Continuous gradient high-temperature-resistant resistive film and preparation method thereof
By using the conductive paste with silicone resin as the binder, it is cured on the same substrate in order of resistance value, and a high-temperature resistance film that continuously changes at high temperature is achieved, and the insufficient temperature resistance and resistance in the prior art are solved. The problem of difficult value gradation is difficult to achieve, which improves the performance and appearance quality of the resistor film.
Patent Information
- Application Number
- CN202411112522.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-11-12
AI Technical Summary
The existing high-temperature resistant flexible resistive film has low temperature resistance and cannot be used in scenarios above 200°C. It is difficult for existing methods to achieve continuous gradient of resistance values on the same flexible substrate, and there are cross overlap or gap areas. , affects the conductivity.
Use silicone resin as the binder to prepare conductive pastes with different resistance values, and cure them on the same substrate in the order of resistance values from small to large or from large to small, so as to achieve continuous gradient resistance through screen printing technology. High temperature resistive film.
A continuous gradient high-temperature resistance film used at 300°C to 380°C is realized, which simplifies the processing process, avoids cross-overlapping or gap areas, and improves the conductivity.
Smart Images

Figure CN118942823A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of electronic materials and relates to a continuous gradient high temperature resistant resistor film and a preparation method thereof. Background Art
[0002] As an electronic functional composite material, high temperature resistant flexible resistor film is composed of high temperature resistant flexible substrate and high temperature resistant conductive functional layer. It is widely used in various electronic devices such as thick film integrated circuits, resistance strain gauges and pressure sensitive sensors. The high temperature resistant conductive functional layer is cured by high temperature resistant flexible conductive paste, which is the key to ensure the conductive performance of the material. The conductive paste is composed of organic carrier, conductive filler and necessary additives.
[0003] In recent years, carbon black (CB), carbon nanotubes, graphite, graphene and carbon fiber (CF) have been widely used as conductive fillers in the preparation of carbon-based conductive pastes due to their excellent conductivity. The prepared conductive paste can usually be applied to the surface of plastic films or fiber fabrics such as methyl vinyl silicone rubber (VMQ), glass fiber silicone cloth, high-silica glass fiber cloth, PET substrate film, PE substrate film and PI substrate film by screen printing, scraping or spraying, and then a flexible resistor film with a specific resistance value can be obtained by baking and curing.
[0004] However, the conductive paste formulas reported so far mainly use one or more of polyurethane resin, acrylic resin, epoxy resin, etc. as system film-forming materials to make conductive pastes. Since the temperature resistance of such resins is not high, the temperature resistance of the resistor film made from them is not high and cannot be used in scenarios where the temperature is higher than 200°C or even higher. In addition, the resistor film is mainly formed with one resistance value on the same film. The current methods for forming resistor films with continuously changing resistance values on the same flexible substrate are not simple enough. If multiple resistance values are to exist at the same time, a cumbersome processing process is required, and there are certain cross-overlaps or gaps between resistor films with different resistance values, which greatly affects the product appearance and conductive properties. Summary of the invention
[0005] The purpose of the present invention is to overcome the above-mentioned shortcomings of the prior art and to provide a continuous gradient high temperature resistant resistor film and a preparation method thereof.
[0006] In order to achieve the above-mentioned purpose, the present invention adopts the following technical scheme: a continuous gradient high temperature resistant resistor film, comprising: a high temperature resistant conductive functional layer distributed on a substrate, wherein the high temperature resistant conductive functional layer is formed by sequentially curing conductive pastes of different resistance values with silicone resin as a binder in the order of resistance from small to large or from large to small.
[0007] A method for preparing a continuously gradient high temperature resistant resistor film, using silicone resin as a binder to make conductive pastes with different resistance values, and curing the conductive pastes with different resistance values on the same substrate in the order of resistance from small to large or from large to small, to obtain a resistor film with continuously gradient resistance value.
[0008] Furthermore, the method specifically includes the following steps:
[0009] Step 1, preparing a conductive paste: using silicone resin as a binder to prepare conductive pastes of different resistance values, and dividing the conductive pastes into conductive paste A, conductive paste B, and conductive paste C in order of resistance from small to large or from large to small;
[0010] Step 2, preparing the template: preparing the template A, template B, and template C required for screen printing, wherein: the template A is provided with a first forming pattern, and the distance between the upper side length of the first forming pattern and the upper frame of the template A is b; the template B is provided with a second forming pattern, and the distance between the upper side length of the second forming pattern and the upper frame of the template A is b+h1; the template C is provided with a second forming pattern, and the distance between the upper side length of the second forming pattern and the upper frame of the template A is b+h1+h2;
[0011] Step 3. Preparation of a continuous gradient high-temperature resistant resistor film: fix template A on the cleaned substrate, print conductive paste A onto the substrate through template A, and obtain a substrate with resistor film A after heat treatment; fix template B and template C on the same substrate in sequence, print conductive paste B through template B and conductive paste C through template C in the same way, and then obtain a substrate with resistor film A, resistor film B, and resistor film C after heat treatment.
[0012] Furthermore, in the step 1, the conductive paste A, the conductive paste B, and the conductive paste C are all carbon black conductive paste, graphite conductive paste, or carbon fiber conductive paste.
[0013] Furthermore, in the process of preparing the carbon black conductive slurry, the following raw materials are included by weight: 4 to 10 parts of carbon black, 30 to 65 parts of silicone resin, and 30 to 55 parts of the first solvent.
[0014] Furthermore, in the process of preparing the graphite conductive slurry, the following raw materials are included by mass: 20 to 40 parts of graphite powder, 20 to 50 parts of silicone resin, and 20 to 40 parts of a first solvent.
[0015] Furthermore, in the process of preparing carbon fiber conductive slurry, the following raw materials are included by mass: 1.2 to 3.5 parts of chopped carbon fiber, 4 to 9 parts of carbon black, 10 to 45 parts of silicone resin, 1 to 2.5 parts of dispersant, and 49 to 55 parts of a second solvent.
[0016] Furthermore, in the step three, the template A, template B, template C and the substrate are fixed by a template positioning tool, and the template positioning tool includes a square fixing frame and four limiters, and the four limiters are respectively located on the four top corners of the square fixing frame, and the area defined by the four limiters is the same as the area of the template A.
[0017] Furthermore, the heat treatment in step three is: firstly, curing the substrate with the conductive layer A at 120°C to 150°C for 0.5h to 1h; and then sintering at 380±2°C.
[0018] Furthermore, the substrate is a polyimide film, glass fiber silicone cloth or high-silica glass fiber cloth.
[0019] Compared with the prior art, the present invention has the following beneficial effects:
[0020] 1. The continuous gradient high temperature resistant resistor film provided by the present invention is prepared by brushing a conductive slurry, wherein a silicone resin is used as a binder in the conductive slurry. The silicone resin has good high temperature resistance and can be used at 300°C or even 380°C. Therefore, the resistor film of the present invention can be used at 300°C or even 380°C.
[0021] 2. In the present invention, conductive pastes with different resistance values are used to prepare resistor films with different resistance values, which are printed on the same flexible substrate using a printing process, thereby achieving a resistor film with a continuously gradient resistance value formed on the same flexible substrate. The method is simple and there is no cross-overlap or gap area. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] The accompanying drawings are incorporated in and constitute a part of this specification and, together with the description, serve to explain the principles of the present invention.
[0023] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.
[0024] Figure 1 This is a schematic diagram of the structure of the continuous gradient high temperature resistant resistor film provided by the present invention;
[0025] Figure 2 This is a schematic diagram of the structure of the template A provided by the present invention;
[0026] Figure 3 This is a schematic diagram of the structure of the template B provided by the present invention;
[0027] Figure 4This is a schematic diagram of the structure of the template C provided by the present invention;
[0028] Figure 5 This is a schematic diagram of the structure of the template positioning tooling provided by the present invention;
[0029] Figure 6 A schematic diagram of a process of fixing a substrate on a template positioning tool provided by the present invention;
[0030] Figure 7 This is a schematic diagram of the assembly process of the template provided by the present invention and the positioning tool with a flexible substrate.
[0031] Among them: 1 represents a limiter; 2 represents a square fixing frame. DETAILED DESCRIPTION
[0032] Here, exemplary embodiments will be described in detail, and the embodiments described in the following exemplary embodiments do not represent all embodiments consistent with the present invention. Instead, they are only examples of devices consistent with some aspects of the present invention as detailed in the appended claims.
[0033] like Figure 1 As shown, a continuous gradient high temperature resistant resistor film includes: a high temperature resistant conductive functional layer distributed on a substrate, wherein the high temperature resistant conductive functional layer is formed by sequentially curing conductive pastes of different resistance values using silicone resin as a binder in the order of resistance from small to large or from large to small.
[0034] A method for preparing a continuously gradient high temperature resistant resistor film, using silicone resin as a binder to make conductive pastes with different resistance values, and curing the conductive pastes with different resistance values on the same substrate in the order of resistance from small to large or from large to small, to obtain a resistor film with continuously gradient resistance value.
[0035] Furthermore, the method specifically includes the following steps:
[0036] Step 1, preparing a conductive paste: using silicone resin as a binder to prepare conductive pastes of different resistance values, and dividing the conductive pastes into conductive paste A, conductive paste B, and conductive paste C in order of resistance from small to large or from large to small;
[0037] Step 2, preparing the template: preparing the template A, template B, and template C required for screen printing, wherein: the template A is provided with a first forming pattern, and the distance between the upper side length of the first forming pattern and the upper frame of the template A is b; the template B is provided with a second forming pattern, and the distance between the upper side length of the second forming pattern and the upper frame of the template A is b+h1; the template C is provided with a second forming pattern, and the distance between the upper side length of the second forming pattern and the upper frame of the template A is b+h1+h2;
[0038] Step 3. Preparation of a continuous gradient high-temperature resistant resistor film: fix template A on the cleaned substrate, print conductive paste A onto the substrate through template A, and obtain a substrate with resistor film A after heat treatment; fix template B and template C on the same substrate in sequence, print conductive paste B through template B and conductive paste C through template C in the same way, and then obtain a substrate with resistor film A, resistor film B, and resistor film C after heat treatment.
[0039] Furthermore, in the step 1, the conductive paste A, the conductive paste B, and the conductive paste C are all carbon black conductive paste, graphite conductive paste, or carbon fiber conductive paste.
[0040] Furthermore, in the process of preparing the carbon black conductive slurry, the following raw materials are included by weight: 4 to 10 parts of carbon black, 30 to 65 parts of silicone resin, and 30 to 55 parts of the first solvent.
[0041] Furthermore, in the process of preparing the graphite conductive slurry, the following raw materials are included by mass: 20 to 40 parts of graphite powder, 20 to 50 parts of silicone resin, and 20 to 40 parts of a first solvent.
[0042] Furthermore, in the process of preparing carbon fiber conductive slurry, the following raw materials are included by mass: 1.2 to 3.5 parts of chopped carbon fiber, 4 to 9 parts of carbon black, 10 to 45 parts of silicone resin, 1 to 2.5 parts of dispersant, and 49 to 55 parts of a second solvent.
[0043] Furthermore, in the step three, the template A, template B, template C and the substrate are fixed by a template positioning tool, and the template positioning tool includes a square fixing frame and four limiters, and the four limiters are respectively located on the four top corners of the square fixing frame, and the area defined by the four limiters is the same as the area of the template A.
[0044] Furthermore, the heat treatment in step three is: firstly, curing the substrate with the conductive layer A at 120°C to 150°C for 0.5h to 1h; and then sintering at 380±2°C for 0.5h.
[0045] Furthermore, the substrate is a polyimide film, glass fiber silicone cloth or high-silica glass fiber cloth.
[0046] Specifically, the preparation method is as follows:
[0047] (1) Preparation of conductive paste:
[0048] 1) Preparation of carbon black conductive slurry:
[0049] Weigh carbon black conductive paste according to proportion, wherein the components of the carbon black conductive paste are as follows by mass: 4 to 10 parts of carbon black, 30 to 65 parts of silicone resin, and 30 to 55 parts of solvent A, wherein the solvent A is xylene;
[0050] The carbon black, the silicone resin and the solvent A are mixed evenly to obtain a carbon black conductive slurry;
[0051] The homogenizer is used for uniform mixing, the speed of the homogenizer is 1000r / min, and the dispersion time is 0.5 to 1h;
[0052] 2) Preparation of graphite conductive slurry:
[0053] Weigh graphite conductive slurry in proportion, wherein the components of the graphite conductive slurry are as follows by mass: 20 to 40 parts of graphite powder, 20 to 50 parts of silicone resin, and 20 to 40 parts of solvent A, wherein the solvent A is xylene;
[0054] The graphite powder, the silicone resin and the solvent A are mixed evenly to obtain a graphite conductive slurry;
[0055] The homogenizer is used for uniform mixing, the speed of the homogenizer is 1000r / min, and the dispersion time is 0.5 to 1h;
[0056] 3) Preparation of carbon fiber conductive slurry:
[0057] Weigh carbon fiber conductive slurry in proportion, wherein the components of the carbon fiber conductive slurry are as follows by mass: 1.2-3.5 parts of chopped carbon fiber, 4-9 parts of carbon black, 10-45 parts of silicone resin, 1-2.5 parts of dispersant, and 49-55 parts of solvent B, wherein the solvent B is a mixture of xylene and n-butanol in a mass ratio of 3:1;
[0058] The chopped carbon fiber, the dispersant and the solvent B are uniformly mixed to obtain a chopped carbon fiber mixed liquid;
[0059] The ultrasonic cleaning machine is used for uniform dispersion, the power of the ultrasonic cleaning machine is 100W, the frequency is 40KHz, and the dispersion time is 30 to 40 minutes;
[0060] Adding the carbon black and the silicone resin into the chopped carbon fiber mixed solution and mixing evenly to obtain a carbon fiber conductive slurry;
[0061] The homogenizer is used for uniform mixing, the speed of the homogenizer is 1500r / min, and the dispersion time is 0.5-1h;
[0062] (2) Template design:
[0063] like Figures 2 to 4 As shown, the templates include template A, template B and template C;
[0064] The template A has a length of m and a width of n, and a first forming pattern is arranged inside; Definition: The upper left corner vertex of the template A is the coordinate origin, the direction along the side length m is defined as the x direction, and the direction along the side length n is defined as the y direction, and the length of the first forming pattern is l , the width of the first forming pattern is h1, the distance between the left side of the first forming pattern and the left side of the template A is a, and the distance between the upper edge of the first forming pattern and the upper edge of the template A is b;
[0065] The length of the template B is m, the width is n, and a second forming pattern is arranged inside; Definition: Taking the upper left corner vertex of the template B as the coordinate origin, the direction along the side length m is defined as the x direction, and the direction along the side length n is defined as the y direction; the length of the second forming pattern is l , the width of the second forming pattern is h2, the distance between the left side of the second forming pattern and the left side of the template B is a, and the distance between the upper edge of the second forming pattern and the upper edge of the template B is b+h1;
[0066] The length of the template C is m, the width is n, and a third forming pattern is arranged inside; Definition: Taking the upper left corner vertex of the template C as the coordinate origin, the direction along the side length m is defined as the x direction, and the direction along the side length n is defined as the y direction; the length of the third forming pattern is l , the width of the third forming pattern is h3, the distance between the left side of the third forming pattern and the left side of the template C is a, and the distance between the upper edge of the third forming pattern and the upper edge of the template C is b+h1+h2;
[0067] (3) Design of template positioning tooling:
[0068] like Figure 5 As shown, the template positioning tooling includes a square fixing frame 2 and four stoppers 1, and the four stoppers 1 are respectively located at the four vertex corners of the square fixing frame 2;
[0069] The area defined by the four stoppers 1 is the same as the area of the template A;
[0070] The material of the square fixing frame 2 is aluminum alloy, stainless steel or other materials that are highly machinable and not prone to deformation;
[0071] (4) Preparation of continuous gradient high temperature resistant resistor film:
[0072] 1) Using a high temperature resistant insulating flexible material as a substrate, and using alcohol to perform ultrasonic cleaning on the substrate, the power of the ultrasonic cleaning process is 40W and the frequency is 40KHz. The cleaned substrate is placed on the square fixing frame, and the four corners of the substrate are fixed with the stoppers;
[0073] 2) If Figures 6-7 As shown, the template A is placed on the substrate, and the four corners of the template A are fixed by the stoppers; the conductive paste is coated on the template A by screen printing, and the adjustable film applicator is used to scrape twice, and the template A is removed to obtain a conductive layer A with the same shape as the first forming pattern on the substrate; the substrate with the conductive layer A is subjected to a first heat treatment to obtain a substrate with a resistor film A;
[0074] The process of the first heat treatment is: firstly, the substrate with the conductive layer A is placed at a temperature of 120° C. to 150° C. for curing for 0.5 h to 1 h; and then, the substrate is placed at a temperature of 380±2° C. for sintering for 0.5 h.
[0075] 3) placing the template B on the substrate and fixing the four corners of the template B with the stoppers; applying the conductive paste on the template B by screen printing, applying twice with an adjustable film applicator, removing the template B, and obtaining a conductive layer B having the same shape as the second forming pattern on the substrate; subjecting the substrate with the conductive layer B to a second heat treatment to obtain a substrate with a resistor film B; the upper edge of the resistor film B is connected to the lower edge of the resistor film A;
[0076] The second heat treatment process is as follows: firstly, the substrate with the conductive layer B is placed at a temperature of 120°C to 150°C for curing for 0.5h to 1h; then, it is placed at 380±2°C for sintering for 0.5h;
[0077] 4) placing the template C on the substrate and fixing the four corners of the template C with the stoppers; applying the conductive paste on the template C by screen printing, applying twice with an adjustable film applicator, removing the template C, and obtaining a conductive layer C with the same shape as the third forming pattern on the substrate; performing a third heat treatment on the substrate with the conductive layer C to obtain a substrate with a resistor film C; the upper edge of the resistor film C is connected to the lower edge of the resistor film B;
[0078] The third heat treatment process is as follows: firstly, the substrate with the conductive layer C is placed at a temperature of 120° C. to 150° C. for curing for 0.5 h to 1 h; and then, the substrate is placed at a temperature of 380±2° C. for sintering for 0.5 h.
[0079] Furthermore, the high temperature resistant insulating flexible material is a polyimide film, a glass fiber silicone cloth or a high silica glass fiber cloth.
[0080] Example 1
[0081] The invention adopts carbon fiber conductive paste to form high temperature resistant resistor films with three resistance values on the same polyimide film, which mainly includes high temperature resistant flexible polyimide film and carbon fiber conductive paste printed on the substrate.
[0082] The specific preparation method is as follows:
[0083] Step 1: prepare carbon fiber conductive slurry, wherein the components in the carbon fiber conductive slurry are calculated by weight:
[0084] 1) Weigh 3.5 parts of chopped carbon fibers without adhesive having a diameter of 7 μm and a length of 0.5 mm, 52 parts of solvent B, 34 parts of silicone resin having a solid content of 55%, 8.6 parts of carbon black, and 1.9 parts of a dispersant;
[0085] Evenly mixing the chopped carbon fiber, the dispersant and the solvent B to obtain a chopped carbon fiber mixed liquid;
[0086] The ultrasonic cleaning machine is used for uniform dispersion, the power of the ultrasonic cleaning machine is 100W, the frequency is 40KHz, and the dispersion time is 30min;
[0087] Adding the carbon black and the silicone resin into the chopped carbon fiber mixed solution and mixing evenly to obtain a first carbon fiber conductive slurry;
[0088] The homogenizer was used for uniform mixing, the speed of the homogenizer was 1500 r / min, and the dispersion time was 1 h;
[0089] 2) Weigh 2.5 parts of chopped carbon fibers without adhesive having a diameter of 7 μm and a length of 0.5 mm, 49.7 parts of solvent B, 41.4 parts of silicone resin having a solid content of 55%, 4.1 parts of carbon black, and 2.3 parts of a dispersant;
[0090] Evenly mixing the chopped carbon fiber, the dispersant and the solvent B to obtain a chopped carbon fiber mixed liquid;
[0091] The ultrasonic cleaning machine is used for uniform dispersion, the power of the ultrasonic cleaning machine is 100W, the frequency is 40KHz, and the dispersion time is 30min;
[0092] Adding the carbon black and the silicone resin into the chopped carbon fiber mixed solution and mixing evenly to obtain a second carbon fiber conductive slurry;
[0093] The homogenizer was used for uniform mixing, the speed of the homogenizer was 1500 r / min, and the dispersion time was 1 h;
[0094] 3) Weigh 1.37 parts of chopped carbon fibers without glue having a diameter of 7 μm and a length of 0.5 mm, 54.9 parts of solvent B, 36.6 parts of silicone resin having a solid content of 55%, 5.9 parts of carbon black, and 1.23 parts of a dispersant;
[0095] The chopped carbon fiber, the dispersant and the solvent B are mixed evenly to obtain a chopped carbon fiber mixed solution; wherein, an ultrasonic cleaning machine is used for uniform dispersion, the power of the ultrasonic cleaning machine is 100W, the frequency is 40KHz, and the dispersion time is 30min;
[0096] The carbon black and the silicone resin are added into the chopped carbon fiber mixed solution and mixed evenly to obtain a third carbon fiber conductive slurry; wherein, a homogenizer is used for mixing evenly, the rotation speed of the homogenizer is 1500r / min, and the dispersion time is 1h.
[0097] Step 2: Clean the polyimide film. Soak the polyimide film in alcohol, clean it with ultrasonic waves for 5 minutes, and then dry it with a nitrogen gun. The power of the ultrasonic cleaning process is 40W and the frequency is 40KHz.
[0098] Step 3: Prepare a resistor film A, place the cleaned polyimide film on the square fixing frame, and fix the four corners of the polyimide film with the stoppers;
[0099] The template A is placed on the polyimide film, and the four corners of the template A are fixed with the stoppers. The first forming pattern set inside the template A is a rectangle with a length of 60 cm and a width of 5 cm, a screen mesh of 100, and a film thickness of 0.1 mm;
[0100] The first carbon fiber conductive slurry is coated on the template A, and an adjustable applicator is used to scrape it twice, the scraper of the adjustable applicator is adjusted to 50μm, the template A is removed, and a conductive layer A with a length of 60cm and a width of 5cm, which is the same as the first forming pattern, is obtained on the polyimide film; the polyimide film with the conductive layer A is subjected to a first heat treatment to obtain a polyimide film with a resistor film A, and the resistance values at different positions on the resistor film A are measured with a four-probe square resistance meter, and the resistance range is 50±10%Ω / sq; wherein, the process of the first heat treatment is: first, the polyimide film with the conductive layer A is placed at a temperature of 150°C for curing for 0.5h; and then, it is placed at 380±2°C for sintering for 0.5h.
[0101] Step 4: Prepare a resistor film B, place the template B on the polyimide film, and fix the four corners of the template B with the stoppers. The second forming pattern set inside the template B is a rectangle with a length of 60 cm and a width of 10 cm, a screen mesh of 100, and a film thickness of 0.1 mm.
[0102] The second carbon fiber conductive slurry is coated on the template B, and an adjustable applicator is used to scrape it twice, the scraper of the adjustable applicator is adjusted to 50μm, the template B is removed, and a conductive layer B with a length of 60cm and a width of 10cm, which is the same as the shape of the second forming pattern, is obtained on the polyimide film; the polyimide film with the conductive layer B is subjected to a second heat treatment to obtain a polyimide film with a resistor film B, the upper edge of the resistor film B is connected to the lower edge of the resistor film A, and the resistance values at different positions on the resistor film B are measured using a four-probe square resistance meter, and the resistance value range is 60±10%Ω / sq; wherein, the process of the second heat treatment is: first, the polyimide film with the conductive layer B is placed at a temperature of 150°C for curing for 0.5h; and then, it is placed at 380±2°C for sintering for 0.5h.
[0103] Step 5: Prepare a resistor film C, place the template C on the polyimide film, and fix the four corners of the template C with the stoppers. The third forming pattern set inside the template C is a rectangle with a length of 60 cm and a width of 8 cm, a screen mesh of 100, and a film thickness of 0.1 mm.
[0104] The third carbon fiber conductive slurry is coated on the template C, and is scraped twice using an adjustable applicator, the scraper of the adjustable applicator is adjusted to 50μm, the template C is removed, and a conductive layer C with a length of 60cm and a width of 8cm, which is the same shape as the third forming pattern, is obtained on the polyimide film; the polyimide film with the conductive layer C is subjected to a third heat treatment to obtain a polyimide film with a resistor film C, the upper edge of the resistor film C is connected to the lower edge of the resistor film B, and the resistance of different positions on the resistor film C is measured using a four-probe square resistance meter, and the resistance range is 75±10%Ω / sq; wherein, the process of the third heat treatment is: first, the polyimide film with the conductive layer C is placed at a temperature of 150°C for curing for 0.5h; and then, it is placed at 380±2°C for sintering for 0.5h.
[0105] Example 2
[0106] Graphite conductive paste and carbon black conductive paste are used to form high temperature resistant resistor films with three resistance values on the same polyimide film. The high temperature resistant resistor films mainly include high temperature resistant flexible polyimide film and carbon fiber high temperature resistant conductive paste coated on the substrate.
[0107] The specific preparation method is as follows:
[0108] Step 1: prepare graphite conductive slurry and carbon black conductive slurry, wherein the components in the graphite conductive slurry and carbon black conductive slurry are calculated by weight:
[0109] 1) Weigh 37 parts of graphite powder with a particle size of 1.3 μm, 30 parts of silicone resin with a solid content of 55%, and 33 parts of solvent A;
[0110] The graphite powder, the silicone resin and the solvent A are mixed evenly to obtain a graphite conductive slurry; wherein the mixing is performed evenly using a homogenizer, the speed of the homogenizer is 1000 r / min, and the dispersion time is 1 hour;
[0111] 2) Weigh 9 parts of carbon black with a particle size of 40 to 48 nm, 38 parts of silicone resin with a solid content of 55%, and 53 parts of solvent A;
[0112] The carbon black, the silicone resin and the solvent A are mixed evenly to obtain a first carbon black conductive slurry; wherein the mixing is performed evenly using a homogenizer, the speed of the homogenizer is 1000 r / min, and the dispersion time is 1 hour;
[0113] 3) Weigh 8 parts of carbon black with a particle size of 40 to 48 nm, 39.6 parts of silicone resin with a solid content of 55%, and 52.4 parts of solvent A;
[0114] The carbon black, the silicone resin and the solvent A are mixed evenly to obtain a second carbon black conductive slurry; wherein the mixing is performed evenly using a homogenizer, the speed of the homogenizer is 1000 r / min, and the dispersion time is 1 hour;
[0115] Step 2: Clean the polyimide film. Soak the polyimide film in alcohol, clean it with ultrasonic waves for 5 minutes, and then dry it with a nitrogen gun. The power of the ultrasonic cleaning process is 40W and the frequency is 40KHz.
[0116] Step 3: Prepare a resistor film A, place the cleaned polyimide film on the square fixing frame, and fix the four corners of the polyimide film with the stoppers;
[0117] The template A is placed on the polyimide film, and the four corners of the template A are fixed with the stoppers. The first forming pattern set inside the template A is a rectangle with a length of 20 cm and a width of 5 cm, a screen mesh of 100, and a film thickness of 0.1 mm;
[0118] The graphite conductive slurry is coated on the template A, and an adjustable applicator is used to scrape it twice, the scraper of the adjustable applicator is adjusted to 50μm, the template A is removed, and a conductive layer A with a length of 20cm and a width of 5cm, which is the same as the first forming pattern, is obtained on the polyimide film; the polyimide film with the conductive layer A is subjected to a first heat treatment to obtain a polyimide film with a resistor film A, and the resistance values at different positions on the resistor film A are measured with a four-probe square resistance meter, and the resistance value range is 130±10%Ω / sq; wherein, the process of the first heat treatment is: first, the polyimide film with the conductive layer A is placed at a temperature of 120°C for curing for 0.5h; and then, it is placed at 380±2°C for sintering for 0.5h.
[0119] Step 4: Prepare a resistor film B, place the template B on the polyimide film, and fix the four corners of the template B with the stoppers. The second forming pattern set inside the template B is a rectangle with a length of 20 cm and a width of 4 cm, a screen mesh of 100, and a film thickness of 0.1 mm.
[0120] The first carbon black conductive slurry is coated on the template B, and is scraped twice by an adjustable applicator, the scraper of the adjustable applicator is adjusted to 50μm, the template B is removed, and a conductive layer B with a length of 20cm and a width of 4cm, which is the same as the shape of the second forming pattern, is obtained on the polyimide film; the polyimide film with the conductive layer B is subjected to a second heat treatment to obtain a polyimide film with a resistor film B, the upper edge of the resistor film B is connected to the lower edge of the resistor film A, and the resistance values at different positions on the resistor film B are measured by a four-probe square resistance meter, and the resistance value range is 150±10%Ω / sq; wherein, the process of the second heat treatment is: first, the polyimide film with the conductive layer B is placed at a temperature of 150°C for curing for 0.5h; and then placed at 380±2°C for sintering for 0.5h.
[0121] Step 5: Prepare a resistor film C, place the template C on the polyimide film, and fix the four corners of the template C with the stoppers. The third forming pattern set inside the template C is a rectangle with a length of 20 cm and a width of 6 cm, a mesh number of 100, and a film thickness of 0.1 mm.
[0122] The third carbon fiber conductive slurry is coated on the template C, and is scraped twice using an adjustable applicator, the scraper of the adjustable applicator is adjusted to 50μm, the template C is removed, and a conductive layer C with a length of 20cm and a width of 6cm, which is the same shape as the third forming pattern, is obtained on the polyimide film; the polyimide film with the conductive layer C is subjected to a third heat treatment to obtain a polyimide film with a resistor film C, the upper edge of the resistor film C is connected to the lower edge of the resistor film B, and the resistance of different positions on the resistor film C is measured using a four-probe square resistance meter, and the resistance range is 180±10%Ω / sq; wherein, the process of the third heat treatment is: first, the polyimide film with the conductive layer C is placed at a temperature of 150°C for curing for 0.5h; and then, it is placed at 380±2°C for sintering for 0.5h.
[0123] Example 3
[0124] Carbon fiber conductive paste and carbon black conductive paste are used to form high temperature resistant resistor films with three resistance values on the same polyimide film. The high temperature resistant resistor films mainly include a high temperature resistant flexible polyimide film and a carbon fiber high temperature resistant conductive paste coated on a substrate.
[0125] The specific preparation method is as follows:
[0126] Step 1: prepare carbon fiber conductive slurry and carbon black conductive slurry, wherein the components in the carbon fiber conductive slurry and carbon black conductive slurry are calculated by weight:
[0127] 1) Weigh 1.7 parts of chopped carbon fibers without adhesive having a diameter of 7 μm and a length of 0.5 mm, 50 parts of solvent B, 41.6 parts of silicone resin having a solid content of 55%, 5 parts of carbon black, and 1.7 parts of a dispersant;
[0128] The chopped carbon fiber, the dispersant and the solvent B are mixed evenly to obtain a chopped carbon fiber mixed solution; wherein, an ultrasonic cleaning machine is used for uniform dispersion, the power of the ultrasonic cleaning machine is 100W, the frequency is 40KHz, and the dispersion time is 30min;
[0129] The carbon black and the silicone resin are added into the chopped carbon fiber mixed solution and mixed evenly to obtain the carbon fiber conductive slurry; wherein, a homogenizer is used for mixing evenly, the rotation speed of the homogenizer is 1500r / min, and the dispersion time is 1h.
[0130] 2) Weigh 7.3 parts of carbon black with a particle size of 40-48 nm, 47.7 parts of silicone resin with a solid content of 55%, and 45 parts of solvent A;
[0131] The carbon black, the silicone resin and the solvent A are mixed evenly to obtain a first carbon black conductive slurry; wherein the mixing is performed evenly using a homogenizer, the speed of the homogenizer is 1000 r / min, and the dispersion time is 1 hour;
[0132] 3) Weigh 4.9 parts of conductive carbon black with a particle size of 40 to 48 nm, 62.1 parts of silicone resin with a solid content of 55%, and 33 parts of solvent A;
[0133] The carbon black, the silicone resin and the solvent A are mixed evenly to obtain a second carbon black conductive slurry; wherein the mixing is performed evenly using a homogenizer, the speed of the homogenizer is 1000 r / min, and the dispersion time is 1 hour;
[0134] Step 2: Clean the polyimide film. Soak the polyimide film in alcohol, clean it with ultrasonic waves for 5 minutes, and then dry it with a nitrogen gun. The power of the ultrasonic cleaning process is 40W and the frequency is 40KHz.
[0135] Step 3: Prepare a resistor film A, place the cleaned polyimide film on the square fixing frame, and fix the four corners of the polyimide film with the stoppers;
[0136] The template A is placed on the polyimide film, and the four corners of the template A are fixed with the stoppers. The first forming pattern set inside the template A is a rectangle with a length of 30 cm and a width of 5 cm, a screen mesh of 100, and a film thickness of 0.1 mm;
[0137] The carbon fiber conductive slurry is coated on the template A, and an adjustable applicator is used to scrape it twice, the scraper of the adjustable applicator is adjusted to 50μm, the template A is removed, and a conductive layer A with a length of 30cm and a width of 5cm, which is the same as the first forming pattern, is obtained on the polyimide film; the polyimide film with the conductive layer A is subjected to a first heat treatment to obtain a polyimide film with a resistor film A, and the resistance values at different positions on the resistor film A are measured with a four-probe square resistance meter, and the resistance range is 65±10%Ω / sq; wherein, the process of the first heat treatment is: first, the polyimide film with the conductive layer A is placed at a temperature of 150°C for curing for 0.5h; and then, it is placed at 380±2°C for sintering for 0.5h.
[0138] Step 4: Prepare a resistor film B, place the template B on the polyimide film, and fix the four corners of the template B with the stoppers. The second forming pattern set inside the template B is a rectangle with a length of 30 cm and a width of 4 cm, a screen mesh of 100, and a film thickness of 0.1 mm.
[0139] The first carbon black conductive slurry is coated on the template B, and the adjustable film applicator is used to scrape it twice, the scraper of the adjustable film applicator is adjusted to 50μm, the template B is removed, and a conductive layer B with a length of 30cm and a width of 4cm, which is the same as the shape of the second forming pattern, is obtained on the polyimide film; the polyimide film with the conductive layer B is subjected to a second heat treatment to obtain a polyimide film with a resistor film B, the upper edge of the resistor film B is connected to the lower edge of the resistor film A, and the resistance values at different positions on the resistor film B are measured using a four-probe square resistance meter, and the resistance value range is 185±10%Ω / sq; wherein, the process of the second heat treatment is: first, the polyimide film with the conductive layer B is placed at a temperature of 150°C for curing for 0.5h; and then placed at 380±2°C for sintering for 0.5h.
[0140] Step 5: Prepare a resistor film C, place the template C on the polyimide film, and fix the four corners of the template C with the stoppers. The third forming pattern set inside the template C is a rectangle with a length of 30 cm and a width of 6 cm, a mesh number of 100, and a film thickness of 0.1 mm.
[0141] The second carbon black conductive slurry is coated on the template C, and the adjustable film applicator is used to scrape it twice, the scraper of the adjustable film applicator is adjusted to 50μm, and the template C is removed to obtain a conductive layer C with a length of 30cm and a width of 6cm, which is the same as the shape of the third forming pattern, on the polyimide film; the polyimide film with the conductive layer C is subjected to a third heat treatment to obtain a polyimide film with a resistor film C, the upper edge of the resistor film C is connected to the lower edge of the resistor film B, and the resistance of different positions on the resistor film C is measured by a four-probe square resistance meter, and the resistance range is 550±10%Ω / sq; wherein, the process of the third heat treatment is: first, the polyimide film with the conductive layer C is placed at a temperature of 150°C for curing for 0.5h; and then placed at 382°C for sintering for 0.5h.
[0142] Example 4
[0143] Graphite conductive paste and carbon fiber conductive paste are used to form high temperature resistant resistor films with three resistance values on the same polyimide film. The high temperature resistant resistor films mainly include high temperature resistant flexible polyimide film, and high temperature resistant graphite conductive paste and carbon fiber conductive paste coated on the substrate.
[0144] The specific preparation method is as follows:
[0145] Step 1: Prepare graphite conductive slurry and carbon fiber conductive slurry, wherein the components in the graphite conductive slurry and carbon fiber conductive slurry are calculated by weight:
[0146] 1) Weigh 37 parts of graphite powder with a particle size of 1.3 μm, 30 parts of silicone resin with a solid content of 55%, and 33 parts of solvent A;
[0147] The graphite powder, the silicone resin and the solvent A are mixed evenly to obtain a graphite conductive slurry;
[0148] The homogenizer was used for uniform mixing, the speed of the homogenizer was 1000 r / min, and the dispersion time was 1 h;
[0149] 2) Weigh 2.5 parts of chopped carbon fibers without adhesive having a diameter of 7 μm and a length of 0.5 mm, 49.7 parts of solvent B, 41.4 parts of a silicone resin having a solid content of 55%, 4.1 parts of carbon black, and 2.3 parts of a polyvinyl pyrrolidone dispersant;
[0150] The chopped carbon fiber, the polyvinyl pyrrolidone dispersant and the solvent B are uniformly mixed to obtain a chopped carbon fiber mixed liquid;
[0151] The ultrasonic cleaning machine is used for uniform dispersion, the power of the ultrasonic cleaning machine is 100W, the frequency is 40KHz, and the dispersion time is 30min;
[0152] Adding the carbon black and the silicone resin into the chopped carbon fiber mixed solution and mixing evenly to obtain a first carbon fiber conductive slurry;
[0153] The homogenizer was used for uniform mixing, the speed of the homogenizer was 1500 r / min, and the dispersion time was 1 h;
[0154] 3) Weigh 3.5 parts of chopped carbon fibers without glue having a diameter of 7 μm and a length of 0.5 mm, 52 parts of solvent B, 34 parts of silicone resin having a solid content of 55%, 8.6 parts of carbon black, and 1.9 parts of polyvinyl pyrrolidone dispersant;
[0155] The chopped carbon fiber, the polyvinyl pyrrolidone dispersant and the solvent B are uniformly mixed to obtain a chopped carbon fiber mixed solution; wherein, an ultrasonic cleaning machine is used for uniform dispersion, the power of the ultrasonic cleaning machine is 100W, the frequency is 40KHz, and the dispersion time is 30min;
[0156] The carbon black and the silicone resin are added to the chopped carbon fiber mixed solution and mixed evenly to obtain a second carbon fiber conductive slurry; wherein the mixing is performed evenly using a homogenizer, the speed of the homogenizer is 1500 r / min, and the dispersion time is 1 hour;
[0157] Step 2: Clean the polyimide film. Soak the polyimide film in alcohol, clean it with ultrasonic waves for 5 minutes, and then dry it with a nitrogen gun. The power of the ultrasonic cleaning process is 40W and the frequency is 40KHz.
[0158] Step 3: Prepare a resistor film A, place the cleaned polyimide film on the square fixing frame, and fix the four corners of the polyimide film with the stoppers;
[0159] The template A is placed on the polyimide film, and the four corners of the template A are fixed with the stoppers. The first forming pattern set inside the template A is a rectangle with a length of 50 cm and a width of 6 cm, a screen mesh of 100, and a film thickness of 0.1 mm;
[0160] The graphite conductive slurry is coated on the template A, and an adjustable applicator is used to scrape it twice, the scraper of the adjustable applicator is adjusted to 50μm, the template A is removed, and a conductive layer A with a length of 50cm and a width of 6cm, which is the same as the first forming pattern, is obtained on the polyimide film; the polyimide film with the conductive layer A is subjected to a first heat treatment to obtain a polyimide film with a resistor film A, and the resistance values at different positions on the resistor film A are measured with a four-probe square resistance meter, and the resistance value range is 130±10%Ω / sq; wherein, the process of the first heat treatment is: first, the polyimide film with the conductive layer A is placed at a temperature of 120°C for curing for 0.5h; and then, it is placed at 380±2°C for sintering for 0.5h.
[0161] Step 4: Prepare a resistor film B, place the template B on the polyimide film, and fix the four corners of the template B with the stoppers. The second forming pattern set inside the template B is a rectangle with a length of 50 cm and a width of 4 cm, a screen mesh of 100, and a film thickness of 0.1 mm.
[0162] The first carbon fiber conductive slurry is coated on the template B, and an adjustable applicator is used to scrape it twice, the scraper of the adjustable applicator is adjusted to 50μm, the template B is removed, and a conductive layer B with a length of 50cm and a width of 4cm, which is the same as the shape of the second forming pattern, is obtained on the polyimide film; the polyimide film with the conductive layer B is subjected to a second heat treatment to obtain a polyimide film with a resistor film B, the upper edge of the resistor film B is connected to the lower edge of the resistor film A, and the resistance values at different positions on the resistor film B are measured using a four-probe square resistance meter, and the resistance value range is 60±10%Ω / sq; wherein, the process of the second heat treatment is: first, the polyimide film with the conductive layer B is placed at a temperature of 150°C for curing for 0.5h; and then placed at 380±2°C for sintering for 0.5h.
[0163] Step 5: Prepare a resistor film C, place the template C on the polyimide film, and fix the four corners of the template C with the stoppers. The third forming pattern set inside the template C is a rectangle with a length of 50 cm and a width of 8 cm, a screen mesh of 100, and a film thickness of 0.1 mm.
[0164] The second carbon fiber conductive slurry is coated on the template C, and an adjustable applicator is used to scrape it twice, the scraper of the adjustable applicator is adjusted to 50μm, the template C is removed, and a conductive layer C with a length of 50cm and a width of 8cm, which is the same as the shape of the third forming pattern, is obtained on the polyimide film; the polyimide film with the conductive layer C is subjected to a third heat treatment to obtain a polyimide film with a resistor film C, the upper edge of the resistor film C is connected to the lower edge of the resistor film B, and the resistance of different positions on the resistor film C is measured by a four-probe square resistance meter, and the resistance range is 50±10%Ω / sq; wherein, the process of the third heat treatment is: first, the polyimide film with the conductive layer C is placed at a temperature of 150°C for curing for 0.5h; and then placed at 380±2°C for sintering for 0.5h.
[0165] Example 5
[0166] Carbon black conductive paste is used to form two high-temperature resistant resistor films with different resistance values on the same polyimide film. The high-temperature resistant resistor films mainly include a high-temperature resistant flexible polyimide film and a high-temperature resistant carbon black conductive paste coated on a substrate.
[0167] The specific preparation method is as follows:
[0168] Step 1: prepare carbon black conductive slurry, wherein the components in the carbon black conductive slurry are calculated by weight:
[0169] 1) Weigh 4.9 parts of carbon black with a particle size of 40 to 48 nm, 62.1 parts of silicone resin with a solid content of 55%, and 33 parts of solvent A;
[0170] The carbon black, the silicone resin and the solvent A are mixed evenly to obtain a first carbon black conductive slurry;
[0171] The homogenizer was used for uniform mixing, the speed of the homogenizer was 1000 r / min, and the dispersion time was 1 h;
[0172] 2) Weigh 7.3 parts of conductive carbon black with a particle size of 40 to 48 nm, 47.7 parts of silicone resin with a solid content of 55%, and 45 parts of solvent A;
[0173] The carbon black, the silicone resin and the solvent A are mixed evenly to obtain a second carbon black conductive slurry; wherein the mixing is performed evenly using a homogenizer, the speed of the homogenizer is 1000 r / min, and the dispersion time is 1 hour;
[0174] Step 2: Clean the polyimide film. Soak the polyimide film in alcohol, clean it with ultrasonic waves for 5 minutes, and then dry it with a nitrogen gun. The power of the ultrasonic cleaning process is 40W and the frequency is 40KHz.
[0175] Step 3: Prepare a resistor film A, place the cleaned polyimide film on the square fixing frame, and fix the four corners of the polyimide film with the stoppers;
[0176] The template A is placed on the polyimide film, and the four corners of the template A are fixed with the stoppers. The first forming pattern set inside the template A is a rectangle with a length of 50 cm and a width of 4 cm, a screen mesh of 100, and a film thickness of 0.1 mm;
[0177] The first carbon black conductive slurry is coated on the template A, and an adjustable applicator is used to scrape it twice, the scraper of the adjustable applicator is adjusted to 50μm, and the template A is removed to obtain a conductive layer A with a length of 50cm and a width of 4cm, which is the same as the first forming pattern, on the polyimide film; the polyimide film with the conductive layer A is subjected to a first heat treatment to obtain a polyimide film with a resistor film A, and the resistance values at different positions on the resistor film A are measured with a four-probe square resistance meter, and the resistance value range is 550±10%Ω / sq; wherein, the process of the first heat treatment is: first, the polyimide film with the conductive layer A is placed at a temperature of 150°C for curing for 0.5h; and then, it is placed at 380±2°C for sintering for 0.5h.
[0178] Step 4: Prepare a resistor film B, place the template B on the polyimide film, and fix the four corners of the template B with the stoppers. The second forming pattern set inside the template B is a rectangle with a length of 50 cm and a width of 5 cm, a screen mesh of 100, and a film thickness of 0.1 mm.
[0179] The second carbon black conductive slurry is coated on the template B, and is scraped twice by an adjustable applicator, the scraper of the adjustable applicator is adjusted to 50μm, the template B is removed, and a conductive layer B with a length of 50cm and a width of 5cm, which is the same as the shape of the second forming pattern, is obtained on the polyimide film; the polyimide film with the conductive layer B is subjected to a second heat treatment to obtain a polyimide film with a resistor film B, the upper edge of the resistor film B is connected to the lower edge of the resistor film A, and the resistance values at different positions on the resistor film B are measured by a four-probe square resistance meter, and the resistance value range is 185±10%Ω / sq; wherein, the process of the second heat treatment is: first, the polyimide film with the conductive layer B is placed at a temperature of 150°C for curing for 0.5h; and then, it is placed at 380±2°C for sintering for 0.5h.
[0180] The above description is only a specific embodiment of the present invention, so that those skilled in the art can understand or implement the present invention. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present invention.
[0181] It should be understood that the present invention is not limited to what has been described above and that various modifications and changes may be made without departing from its scope. The scope of the present invention is limited only by the appended claims.
Claims
1. A continuous gradient high temperature resistant resistor film, characterized in that: include: The high temperature resistant conductive functional layer is distributed on the substrate, and the high temperature resistant conductive functional layer is formed by sequentially curing conductive pastes of different resistance values with organic silicone resin as a binder in the order of resistance from small to large or from large to small.
2. The method for preparing a continuous gradient high temperature resistant resistor film according to claim 1, characterized in that: Conductive pastes with different resistance values are made by using organic silicon resin as a binder, and the conductive pastes with different resistance values are cured on the same substrate in the order of resistance from small to large or from large to small, so as to obtain a resistor film with a continuously gradient resistance value.
3. The method for preparing a continuous gradient high temperature resistant resistor film according to claim 2, characterized in that: The specific steps include: Step 1, preparing a conductive paste: using silicone resin as a binder to prepare conductive pastes of different resistance values, and dividing the conductive pastes into conductive paste A, conductive paste B, and conductive paste C in order of resistance from small to large or from large to small; Step 2, preparing the template: preparing the template A, template B, and template C required for screen printing, wherein: the template A is provided with a first forming pattern, and the distance between the upper side length of the first forming pattern and the upper frame of the template A is b; the template B is provided with a second forming pattern, and the distance between the upper side length of the second forming pattern and the upper frame of the template A is b+h1; the template C is provided with a second forming pattern, and the distance between the upper side length of the second forming pattern and the upper frame of the template A is b+h1+h2; Step 3. Preparation of a continuous gradient high-temperature resistant resistor film: fix template A on the cleaned substrate, print conductive paste A onto the substrate through template A, and obtain a substrate with resistor film A after heat treatment; fix template B and template C on the same substrate in sequence, print conductive paste B through template B and conductive paste C through template C in the same way, and then obtain a substrate with resistor film A, resistor film B, and resistor film C after heat treatment.
4. The method for preparing a continuous gradient high temperature resistant resistor film according to claim 3, characterized in that: In the step 1, the conductive paste A, the conductive paste B, and the conductive paste C are all carbon black conductive paste, graphite conductive paste, or carbon fiber conductive paste.
5. The method for preparing a continuous gradient high temperature resistant resistor film according to claim 4, characterized in that: In the process of preparing carbon black conductive slurry, the following raw materials are included by weight: 4 to 10 parts of carbon black, 30 to 65 parts of silicone resin, and 30 to 55 parts of the first solvent.
6. The method for preparing a continuous gradient high temperature resistant resistor film according to claim 4, characterized in that: In the process of preparing graphite conductive slurry, the following raw materials are included by mass: 20 to 40 parts of graphite powder, 20 to 50 parts of silicone resin, and 20 to 40 parts of a first solvent.
7. The method for preparing a continuous gradient high temperature resistant resistor film according to claim 4, characterized in that: In the process of preparing carbon fiber conductive slurry, the following raw materials are included by mass: 1.2 to 3.5 parts of chopped carbon fibers, 4 to 9 parts of carbon black, 10 to 45 parts of silicone resin, 1 to 2.5 parts of dispersant, and 49 to 55 parts of a second solvent.
8. The method for preparing a continuous gradient high temperature resistant resistor film according to claim 3, characterized in that: In the step three, the template A, template B, template C and the substrate are fixed by a template positioning tool, and the template positioning tool comprises a square fixing frame (2) and four limiters (1), and the four limiters (1) are respectively located on the four top corners of the square fixing frame (2), and the area defined by the four limiters (1) is the same as the area of the template A.
9. The method for preparing a continuous gradient high temperature resistant resistor film according to claim 3, characterized in that: The heat treatment in step three is: firstly, the substrate with the conductive layer A is placed at a temperature of 120° C. to 150° C. for curing for 0.5 h to 1 h, and then placed at 380±2° C. for sintering for 0.5 h.
10. The method for preparing a continuous gradient high temperature resistant resistor film according to claim 2, characterized in that: The substrate is a polyimide film, a glass fiber silicone cloth or a high-silica glass fiber cloth.