached, and forming a vertical conductive adhesive layer according with the predetermined thickness; and cutting the vertical conductive adhesive layer with the preset thickness and polishing the adhesive surface. The vertical conductive adhesive system corresponding to the vertical conductive adhesive manufacturing method comprises a basic adhesive film, a first silk-screen template group and a second silk-screen template group.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention provides a method and system for making vertical conductive adhesive for IC testing, belonging to the technical field of testing before chip and semiconductor packaging. Background Art

[0002] At present, semiconductor manufacturing in the market is mainly divided into 8 steps, namely wafer processing, oxidation, lithography, etching, thin film deposition, interconnection, testing, and packaging. Semiconductor testing is an important step in the semiconductor design, production, packaging, and testing process. It is a process of using specific instruments to detect the devices to be inspected, distinguish defects, verify whether the devices meet the design goals, and separate good products from bad products. The tests experienced in the chip production process are mainly divided into design verification, process monitoring test, wafer test, finished product test, reliability test, and user test.

[0003] Finished product testing, or package testing, is the testing of packaged chips. The chip is tested for performance and function by piercing the chip pins with the probe card, and defective chips are screened out before packaging. Among them, the probe card is the core consumable in the chip testing process. The most commonly used in the market is the spring probe. The quality of this probe is mainly reflected in the structure, material, coating, spring, sleeve accuracy and assembly manufacturing process. It is monopolized by foreign countries. The import cost of each probe is tens of RMB, and the number of probes arranged on a probe card can reach hundreds or even thousands. Therefore, the cost of the entire testing process is very high, which has become one of the obstacles in the development of my country's semiconductor technology; at the same time, the traditional soldering and ACF processes are subject to certain limitations. For example, the chip size is too large, the chip itself has a certain warping, and it cannot be effectively bonded with the end of the probe and the carrier board, which leads to a significant reduction in efficiency during the packaging test process. Summary of the invention

[0004] The present invention provides a method and system for manufacturing vertical conductive adhesive for IC testing, which is used to solve the problems of low efficiency and poor quality of the vertical conductive adhesive manufacturing process in the prior art. The technical solutions adopted are as follows:

[0005] A method for making a vertical conductive adhesive for IC testing, the method comprising:

[0006] Step 1: Prepare a silk screen template according to task requirement information, wherein the silk screen template includes silk screen template No. 1 and silk screen template No. 2;

[0007] Step 2: Lay the base film on the operating base;

[0008] Step 3: After the base film is laid, assemble the No. 1 screen printing template and its corresponding conductive adhesive layer and isolation adhesive film on the operating base;

[0009] Step 4, assembling the No. 2 silk screen template and its corresponding conductive adhesive layer and isolation adhesive film on the No. 1 silk screen template and its corresponding isolation adhesive film;

[0010] Step 5, repeating steps 3 and 4 until the predetermined thickness required in the task requirement information is reached, forming a vertical conductive adhesive layer that meets the predetermined thickness;

[0011] Step 6: Cut and polish the vertical conductive adhesive layer that meets the predetermined thickness.

[0012] Furthermore, a silk-screen template is produced according to the task requirement information, including:

[0013] Step 101, retrieve task requirement information for IC testing from a database; wherein the task requirement information includes a pitch between project measurement points and a particle size of conductive glue;

[0014] Step 102: preparing a No. 1 silk screen printing template and a No. 2 silk screen printing template according to the task requirement information for IC testing;

[0015] The gap between the No. 1 screen printing template and the No. 2 screen printing template is larger than the particle size of the conductive glue, and the gap between the No. 1 screen printing template and the No. 2 screen printing template should be staggered by 2×Pitch distance;

[0016] or,

[0017] The specific gap between the No. 1 silk screen printing template and the No. 2 silk screen printing template is set according to the constraint conditions of the gap.

[0018] Specifically, the process of setting the constraint conditions of the gap between the No. 1 silk screen template and the No. 2 silk screen template is as follows:

[0019] S1, extracting the distance Pitch between the measuring points of the project;

[0020] S2, extracting the particle size of the conductive glue;

[0021] S3, using the pitch Pitch between the project measurement points and the particle size of the conductive glue to set the gap adjustment factor between the No. 1 screen printing template and the No. 2 screen printing template;

[0022] S4. Using the gap adjustment factor between the No. 1 silk screen printing template and the No. 2 silk screen printing template, an upper limit value and a lower limit value of the constraint condition of the gap are set.

[0023] Specifically, the gap adjustment factor between the No. 1 screen printing template and the No. 2 screen printing template is set by using the pitch Pitch between the project measurement points and the particle size of the conductive glue, including:

[0024] S301, setting a first gap adjustment factor between the No. 1 screen printing template and the No. 2 screen printing template using the pitch Pitch between the project measurement points and the particle size of the conductive glue;

[0025] S302, setting a second gap adjustment factor between the No. 1 screen printing template and the No. 2 screen printing template using the pitch Pitch between the project measurement points and the particle size of the conductive glue;

[0026] The first gap adjustment factor and the second gap adjustment factor are obtained by the following formula:

[0027]

[0028]

[0029] Among them, Q 01 and Q 02 They represent the first gap adjustment factor and the second gap adjustment factor respectively; Q0 ​​represents the preset factor reference value; D represents the particle size of the conductive glue; P represents the pitch between the project measurement points; W s Indicates the actual viscosity of the conductive adhesive during preparation; W e It represents the theoretical viscosity of the material corresponding to the conductive adhesive; X represents the thixotropic index of the material corresponding to the conductive adhesive; W0 represents the viscosity corresponding to the pure base material of the conductive adhesive; Represents the volume fraction of particles in the conductive adhesive; It represents the maximum possible particle volume fraction of the conductive adhesive, usually close to the closest packing of particles;

[0030] At the same time, the gap adjustment factor between the No. 1 screen printing template and the No. 2 screen printing template is used to set the upper limit and lower limit of the gap constraint condition, including:

[0031] S401, using a first gap adjustment factor to set an upper limit value of a gap constraint condition;

[0032] S402, using the first gap adjustment factor to set a lower limit value of the gap constraint condition;

[0033] The upper limit and lower limit of the constraint condition of the gap are obtained by the following formula:

[0034] K up =(1-λ1·Q 01 )·αP

[0035] K down =(1+λ2·Q 02 )·D

[0036] Among them, K upand K down They respectively represent the upper limit value of the gap constraint condition and the lower limit value of the gap constraint condition; α represents the adjustment coefficient, and the value range is 1.91-2.03; P represents the pitch between the measuring points of the project; D represents the particle size of the conductive glue; λ1 and λ2 represent the first limit adjustment coefficient and the second limit adjustment coefficient respectively; specifically, the first limit adjustment coefficient and the second limit adjustment coefficient are obtained by the following formula:

[0037]

[0038] Wherein, λ1 and λ2 represent the first limit adjustment coefficient and the second limit adjustment coefficient respectively; Represents the volume fraction of particles in the conductive adhesive; Represents the maximum possible particle volume fraction of the conductive adhesive, usually close to the closest packing of particles.

[0039] Furthermore, laying a basic adhesive film on the operating base includes:

[0040] Step 201, performing flatness processing on the operating base to obtain an operating base whose average flatness meets preset requirements;

[0041] Step 202, aligning and fixing the silk-screen frame on the operating base platform where the average degree reaches the preset requirement;

[0042] Step 203, applying a non-stick release material by spraying or coating;

[0043] Step 204: Lay the base adhesive film on the operating base after the non-stick release material is laid out, and fix the edges and corners of the base adhesive film.

[0044] Furthermore, the No. 1 screen printing template and its corresponding conductive adhesive layer and isolation adhesive film are assembled on the operating base after the base adhesive film is laid, including:

[0045] Step 301, positioning the No. 1 screen printing template at a preset height, and controlling the installation device to press the No. 1 screen printing template downward to a predetermined position;

[0046] Step 302: Apply a conductive adhesive layer on the No. 1 screen printing template using a multi-pass molding process;

[0047] Step 303: After the conductive adhesive layer is formed, it is covered with an insulating adhesive film to form an isolation adhesive film.

[0048] Furthermore, an insulating film is used for covering to form an isolation film, including:

[0049] Step 3031, adjusting the dimensions of the insulating film in the X and Y directions;

[0050] Step 3032: After the dimensions of the insulating adhesive film in the X and Y directions are adjusted, the insulating adhesive film is covered on the conductive adhesive layer in the Z direction to form an isolation adhesive film.

[0051] Furthermore, the No. 2 silk screen template and its corresponding conductive adhesive layer and the isolation adhesive film are assembled on the No. 1 silk screen template and its corresponding isolation adhesive film, including:

[0052] Step 401, positioning the No. 2 screen printing template at a preset height, and controlling the installation device to press the No. 2 screen printing template downward to a predetermined position on the isolation film corresponding to the No. 1 screen printing template;

[0053] Step 402, applying a conductive adhesive layer on the No. 2 silk screen template by a multi-pass molding process;

[0054] Step 403: After the conductive adhesive layer corresponding to the No. 2 screen printing template is formed, it is covered with an insulating adhesive film to form an insulating adhesive film corresponding to the No. 2 screen printing template.

[0055] Further, after the conductive adhesive layer corresponding to the No. 2 screen printing template is formed, it is covered with an insulating adhesive film to form an insulating adhesive film corresponding to the No. 2 screen printing template, including:

[0056] Step 4031, adjusting the dimensions of the insulating film in the X and Y directions;

[0057] Step 4032: After the size of the insulating film in the X and Y directions is adjusted, the insulating film is covered on the conductive adhesive layer corresponding to the No. 2 screen printing template in the Z direction to form an insulating film corresponding to the No. 2 screen printing template.

[0058] Furthermore, the vertical conductive adhesive layer meeting the predetermined thickness is cut and the adhesive surface is polished, including:

[0059] Step 601, cutting the vertical conductive adhesive layer having a predetermined thickness perpendicular to the laying surface to form a cut vertical conductive adhesive layer block;

[0060] Step 602: fix the cut vertical conductive adhesive layer block, and after fixation, polish it with a grinding and polishing device to achieve a preset flatness.

[0061] Further, the vertical conductive adhesive layer having a predetermined thickness is cut perpendicularly to the laying surface to form a cut vertical conductive adhesive layer block, including:

[0062] Step 6011, controlling the displacement of the thermo-soft pressing head in the X-axis and Y-axis directions, and using the thermo-soft pressing head with displacement in the X-axis and Y-axis directions to pre-press the vertical conductive adhesive layer that meets the predetermined thickness;

[0063] Step 6012: After the vertical conductive adhesive layer having a predetermined thickness is cured, the cutting thickness of the adhesive layer is determined according to the pre-pressing stroke of the project and the performance of the conductive adhesive;

[0064] Step 6013, performing three-axis displacement fixing on the cured vertical conductive adhesive layer;

[0065] Step 6014: cutting the solidified vertical conductive adhesive layer according to the cutting thickness to form a cut vertical conductive adhesive layer block.

[0066] A vertical conductive adhesive system corresponding to the vertical conductive adhesive manufacturing method, the vertical conductive adhesive system comprises a base adhesive film, a No. 1 screen printing template group and a No. 2 screen printing template group; wherein the No. 1 screen printing template group is laid on the base adhesive film, and the No. 2 screen printing template group is laid on the No. 1 screen printing template group;

[0067] The No. 1 screen printing template group includes a No. 1 screen printing template, a conductive adhesive layer and an isolation adhesive film; the No. 1 screen printing template is laid on the base adhesive film, the conductive adhesive layer is laid on the side of the No. 1 screen printing template away from the base adhesive film; the isolation adhesive film is laid on the side of the conductive adhesive layer away from the No. 1 screen printing template;

[0068] The silk screen template group No. 2 includes silk screen template No. 2, a conductive adhesive layer and an isolation adhesive film; the silk screen template No. 2 is laid on the side of the isolation adhesive film of the silk screen template group No. 1 away from the conductive adhesive layer of the silk screen template group No. 1, and the conductive adhesive layer of the silk screen template group No. 2 is laid on the side of the silk screen template No. 2 away from the isolation adhesive film of the silk screen template group No. 1; the isolation adhesive film of the silk screen template group No. 2 is laid on the side of the conductive adhesive layer of the silk screen template group No. 2 away from the silk screen template No. 2.

[0069] Beneficial effects of the present invention:

[0070] The present invention proposes a method and system for making a vertical conductive adhesive for IC testing to address the shortcomings of the current technologies in the market. It integrates high-elasticity special silicone rubber, conductive adhesive, silk screen printing technology, etc. to develop a better alternative to the traditional typical connection method, which can solve the problems of deformation and poor flatness of components to be tested. The entire production can be completed at room temperature, the production process is simple, and batch production and automated production can be realized with low cost. It can be repeatedly disassembled and assembled, and maintenance and replacement are simple and easy to operate. BRIEF DESCRIPTION OF THE DRAWINGS

[0071] Figure 1 It is a schematic diagram of installation and testing of the method for making the vertical conductive adhesive of the present invention;

[0072] Figure 2 It is a three-dimensional diagram of the overall process of the vertical conductive adhesive manufacturing method of the present invention;

[0073] Figure 3 This is a front view of the overall process of the vertical conductive adhesive manufacturing method of the present invention;

[0074] Figure 4 It is an overall process schematic diagram of the method for manufacturing the vertical conductive adhesive of the present invention;

[0075] Figure 5 A schematic diagram of a template for the method for making the vertical conductive adhesive of the present invention. DETAILED DESCRIPTION

[0076] The preferred embodiments of the present invention are described below in conjunction with the accompanying drawings. It should be understood that the preferred embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.

[0077] The embodiment of the present invention provides a method for manufacturing a vertical conductive adhesive for IC testing, and the method comprises:

[0078] Step 1: Prepare a silk screen template according to task requirement information, wherein the silk screen template includes silk screen template No. 1 and silk screen template No. 2;

[0079] Step 2: Lay the base film on the operating base;

[0080] Step 3: After the base film is laid, assemble the No. 1 screen printing template and its corresponding conductive adhesive layer and isolation adhesive film on the operating base;

[0081] Step 4, assembling the No. 2 silk screen template and its corresponding conductive adhesive layer and isolation adhesive film on the No. 1 silk screen template and its corresponding isolation adhesive film;

[0082] Step 5, repeating steps 3 and 4 until the predetermined thickness required in the task requirement information is reached, forming a vertical conductive adhesive layer that meets the predetermined thickness;

[0083] Step 6: Cut and polish the vertical conductive adhesive layer that meets the predetermined thickness.

[0084] Among them, the silk screen template is made according to the task requirement information, including:

[0085] Step 101, retrieve task requirement information for IC testing from a database; wherein the task requirement information includes a pitch between project measurement points and a particle size of conductive glue;

[0086] Step 102: preparing a No. 1 silk screen printing template and a No. 2 silk screen printing template according to the task requirement information for IC testing;

[0087] The gap between the No. 1 screen printing template and the No. 2 screen printing template is larger than the particle size of the conductive glue, and the gap between the No. 1 screen printing template and the No. 2 screen printing template should be staggered by 2×Pitch distance;

[0088] or,

[0089] The specific gap between the No. 1 silk screen printing template and the No. 2 silk screen printing template is set according to the constraint conditions of the gap.

[0090] Among them, laying the basic adhesive film on the operating base includes:

[0091] Step 201, performing flatness processing on the operating base to obtain an operating base whose average flatness meets preset requirements;

[0092] Step 202, aligning and fixing the silk-screen frame on the operating base platform where the average degree reaches the preset requirement;

[0093] Step 203, applying a non-stick release material by spraying or coating;

[0094] Step 204: Lay the base adhesive film on the operating base after the non-stick release material is laid out, and fix the edges and corners of the base adhesive film.

[0095] Among them, the No. 1 screen printing template and its corresponding conductive adhesive layer and isolation adhesive film are assembled on the operating base after the basic adhesive film is laid, including:

[0096] Step 301, positioning the No. 1 screen printing template at a preset height, and controlling the installation device to press the No. 1 screen printing template downward to a predetermined position;

[0097] Step 302: Apply a conductive adhesive layer on the No. 1 screen printing template using a multi-pass molding process;

[0098] Step 303: After the conductive adhesive layer is formed, it is covered with an insulating adhesive film to form an isolation adhesive film.

[0099] Wherein, an insulating film is used for covering to form an isolation film, including:

[0100] Step 3031, adjusting the dimensions of the insulating film in the X and Y directions;

[0101] Step 3032: After the dimensions of the insulating adhesive film in the X and Y directions are adjusted, the insulating adhesive film is covered on the conductive adhesive layer in the Z direction to form an isolation adhesive film.

[0102] The No. 2 screen printing template and its corresponding conductive adhesive layer and the isolation adhesive film are assembled on the No. 1 screen printing template and its corresponding isolation adhesive film, including:

[0103] Step 401, positioning the No. 2 screen printing template at a preset height, and controlling the installation device to press the No. 2 screen printing template downward to a predetermined position on the isolation film corresponding to the No. 1 screen printing template;

[0104] Step 402, applying a conductive adhesive layer on the No. 2 silk screen template by a multi-pass molding process;

[0105] Step 403: After the conductive adhesive layer corresponding to the No. 2 screen printing template is formed, it is covered with an insulating adhesive film to form an insulating adhesive film corresponding to the No. 2 screen printing template.

[0106] Wherein, after the conductive adhesive layer corresponding to the No. 2 screen printing template is formed, an insulating adhesive film is used to cover it to form an insulating adhesive film corresponding to the No. 2 screen printing template, including:

[0107] Step 4031, adjusting the dimensions of the insulating film in the X and Y directions;

[0108] Step 4032: After the size of the insulating film in the X and Y directions is adjusted, the insulating film is covered on the conductive adhesive layer corresponding to the No. 2 screen printing template in the Z direction to form an insulating film corresponding to the No. 2 screen printing template.

[0109] The vertical conductive adhesive layer meeting the predetermined thickness is cut and the adhesive surface is polished, including:

[0110] Step 601, cutting the vertical conductive adhesive layer having a predetermined thickness perpendicular to the laying surface to form a cut vertical conductive adhesive layer block;

[0111] Step 602: fix the cut vertical conductive adhesive layer block, and after fixation, polish it with a grinding and polishing device to achieve a preset flatness.

[0112] The vertical conductive adhesive layer having a predetermined thickness is cut perpendicularly to the laying surface to form a vertical conductive adhesive layer block after cutting, including:

[0113] Step 6011, controlling the displacement of the thermo-soft pressing head in the X-axis and Y-axis directions, and using the thermo-soft pressing head with displacement in the X-axis and Y-axis directions to pre-press the vertical conductive adhesive layer that meets the predetermined thickness;

[0114] Step 6012: After the vertical conductive adhesive layer having a predetermined thickness is cured, the cutting thickness of the adhesive layer is determined according to the pre-pressing stroke of the project and the performance of the conductive adhesive;

[0115] Step 6013, performing three-axis displacement fixing on the cured vertical conductive adhesive layer;

[0116] Step 6014: cutting the solidified vertical conductive adhesive layer according to the cutting thickness to form a cut vertical conductive adhesive layer block.

[0117] The working principle of the above technical solution is: make a silk screen template according to project requirements: the silk screen template is divided into template No. 1 and template No. 2, the slit width of the template should be slightly larger than the particle size of the conductive glue, and it should be determined by comprehensive consideration of the viscosity and thixotropic index of the conductive glue; at the same time, the distance between the slits should not be too large, and it should be determined in combination with the Pitch of the chip to be tested; the gap of template No. 1 and the gap of template No. 2 should be staggered by 2*pitch distance, and the template should be coated according to the characteristics of the conductive glue to prevent adhesion during the processing.

[0118] Lay the base adhesive film; first use an operating base with good flatness, align and fix the silk-screen frame to ensure installation accuracy, spray non-stick release material on the operating base, or process the base into a coated non-stick material, lay the base adhesive film on the surface of the operating base, and fix the edges and corners.

[0119] Assemble template No. 1; position template No. 1 at a certain height, and then press it down to the predetermined position. The installation device needs to be set with limits to avoid deformation of the film when the pressure is too high, which will cause position deviation.

[0120] Conductive glue is applied by silk screen printing technology; the conductive glue is applied by multi-pass molding process. The conductive glue is a special product made according to the project. During the silk screen printing process, special equipment is required for real-time detection to ensure that the conductive glue will not be broken, so as to avoid affecting the signal connection effect later.

[0121] Lay the isolation film; after the conductive adhesive is formed, cover it with the insulating film. When covering the film, you must first adjust the dimensions of the film in the X and Y directions, and then cover it in the Z direction. After the film and the conductive adhesive are in contact, it cannot be adjusted or moved to avoid damaging the conductive adhesive line.

[0122] Assemble template No. 2; For the installation of template No. 2, refer to the corresponding steps for assembling template No. 1. Note that you must first determine the X and Y directions, and then install in the Z direction. After installing to the predetermined height, use fixing measures to prevent movement and damage to the lower adhesive layer.

[0123] Apply conductive glue using silk screen printing technology: Please refer to the corresponding steps of applying conductive glue using silk screen printing technology for operation.

[0124] Repeat step 1 to assemble template No. 1 to step 2 to apply conductive adhesive using screen printing technology. When the predetermined thickness is reached, proceed to the corresponding steps of laying the base adhesive film.

[0125] A special process is used to cut perpendicular to the paving surface: a hot soft pressure head is used to pre-press the adhesive layer. During the pre-pressing process, attention should be paid to controlling the displacement in the X and Y axis directions. After the curing is completed, the cutting thickness of the adhesive layer is determined according to the pre-pressing stroke of the project, the performance of the conductive adhesive, etc., and a special process is used to cut it into thin slices. During the cutting process, attention should be paid to fixing the three-axis displacement to avoid the adhesive layer falling off and the conductive adhesive line being damaged.

[0126] Polishing and leveling of rubber surface: Use special fixtures to fix the cut and shaped rubber sheets, and use grinding and polishing equipment to polish the rubber surface to the designed flatness.

[0127] Meanwhile, the application introduction of the present invention in this embodiment is only directed to the application of the present invention in automated testing, but does not exclude other application scenarios in which the present invention is used in conjunction with other components.

[0128] Make a silk-screen template according to project requirements: The biggest feature of this invention is its versatility in IC testing. Therefore, when designing a silk-screen template, it is necessary to determine the template's seam width, thickness, position, Pitch, etc. based on specific project measurement point PITCH, particle size of the conductive glue, material properties, processing technology, and other specific considerations.

[0129] Laying the base film: Since the base film is used to fix the upper adhesive layer, it must be a film with small deformation, single-sided adhesive, and strong tear resistance, and fixed at the boundary.

[0130] Assemble template No. 1: The template needs to be treated with anti-stick coating measures, and it needs to be cleaned after each application of conductive glue. During the assembly process, first determine the position of the X and Y axes, and then move in the Z axis direction. After installing to the predetermined position, it cannot be moved again to avoid deformation of the glue layer.

[0131] Use silk screen printing technology to apply conductive glue: The conductive glue is specially made for the project, the particle size needs to be compatible with the template, and the application can be formed in multiple passes. The line must not be broken during the application process to avoid unstable transmission signals in the later stage.

[0132] Laying the isolation film: The isolation film must have good insulation and compatibility, high mutual bonding strength, be compatible as a whole at high temperature, and will not debond.

[0133] The steps for assembling template No. 2 are the same as those for assembling template No. 1. Pay attention to the staggered installation with template No. 1.

[0134] Applying conductive glue using silk screen printing technology: The steps are the same as applying conductive glue using silk screen printing technology.

[0135] Repeat the steps of assembling formwork No. 1 to assembling formwork No. 2. When the predetermined thickness is reached, proceed to the step of laying the base film.

[0136] A special process is used to cut perpendicular to the paving surface: before cutting, the conductive adhesive is first cured to make it completely solidified, and then the X and Y axes are fixed in reverse, and the Z axis is pre-pressed with a hot soft press head in the reverse direction to ensure that the adhesive films and the adhesive films and the conductive adhesive are fully bonded. Be careful not to cause cracking and deformation of the adhesive layer.

[0137] Polishing and leveling of the rubber surface: The rubber surface needs to be perpendicular to the rubber line, and the cutting surface of the rubber layer is processed by grinding and polishing technology to achieve the designed flatness. At the same time, the part of the rubber film close to the boundary also needs to be cut off, and the verticality of the rubber line and the flatness of the rubber surface are strictly controlled. The cross-section of the overall rubber line is arranged in a plum blossom shape.

[0138] The technical effect of the above technical solution is as follows: The above technical solution of this embodiment describes a step-by-step method for preparing a vertical conductive adhesive layer by stacking different materials, including a conductive adhesive layer and an isolation adhesive film. This vertical conductive adhesive layer can be applied to different fields, such as semiconductor manufacturing.

[0139] The above technical solution of this embodiment ensures that the thickness of the final vertical conductive adhesive layer reaches the predetermined requirements by repeatedly assembling and stacking different layers. This precise control enables the prepared conductive adhesive layer to meet specific engineering requirements. Once the predetermined thickness is reached, the technical solution further describes the steps of cutting and polishing the adhesive surface. This helps to obtain a vertical conductive adhesive layer of the desired size and surface quality. Vertical conductive adhesive layers are commonly used in electronic component manufacturing, making the production of vertical conductive adhesive layers that meet the requirements more controllable and efficient.

[0140] In summary, the above technical solution of this embodiment provides a process for producing a vertical conductive adhesive layer, which allows controlling its thickness and ensuring its quality, and is applicable to a variety of application fields, which helps to improve the performance and reliability of electronic components.

[0141] In one embodiment of the present invention, the process of setting the constraint conditions of the gap between the No. 1 silk screen template and the No. 2 silk screen template is as follows:

[0142] S1, extracting the distance Pitch between the measuring points of the project;

[0143] S2, extracting the particle size of the conductive glue;

[0144] S3, using the pitch Pitch between the project measurement points and the particle size of the conductive glue to set the gap adjustment factor between the No. 1 screen printing template and the No. 2 screen printing template;

[0145] S4. Using the gap adjustment factor between the No. 1 silk screen printing template and the No. 2 silk screen printing template, an upper limit value and a lower limit value of the constraint condition of the gap are set.

[0146] Specifically, the gap adjustment factor between the No. 1 screen printing template and the No. 2 screen printing template is set by using the pitch Pitch between the project measurement points and the particle size of the conductive glue, including:

[0147] S301, setting a first gap adjustment factor between the No. 1 screen printing template and the No. 2 screen printing template using the pitch Pitch between the project measurement points and the particle size of the conductive glue;

[0148] S302, setting a second gap adjustment factor between the No. 1 screen printing template and the No. 2 screen printing template using the pitch Pitch between the project measurement points and the particle size of the conductive glue;

[0149] The first gap adjustment factor and the second gap adjustment factor are obtained by the following formula:

[0150]

[0151] Among them, Q 01 and Q 02 They represent the first gap adjustment factor and the second gap adjustment factor respectively; Q0 ​​represents the preset factor reference value; D represents the particle size of the conductive glue; P represents the pitch between the project measurement points; W s Indicates the actual viscosity of the conductive adhesive during preparation; W e It represents the theoretical viscosity of the material corresponding to the conductive adhesive; X represents the thixotropic index of the material corresponding to the conductive adhesive; W0 represents the viscosity corresponding to the pure base material of the conductive adhesive; Represents the volume fraction of particles in the conductive adhesive; It represents the maximum possible particle volume fraction of the conductive adhesive, usually close to the closest packing of particles;

[0152] At the same time, the gap adjustment factor between the No. 1 screen printing template and the No. 2 screen printing template is used to set the upper limit and lower limit of the gap constraint condition, including:

[0153] S401, using a first gap adjustment factor to set an upper limit value of a gap constraint condition;

[0154] S402, using the first gap adjustment factor to set a lower limit value of the gap constraint condition;

[0155] The upper limit and lower limit of the constraint condition of the gap are obtained by the following formula:

[0156] K up =(1-λ1·Q 01 )·αP

[0157] K down =(1+λ2·Q 02 )·D

[0158] Among them, K up and K down They respectively represent the upper limit value of the gap constraint condition and the lower limit value of the gap constraint condition; α represents the adjustment coefficient, and the value range is 1.91-2.03; P represents the pitch between the measuring points of the project; D represents the particle size of the conductive glue; λ1 and λ2 represent the first limit adjustment coefficient and the second limit adjustment coefficient respectively; specifically, the first limit adjustment coefficient and the second limit adjustment coefficient are obtained by the following formula:

[0159]

[0160] Wherein, λ1 and λ2 represent the first limit adjustment coefficient and the second limit adjustment coefficient respectively; Represents the volume fraction of particles in the conductive adhesive; Represents the maximum possible particle volume fraction of the conductive adhesive, usually close to the closest packing of particles.

[0161] The working principle of the above technical solution is: Extract parameters (S1 and S2): obtain two key parameters from the project measurement points.

[0162] Pitch: This is the parameter of the spacing between the project measurement points, which may be related to the characteristics of the template and conductive adhesive.

[0163] Conductive adhesive particle size: This is the size of the particles in the conductive adhesive and may affect the performance of the conductive adhesive.

[0164] Set gap adjustment factor (S3): Use the extracted parameters (pitch and particle size) to calculate and set the gap adjustment factor. These factors will be used to adjust the gap size between the silk screen templates.

[0165] Setting gap constraints (S4): Using the gap adjustment factor, set the upper and lower limits of the gap constraints. These constraints will limit the range of variation of the gap size between the templates.

[0166] Specifically, first, two important parameters are extracted from the project measurement points, namely the pitch and the particle size of the conductive glue. These parameters are the basis for subsequent calculations.

[0167] Second, set the gap adjustment factor:

[0168] S301-First gap adjustment factor: Using the extracted parameters, calculate the first gap adjustment factor Q01. This factor is used to adjust the gap size between the first screen printing template and the second screen printing template.

[0169] S302 - Second gap adjustment factor: Also using the extracted parameters, calculate the second gap adjustment factor Q02, which is used to adjust the gap size between the first and second silk screen templates.

[0170] Finally, calculate the gap adjustment factor: The calculation of these two adjustment factors uses a complex formula, which includes multiple variables and parameters, such as the actual viscosity of the conductive adhesive, the theoretical viscosity of the material corresponding to the conductive adhesive, the thixotropic index, the particle volume fraction, etc. These parameters will affect the characteristics of the conductive adhesive.

[0171] On the other hand, set the upper and lower limits:

[0172] S401-Upper limit setting: using the first gap adjustment factor, calculate the upper limit value (Kup) of the gap constraint condition.

[0173] S402 - setting the lower limit: also using the first gap adjustment factor, calculate the lower limit value (Kdown) of the gap constraint condition.

[0174] Calculating the upper limit and the lower limit: The calculation of these upper limit and the lower limit involves multiple parameters and adjustment coefficients, such as the adjustment coefficient α, the pitch Pitch, the particle size of the conductive adhesive, the first limit adjustment coefficient λ1 and the second limit adjustment coefficient λ2.

[0175] The effect of the above technical solution is: by calculating and adjusting the gap adjustment factor and setting the gap constraint conditions, the technical solution allows precise control of the characteristics of the conductive adhesive layer, such as thickness and uniformity. At the same time, it can adapt to different preparation conditions according to the particle size of the conductive adhesive and the spacing of the project measurement points. This increases its applicability. By effectively controlling the gap size, the preparation process of the conductive adhesive can be optimized to meet specific engineering requirements. At the same time, the above method can effectively improve the matching of the gap size with the processing project, as well as the adaptive adjustability of the gap size to change with the actual processing situation, thereby preventing the occurrence of quality problems in the processed products due to unreasonable gap size settings.

[0176] At the same time, the above technical solution of this embodiment allows the gap between the screen printing templates to be accurately adjusted to control the characteristics of the conductive adhesive layer, such as thickness and uniformity. According to factors such as the particle size and actual viscosity of the conductive adhesive, it can be adapted to different preparation situations, making it more versatile. By effectively adjusting the gap between the templates, the preparation process of the conductive adhesive can be optimized to meet specific engineering requirements. It is used to control the characteristics of the conductive adhesive layer to improve the accuracy and applicability of the optimized preparation, and at the same time, improve the efficiency and quality of the conductive adhesive preparation.

[0177] On the other hand, by setting upper and lower limits, the technical solution limits the range of variation of the gap size between the templates. This helps to ensure that the characteristics of the conductive adhesive layer are within an acceptable range. At the same time, by using adjustment coefficients α, λ1 and λ2, the constraints of the gap can be flexibly adjusted according to specific needs and the characteristics of the conductive adhesive. The above technical solution of this embodiment can effectively control the preparation process of the conductive adhesive to meet specific engineering requirements and improve the preparation quality. The working principle of the above technical solution involves calculating and setting upper and lower limits to control the characteristics of the conductive adhesive layer. By improving the preparation limitability, adjustability and flexibility of the preparation process during the preparation process, the efficiency and quality of the conductive adhesive preparation are improved.

[0178] The embodiment of the present invention provides a vertical conductive adhesive system corresponding to the vertical conductive adhesive manufacturing method, wherein the vertical conductive adhesive system includes a base adhesive film, a No. 1 screen printing template group and a No. 2 screen printing template group; wherein the No. 1 screen printing template group is laid on the base adhesive film, and the No. 2 screen printing template group is laid on the No. 1 screen printing template group;

[0179] The No. 1 screen printing template group includes a No. 1 screen printing template, a conductive adhesive layer and an isolation adhesive film; the No. 1 screen printing template is laid on the base adhesive film, the conductive adhesive layer is laid on the side of the No. 1 screen printing template away from the base adhesive film; the isolation adhesive film is laid on the side of the conductive adhesive layer away from the No. 1 screen printing template;

[0180] The silk screen template group No. 2 includes silk screen template No. 2, a conductive adhesive layer and an isolation adhesive film; the silk screen template No. 2 is laid on the side of the isolation adhesive film of the silk screen template group No. 1 away from the conductive adhesive layer of the silk screen template group No. 1, and the conductive adhesive layer of the silk screen template group No. 2 is laid on the side of the silk screen template No. 2 away from the isolation adhesive film of the silk screen template group No. 1; the isolation adhesive film of the silk screen template group No. 2 is laid on the side of the conductive adhesive layer of the silk screen template group No. 2 away from the silk screen template No. 2.

[0181] The effect of the above technical solution is: the vertical conductive adhesive system corresponding to the vertical conductive adhesive production method for IC testing proposed in this embodiment aims to address the shortcomings of the current technologies on the market, and integrates high-elasticity special silicone rubber, conductive adhesive, silk screen printing technology, etc. to develop a better alternative to the traditional typical connection method, which can solve the problems of deformation and poor flatness of components to be tested. The entire production can be completed at room temperature, the production process is simple, and mass production and automated production can be realized with low cost. It can be repeatedly disassembled and assembled, and maintenance and replacement are simple and easy to operate.

[0182] Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.

Claims

1. A method for making a vertical conductive adhesive for IC testing, characterized in that: The vertical conductive adhesive manufacturing method comprises: Step 1: Prepare a silk screen template according to task requirement information, wherein the silk screen template includes silk screen template No. 1 and silk screen template No. 2; Step 2: Lay the base film on the operating base; Step 3: After the base film is laid, assemble the No. 1 screen printing template and its corresponding conductive adhesive layer and isolation adhesive film on the operating base; Step 4, assembling the No. 2 silk screen template and its corresponding conductive adhesive layer and isolation adhesive film on the No. 1 silk screen template and its corresponding isolation adhesive film; Step 5, repeating steps 3 and 4 until the predetermined thickness required in the task requirement information is reached, forming a vertical conductive adhesive layer that meets the predetermined thickness; Step 6, cutting and polishing the vertical conductive adhesive layer that meets the predetermined thickness; Among them, the silk screen template is made according to the task requirement information, including: Step 101, retrieve task requirement information for IC testing from a database; wherein the task requirement information includes a pitch between project measurement points and a particle size of conductive glue; Step 102: preparing a No. 1 silk screen printing template and a No. 2 silk screen printing template according to the task requirement information for IC testing; The gap between the No. 1 screen printing template and the No. 2 screen printing template is larger than the particle size of the conductive glue, and the gap between the No. 1 screen printing template and the No. 2 screen printing template should be staggered by 2×Pitch distance; or, According to the constraint condition of the gap, a specific gap between the No. 1 screen printing template and the No. 2 screen printing template is set; The process of setting the constraint conditions of the gap between the No. 1 silk screen template and the No. 2 silk screen template is as follows: S1, extracting the distance Pitch between the measuring points of the project; S2, extracting the particle size of the conductive glue; S3, using the pitch Pitch between the project measurement points and the particle size of the conductive glue to set the gap adjustment factor between the No. 1 screen printing template and the No. 2 screen printing template; S4. Using the gap adjustment factor between the No. 1 silk screen printing template and the No. 2 silk screen printing template, an upper limit value and a lower limit value of the constraint condition of the gap are set. The gap adjustment factor between the No. 1 screen printing template and the No. 2 screen printing template is set by using the pitch Pitch between the project measurement points and the particle size of the conductive glue, including: S301, setting a first gap adjustment factor between the No. 1 screen printing template and the No. 2 screen printing template using the pitch Pitch between the project measurement points and the particle size of the conductive glue; S302, setting a second gap adjustment factor between the No. 1 screen printing template and the No. 2 screen printing template using the pitch Pitch between the project measurement points and the particle size of the conductive glue; The first gap adjustment factor and the second gap adjustment factor are obtained by the following formula: Among them, Q 01 and Q 02 They represent the first gap adjustment factor and the second gap adjustment factor respectively; Q0 ​​represents the preset factor reference value; D represents the particle size of the conductive glue; P represents the pitch between the project measurement points; W s Indicates the actual viscosity of the conductive adhesive during preparation; W e It represents the theoretical viscosity of the material corresponding to the conductive adhesive; X represents the thixotropic index of the material corresponding to the conductive adhesive; W0 represents the viscosity corresponding to the pure base material of the conductive adhesive; Represents the volume fraction of particles in the conductive adhesive; It represents the maximum possible particle volume fraction of the conductive adhesive, usually close to the closest packing of particles; At the same time, the gap adjustment factor between the No. 1 screen printing template and the No. 2 screen printing template is used to set the upper limit and lower limit of the gap constraint condition, including: S401, using a first gap adjustment factor to set an upper limit value of a gap constraint condition; S402, using the first gap adjustment factor to set a lower limit value of the gap constraint condition; The upper limit and lower limit of the constraint condition of the gap are obtained by the following formula: K up =(1-λ1·Q 01 )·αP K down =(1+λ2·Q 02 )·D Among them, K up and K down They respectively represent the upper limit value of the gap constraint condition and the lower limit value of the gap constraint condition; α represents the adjustment coefficient, and the value range is 1.91-2.03; P represents the pitch between the measuring points of the project; D represents the particle size of the conductive glue; λ1 and λ2 represent the first limit adjustment coefficient and the second limit adjustment coefficient respectively; specifically, the first limit adjustment coefficient and the second limit adjustment coefficient are obtained by the following formula: Wherein, λ1 and λ2 represent the first limit adjustment coefficient and the second limit adjustment coefficient respectively; Represents the volume fraction of particles in the conductive adhesive; Represents the maximum possible particle volume fraction of the conductive adhesive, usually close to the closest packing of particles.

2. The method for making vertical conductive adhesive according to claim 1, characterized in that: Lay the base film on the operating base, including: Step 201, performing flatness processing on the operating base to obtain an operating base whose average flatness meets preset requirements; Step 202, aligning and fixing the silk-screen frame on the operating base platform where the average degree reaches the preset requirement; Step 203, applying a non-stick release material by spraying or coating; Step 204: Lay the base adhesive film on the operating base after the non-stick release material is laid out, and fix the edges and corners of the base adhesive film.

3. The method for making vertical conductive adhesive according to claim 1, characterized in that: After the base film is laid, the No. 1 screen printing template and its corresponding conductive adhesive layer and isolation film are assembled on the operating base, including: Step 301, positioning the No. 1 screen printing template at a preset height, and controlling the installation device to press the No. 1 screen printing template downward to a predetermined position; Step 302: Apply a conductive adhesive layer on the No. 1 screen printing template using a multi-pass molding process; Step 303: After the conductive adhesive layer is formed, it is covered with an insulating adhesive film to form an isolation adhesive film.

4. The method for making vertical conductive adhesive according to claim 3, characterized in that: The insulating film is used for covering to form an isolation film, including: Step 3031, adjusting the dimensions of the insulating film in the X and Y directions; Step 3032: After the dimensions of the insulating adhesive film in the X and Y directions are adjusted, the insulating adhesive film is covered on the conductive adhesive layer in the Z direction to form an isolation adhesive film.

5. The method for making vertical conductive adhesive according to claim 1, characterized in that: Assemble No. 2 screen printing template and its corresponding conductive adhesive layer and isolation adhesive film on No. 1 screen printing template and its corresponding isolation adhesive film, including: Step 401, positioning the No. 2 screen printing template at a preset height, and controlling the installation device to press the No. 2 screen printing template downward to a predetermined position on the isolation film corresponding to the No. 1 screen printing template; Step 402, applying a conductive adhesive layer on the No. 2 silk screen template by a multi-pass molding process; Step 403: After the conductive adhesive layer corresponding to the No. 2 screen printing template is formed, it is covered with an insulating adhesive film to form an insulating adhesive film corresponding to the No. 2 screen printing template.

6. The method for making vertical conductive adhesive according to claim 5, characterized in that: After the conductive adhesive layer corresponding to the No. 2 screen printing template is formed, an insulating adhesive film is used to cover it to form an insulating adhesive film corresponding to the No. 2 screen printing template, including: Step 4031, adjusting the dimensions of the insulating film in the X and Y directions; Step 4032: After the dimensions of the insulating film in the X and Y directions are adjusted, the insulating film is covered on the conductive adhesive layer corresponding to the No. 2 screen printing template in the Z direction to form an insulating film corresponding to the No. 2 screen printing template.

7. The method for making vertical conductive adhesive according to claim 1, characterized in that: Cutting and polishing the vertical conductive adhesive layer that meets the predetermined thickness, including: Step 601, cutting the vertical conductive adhesive layer having a predetermined thickness perpendicular to the laying surface to form a cut vertical conductive adhesive layer block; Step 602: fix the cut vertical conductive adhesive layer block, and after fixation, polish it with a grinding and polishing device to achieve a preset flatness.

8. The method for making vertical conductive adhesive according to claim 7, characterized in that: Cutting the vertical conductive adhesive layer that meets the predetermined thickness perpendicular to the laying surface to form a cut vertical conductive adhesive layer block, including: Step 6011, controlling the displacement of the thermo-soft pressing head in the X-axis and Y-axis directions, and using the thermo-soft pressing head with displacement in the X-axis and Y-axis directions to pre-press the vertical conductive adhesive layer that meets the predetermined thickness; Step 6012: After the vertical conductive adhesive layer having a predetermined thickness is cured, the cutting thickness of the adhesive layer is determined according to the pre-pressing stroke of the project and the performance of the conductive adhesive; Step 6013, performing three-axis displacement fixing on the cured vertical conductive adhesive layer; Step 6014: cutting the solidified vertical conductive adhesive layer according to the cutting thickness to form a cut vertical conductive adhesive layer block.

9. A vertical conductive adhesive system corresponding to the vertical conductive adhesive manufacturing method according to claim 1, characterized in that: The vertical conductive adhesive system includes a base adhesive film, a No. 1 screen printing template group and a No. 2 screen printing template group; wherein the No. 1 screen printing template group is laid on the base adhesive film, and the No. 2 screen printing template group is laid on the No. 1 screen printing template group; The No. 1 screen printing template group includes a No. 1 screen printing template, a conductive adhesive layer and an isolation adhesive film; the No. 1 screen printing template is laid on the base adhesive film, the conductive adhesive layer is laid on the side of the No. 1 screen printing template away from the base adhesive film; the isolation adhesive film is laid on the side of the conductive adhesive layer away from the No. 1 screen printing template; The silk screen template group No. 2 includes silk screen template No. 2, a conductive adhesive layer and an isolation adhesive film; the silk screen template No. 2 is laid on the side of the isolation adhesive film of the silk screen template group No. 1 away from the conductive adhesive layer of the silk screen template group No. 1, and the conductive adhesive layer of the silk screen template group No. 2 is laid on the side of the silk screen template No. 2 away from the isolation adhesive film of the silk screen template group No. 1; the isolation adhesive film of the silk screen template group No. 2 is laid on the side of the conductive adhesive layer of the silk screen template group No. 2 away from the silk screen template No. 2.