Method for improving conductivity of copper-loaded porous carbon electrode
The preparation of copper oxide/porous carbon electrodes through hydrothermal treatment and electrochemical conversion solves the problem of poor conductivity of porous carbon electrodes, thereby improving the performance and reducing the cost of supercapacitors. This method is suitable for supercapacitor electrode materials.
Patent Information
- Application Number
- CN202411191983.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-08-28
AI Technical Summary
The poor conductivity of existing porous carbon electrode materials limits the performance improvement of supercapacitors, and existing reduction methods may damage the electrode structure or affect the material properties.
A copper oxide/porous carbon composite material was prepared by mixing copper source with porous carbon using a hydrothermal treatment method. The composite material was then converted into elemental copper through electrochemical charge-discharge and loaded onto the surface and pores of the porous carbon to form a copper oxide/porous carbon electrode.
It improves the conductivity and stability of the electrodes, enhances the charging and discharging efficiency and energy density of supercapacitors, and has a simple and low-cost preparation method, making it suitable for industrial production.
Smart Images

Figure CN118942916A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of copper-loaded porous carbon electrodes, and in particular relates to a method for improving the conductivity of copper-loaded porous carbon electrodes. Background Art
[0002] Supercapacitors are a new type of energy storage device between traditional capacitors and batteries, with the advantages of fast charging and discharging speed, long cycle life, and high energy density. Among them, the electrode material is the key factor affecting the electrochemical performance of supercapacitors. Porous carbon is widely used as the electrode material of supercapacitors due to its large specific surface area, good chemical stability, and low cost. However, porous carbon electrode materials have the problem of poor conductivity, which limits the performance improvement of supercapacitors.
[0003] Copper has good electrical conductivity, and loading it onto porous carbon can improve its conductivity. In the prior art, copper ions are generally reduced to copper elements through solid reduction, solution reduction, and electrochemical reduction. The solid reduction method requires a relatively high temperature, generally above 500°C, which is prone to secondary damage to the electrode structure; the solution reduction method requires the addition of chemical reducing agents, such as iron powder, which will affect the performance of the material; the electrochemical reduction method is to electrolyze a solution containing copper ions, but the electrolysis efficiency is slow and copper is only reduced on the electrode surface. Therefore, there is an urgent need for a method for preparing a copper-loaded porous carbon electrode that can improve the conductivity and stability of the electrode. Summary of the invention
[0004] In view of the defects of the prior art, the present invention aims to provide a method for improving the conductivity of copper-loaded porous carbon electrodes.
[0005] In order to achieve the above object, the present invention adopts the following technical solutions: A method for improving the conductivity of a copper-loaded porous carbon electrode comprises the following steps: (1) mixing a copper source and porous carbon in deionized water to obtain a mixed solution; (2) placing the mixed solution in a hydrothermal reactor and performing hydrothermal treatment in an oven at 150°C to 220°C for 12 to 36 h. After the reactor is naturally cooled to room temperature, the reaction product is obtained by centrifugal separation. The product is then repeatedly washed with deionized water and ethanol solution, and vacuum dried at 55 to 65°C for 12 to 15 h to obtain a copper oxide / porous carbon composite material. (3) The copper oxide / porous carbon composite material is made into a copper oxide / porous carbon electrode, which is then charged and discharged once in a three-electrode system to obtain a copper-loaded porous carbon electrode.
[0006] In step (1), the copper source is one or more of copper acetate, copper chloride, and copper sulfate.
[0007] In step (1), the mass ratio of the copper source to the porous carbon is 1:1-1:9, preferably 1:3-1:6. With this ratio range, the copper source can be more evenly dispersed on the surface of the porous carbon.
[0008] In step (2), the specific surface area of the copper oxide / porous carbon is 800-3000m 2 / g.
[0009] In step (3), the preparation method of the copper oxide / porous carbon electrode is: the copper oxide / porous carbon composite material and the binder are evenly mixed and then coated on the nickel foam to obtain the copper oxide / porous carbon electrode; wherein the binder is PVDF, and the mass ratio of the copper oxide / porous carbon composite material to PVDF is 9:1.
[0010] In step (3), the current density of one charge and discharge is 0.001A / g~10A / g.
[0011] The copper-loaded porous carbon electrode is used in a supercapacitor, and the copper-loaded porous carbon is used as an electrode material to assemble a supercapacitor.
[0012] The present invention has the following beneficial effects: 1. The present invention loads copper oxide onto the surface and pores of porous carbon, and irreversibly converts copper oxide into copper element through electrochemical charge and discharge. The copper is introduced into the activated carbon electrode, which improves the conductivity of the electrode, reduces the internal resistance of the electrode, and is beneficial to improving the charge and discharge efficiency of the supercapacitor.
[0013] 2. The copper oxide / porous carbon electrode of the present invention does not require a conductive agent when used as an electrode material, thereby improving the energy density of the electrode.
[0014] 3. The preparation method of copper-loaded porous carbon electrode is simple, low-cost and easy to realize industrial production.
[0015] 4. Compared with the prior art, the copper-loaded porous carbon prepared by the present invention has excellent energy density and power density and is an ideal supercapacitor electrode material. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 This is a scanning electron microscope image of the copper oxide / porous carbon prepared in Example 1.
[0017] Figure 2 Cyclic voltammetry curves of the copper-loaded porous carbon prepared in Example 1 at different scanning rates. DETAILED DESCRIPTION
[0018] The present invention is further described in detail below in conjunction with specific examples. These examples are implemented based on the technical solution of the present invention, and provide detailed implementation methods and specific operation processes, but the protection scope of the present invention is not limited to these examples.
[0019] All technical and scientific terms used in the present invention have the same meaning as commonly understood by one of ordinary skill in the art to which this application belongs. Example 1
[0020] A method for improving the conductivity of a copper-loaded porous carbon electrode comprises the following steps: (1) Copper acetate and porous carbon were weighed in a mass ratio of 1:5. The copper acetate was first dissolved in 50 mL of deionized water, and then the porous carbon was added. The mixture was shaken on a shaker for 1 h to obtain a mixed solution. (2) The mixed solution was transferred to a hydrothermal reactor and subjected to hydrothermal treatment in an oven at 180°C for 24 h. After the reactor was naturally cooled to room temperature, the reaction product was separated by centrifugation, and then repeatedly washed with deionized water and ethanol solution and vacuum dried at 60°C for 12 h to obtain a copper oxide / porous carbon composite material. (3) The copper oxide / porous carbon composite material and the binder PVDF were mixed evenly in a mass ratio of 9:1, and then coated on the nickel foam to obtain a copper oxide / porous carbon electrode; (4) The obtained copper oxide / porous carbon electrode was charged and discharged for one cycle in a three-electrode system with a charge and discharge current density of 0.5 A / g to obtain a copper-loaded porous carbon electrode.
[0021] The specific surface area of the copper oxide / porous carbon prepared in this example is 2500 m 2 The prepared copper-loaded porous carbon electrode was assembled on a supercapacitor, and a mass specific capacity of 500 F / g was obtained at a current density of 0.5 A / g, and a mass specific capacity of 280 F / g was obtained at a high current density of 10 A / g. The capacity retention rate was 92% after 10,000 cycles.
[0022] Figure 2Cyclic voltammetry curves of copper-loaded porous carbon prepared in Example 1 at different scan rates. It can be seen that when the scan rate is 5 mV / s, the cyclic voltammetry curve area is the smallest, and the increase in scan rate is accompanied by the expansion of the integral area of the cyclic voltammetry curve, and the redox peak on the curve gradually becomes less obvious. This is because at a lower scan rate, the electrolyte ions can be more fully diffused to produce more effective surfaces for Faraday redox reactions. As the scan rate increases, the diffusion time of the electrolyte ions to the active sites of the internal reaction of the electrode is limited, and incomplete Faraday redox reactions occur. When the scan rate reaches 200 mV / s, the curve is close to a rectangular shape, showing good capacitance characteristics, and due to the weak polarization of the electrode, the redox peak position changes slightly, indicating that the prepared composite material has a good reversible charge and discharge capability. Example 2
[0023] A method for improving the conductivity of a copper-loaded porous carbon electrode comprises the following steps: (1) Copper acetate and porous carbon were weighed in a mass ratio of 1:8. The copper acetate was first dissolved in 50 mL of deionized water, and then the porous carbon was added. The mixture was shaken on a shaker for 1 h to obtain a mixed solution. (2) The mixed solution was transferred to a hydrothermal reactor and subjected to hydrothermal treatment in an oven at 22 °C for 24 h. After the reactor was naturally cooled to room temperature, the reaction product was obtained by centrifugal separation. The product was then repeatedly washed with deionized water and ethanol solution and vacuum dried at 60 °C for 12 h to obtain a copper oxide / porous carbon composite material. (3) The copper oxide / porous carbon composite material and the binder PVDF were mixed evenly in a mass ratio of 9:1, and then coated on the nickel foam to obtain a copper oxide / porous carbon electrode; (4) The obtained copper oxide / porous carbon electrode was charged and discharged for one cycle in a three-electrode system with a charge and discharge current density of 0.5 A / g to obtain a copper-loaded porous carbon electrode.
[0024] The specific surface area of the copper oxide / porous carbon prepared in this example is 1500 m 2 The prepared copper-loaded porous carbon electrode was assembled on a supercapacitor, and a mass specific capacity of 350 F / g was obtained at a current density of 0.5 A / g, and a mass specific capacity of 160 F / g was obtained at a high current density of 10 A / g. The capacity retention rate was 91% after 10,000 cycles. Example 3
[0025] A preparation method for improving the conductivity of a copper-loaded porous carbon electrode comprises the following steps: (1) Copper acetate and porous carbon were weighed in a mass ratio of 1:2. The copper acetate was first dissolved in 50 mL of deionized water, and then the porous carbon was added. The mixture was shaken on a shaker for 1 h to obtain a mixed solution. (2) The mixed solution was transferred to a hydrothermal reactor and subjected to hydrothermal treatment in an oven at 190 °C for 24 h. After the reactor was naturally cooled to room temperature, the reaction product was obtained by centrifugal separation. The product was then repeatedly washed with deionized water and ethanol solution and vacuum dried at 60 °C for 12 h to obtain a copper oxide / porous carbon composite material. (3) The copper oxide / porous carbon composite material and the binder PVDF were mixed evenly in a mass ratio of 9:1, and then coated on the nickel foam to obtain a copper oxide / porous carbon electrode; (4) The obtained copper oxide / porous carbon electrode was charged and discharged for one cycle in a three-electrode system with a charge and discharge current density of 0.5 A / g to obtain a copper-loaded porous carbon electrode.
[0026] The specific surface area of the copper oxide / porous carbon prepared in this example is 800 m 2 The prepared copper-loaded porous carbon electrode was assembled on a supercapacitor, and a mass specific capacity of 250 F / g was obtained at a current density of 0.5 A / g, and a mass specific capacity of 130 F / g was obtained at a high current density of 10 A / g. The capacity retention rate was 95% after 10,000 cycles.
Claims
1. A method for improving the conductivity of copper-loaded porous carbon electrodes. It is characterized in that The following steps are involved: (1) mixing a copper source and porous carbon in water to obtain a mixed solution; (2) placing the mixed solution in a hydrothermal reactor and performing hydrothermal treatment in an oven at 150°C to 220°C for 12 to 36 hours. After the reactor is cooled to room temperature, the reaction product is obtained by centrifugal separation. The product is then washed and dried to obtain a copper oxide / porous carbon composite material. (3) The copper oxide / porous carbon composite material is made into a copper oxide / porous carbon electrode, which is then charged and discharged once in a three-electrode system to obtain a copper-loaded porous carbon electrode.
2. A method for improving the conductivity of a copper-loaded porous carbon electrode according to claim 1, It is characterized in that In step (1), the copper source is one or more of copper acetate, copper chloride, and copper sulfate.
3. A method for improving the conductivity of a copper-loaded porous carbon electrode according to claim 1, It is characterized in that In step (1), the mass ratio of the copper source to the porous carbon is 1:1 to 1:
9.
4. A method for improving the conductivity of a copper-loaded porous carbon electrode according to claim 1, It is characterized in that The specific surface area of the copper oxide / porous carbon is 800-3000m 2 / g.
5. A method for improving the conductivity of a copper-loaded porous carbon electrode according to claim 1, It is characterized in that In step (3), the copper oxide / porous carbon electrode is prepared by mixing the copper oxide / porous carbon composite material and a binder evenly and then coating the mixture on nickel foam to obtain a copper oxide / porous carbon electrode.
6. A method for improving the conductivity of a copper-loaded porous carbon electrode according to claim 5, It is characterized in that The binder is PVDF, and the mass ratio of the copper oxide / porous carbon composite material to PVDF is 9:
1.
7. A method for improving the conductivity of a copper-loaded porous carbon electrode according to claim 1, It is characterized in that In step (3), the current density of one charge and discharge is 0.001A / g~10A / g.
8. A copper-loaded porous carbon electrode is obtained according to the method described in any one of claims 1 to 7.
9. Use of the copper-loaded porous carbon electrode as claimed in claim 8 in a supercapacitor.
Citation Information
Patent Citations
Porous active carbon / copper ion super-capacitor preparation method
CN105609327A
In-situ nitrogen-doped porous carbon microsphere / copper matrix composite material and preparation method and application thereof
CN109273284A
Method for preparing three-dimensional biomass carbon / copper sulfide as electrode material
CN110697706A
Preparation method and application of CuO / graphene composite material
CN113809318A
Active carbon-transition metal oxide for electrode active material and manufacturing method of the same
KR1020130116455A