Manufacturing method of eflash storage unit and storage unit
By forming an oxide layer side wall behind the ONO gate structure during the manufacturing process of the eflash memory cell and performing double etching, the problem of lateral etching of the ONO layer during the removal of the hard mask is solved, and the reliability of the memory cell is improved and productivity.
Patent Information
- Application Number
- CN202411002166.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-11-12
AI Technical Summary
During the manufacturing process of the eflash memory cell, the ONO layer in the SONOS structure is susceptible to lateral etching and causes defects, which affects the reliability of the memory cell.
After forming the ONO gate structure, an oxide layer side wall is formed on the first part of the polysilicon layer and the side walls of the ONO gate structure, and the ONO gate and logic gate structure are respectively formed by etching the polysilicon layer twice to avoid removal Transverse etching of the ONO layer during hard masking.
Improves the reliability of the eflash storage unit, reduces damage to the ONO layer, and improves production efficiency and reduces manufacturing costs.
Smart Images

Figure CN118943020A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of semiconductor technology, and in particular to a manufacturing method of an eflash storage unit and a storage unit. Background Art
[0002] Non-volatile memory is a type of memory that can store data even after the power is turned off. Currently, EFlash (embedded flash memory) memory with SONOS (Silicon-Oxide-Nitride-Oxide-Silicon) structure is a non-volatile memory that has the advantages of low operating voltage, fast read and write speed, and large storage capacity. It is widely used in electronic devices such as embedded systems and mobile devices.
[0003] The eflash storage unit with SONOS structure includes a logic device and a SONOS structure, which mainly relies on silicon nitride SiNx with uniform nitrogen / silicon atomic ratio and density as a storage medium. The bottom of the silicon nitride is connected to the tunnel oxide layer (Tunnel Oxide). During the programming process, electrons are excited to tunnel from the channel into the silicon nitride; the top of the silicon nitride is covered with a scheduling oxide layer (Block Oxide) to prevent charge loss. However, in the current manufacturing process of the eflash storage unit, the process of manufacturing the logic gate structure of the logic device is prone to lateral etching of the ONO (Oxide-Nitride-Oxide) layer in the SONOS structure to produce corresponding defects, affecting the reliability of the eflash storage unit.
[0004] Therefore, how to reduce the damage to the ONO layer during the manufacturing process of the eflash memory cell becomes a problem that needs to be solved. Summary of the invention
[0005] Based on the above problems, the present application provides a method for manufacturing an eflash storage unit and a storage unit.
[0006] The embodiments of the present application disclose the following technical solutions:
[0007] In a first aspect, an embodiment of the present application provides a method for manufacturing an eflash storage unit, wherein the eflash storage unit includes a logic device and a SONOS structure, and the method includes:
[0008] Providing a substrate; the substrate comprises a logic region and a SONOS region, the substrate of the logic region comprises a substrate, a gate oxide layer, and a first portion of a polysilicon layer stacked in sequence, and the substrate of the SONOS region comprises a substrate, an ONO layer formed by stacking a first oxide layer, a first nitride layer, and a second oxide layer, and a second portion of a polysilicon layer, stacked in sequence;
[0009] forming a hard mask; the hard mask exposing a second portion of the polysilicon layer located in a non-ONO gate structure formation region; the hard mask comprising a nitride layer;
[0010] Etching the second portion of the polysilicon layer and the ONO layer to form an ONO gate structure;
[0011] Forming an oxide layer sidewall on the first portion of the polysilicon layer and the sidewall of the ONO gate structure;
[0012] Etching the first portion of the polysilicon layer and the gate oxide layer to form a logic gate structure;
[0013] removing the hard mask;
[0014] By ion implantation, a lightly doped drain region and a source-drain implantation region are formed to obtain an eflash storage unit.
[0015] Optionally, forming an oxide layer sidewall on the first portion of the polysilicon layer and the sidewall of the ONO gate structure includes:
[0016] forming a third oxide layer on the first portion of the polysilicon layer and on the sidewalls of the ONO gate structure;
[0017] The first portion of the polysilicon layer and the surface of the ONO gate structure facing away from the substrate and the third oxide layer located on the surface of the substrate are removed to form oxide layer sidewalls.
[0018] Optionally, the third oxide layer is formed by chemical vapor deposition or thermal oxidation.
[0019] Optionally, etching the second portion of the polysilicon layer and the ONO layer to form an ONO gate structure includes:
[0020] dry etching the second portion of the polysilicon layer to obtain a control gate;
[0021] The ONO layer is dry-etched to expose the substrate, forming an ONO gate structure including the etched ONO layer and a control gate.
[0022] Optionally, etching the first portion of the polysilicon layer and the gate oxide layer to form a logic gate structure includes:
[0023] Etching the hard mask to expose a first portion of the polysilicon layer located in a formation area of a non-logic gate structure;
[0024] Under the mask of the etched hard mask, the first portion of the polysilicon layer and the gate oxide layer are etched to form a logic gate structure.
[0025] Optionally, the substrate is prepared by the following process:
[0026] Providing a substrate; the substrate is a silicon substrate;
[0027] forming an ONO layer consisting of a first oxide layer, a first nitride layer and a second oxide layer stacked in sequence on the substrate;
[0028] Etching the ONO layer located in the logic area to expose the substrate;
[0029] forming a gate oxide layer on the surface of the substrate in the logic region;
[0030] A polysilicon layer is grown on the side of the gate oxide layer and the ONO layer away from the substrate to obtain a base; the polysilicon layer includes a first portion of the polysilicon layer located in the logic region and a second portion of the polysilicon layer located in the SONOS region.
[0031] Optionally, after etching the first portion of the polysilicon layer and the gate oxide layer to form a logic gate structure, the method further includes:
[0032] removing the hard mask;
[0033] By ion implantation, a lightly doped drain region and a source-drain implantation region are formed.
[0034] Optionally, in the ONO layer, the thickness of the first oxide layer is in the range of The thickness of the first nitride layer is in the range of The thickness of the second oxide layer is in the range of
[0035]
[0036] Optionally, removing the hard mask includes:
[0037] The hard mask is removed by wet etching using a phosphoric acid solution.
[0038] In a second aspect, an embodiment of the present application provides an eflash storage unit, wherein the eflash storage unit includes a logic device and a SONOS structure, and the manufacturing method of the eflash storage unit described in any implementation manner of the first aspect is applied during the manufacturing process.
[0039] Compared with the prior art, this application has the following beneficial effects:
[0040] The embodiment of the present application provides a method for manufacturing an eflash storage unit, wherein the eflash storage unit includes a logic device and a SONOS structure, and the method includes: first, providing a substrate; the substrate includes a logic region and a SONOS region, the substrate of the logic region includes a substrate, a gate oxide layer, and a first part of a polysilicon layer stacked in sequence, and the substrate of the SONOS region includes a substrate, an ONO layer formed by stacking a first oxide layer, a first nitride layer, and a second oxide layer, and a second part of a polysilicon layer, which are stacked in sequence; then, forming a hard mask; the hard mask exposes the second part of the polysilicon layer located in a formation region of a non-logic gate structure; then, etching the second part of the polysilicon layer and the ONO layer to form an ONO gate structure; then, forming an oxide layer sidewall on the first part of the polysilicon layer and the sidewall of the ONO gate structure; finally, etching the first part of the polysilicon layer and the gate oxide layer to form a logic gate structure. Therefore, in the process of manufacturing the eflash storage unit, after the ONO gate structure is formed, the side wall of the ONO layer is protected by the oxide layer sidewall, which not only ensures the etching accuracy of the logic gate structure of the logic device, but also avoids the ONO layer being lateral etched and causing defects in the process of removing the hard mask in the subsequent process of removing the hard mask because the ONO layer and the hard mask have the same composition, thereby reducing the damage to the ONO layer in the manufacturing process of the eflash storage unit and improving the reliability of the eflash storage unit. In addition, the polysilicon layer formed once is etched twice to form the ONO gate structure and the logic gate structure respectively, reducing the number of polysilicon layer growth times, which can improve production efficiency and reduce manufacturing costs. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0042] Figure 1 A flow chart of a method for manufacturing an eflash storage unit provided in an embodiment of the present application;
[0043] Figure 2A-2H A device structure diagram in each step of a method for manufacturing an eflash storage unit provided in an embodiment of the present application. DETAILED DESCRIPTION
[0044] The manufacturing method of an eflash memory unit and a memory unit provided in the present application can be used in the semiconductor field. The above is only an example and does not limit the application field of the manufacturing method of an eflash memory unit and a memory unit provided in the present application.
[0045] At present, EFlash storage cells with SONOS structure are widely used in various electronic products such as single-chip microcomputers as a non-volatile memory due to their advantages of low operating voltage, fast read and write speed and large storage capacity. In the process of integrating SONOS structure with logic device technology, it is usually necessary to use silicon nitride as a hard mask for etching to form the logic gate structure of the logic device, so as to obtain higher etching accuracy.
[0046] However, the inventors found that since the hard mask needs to be removed after etching is completed, and wet etching is usually used as a method for removing the hard mask, the ONO layer in the SONOS structure has an oxide layer and a nitride layer. During the wet etching process to remove the hard mask, its sidewalls are susceptible to lateral etching and defects, resulting in damage to the ONO layer, affecting the reliability of the eflash storage unit.
[0047] In view of this, the present application provides a method for manufacturing an eflash storage unit, in which, after forming an ONO gate structure in a SONOS structure, an oxide layer sidewall is formed on the first part of the polysilicon layer and the sidewall of the ONO gate structure. Thus, in the process of manufacturing the eflash storage unit, after forming the ONO gate structure, the sidewall of the ONO layer is protected by the oxide layer sidewall, which not only ensures the etching accuracy of the logic gate structure of the logic device, but also avoids the ONO layer being lateral etched and causing defects in the process of removing the hard mask in the subsequent process of removing the hard mask due to the ONO layer and the hard mask having the same nitride, thereby reducing the damage to the ONO layer in the manufacturing process of the eflash storage unit and improving the reliability of the eflash storage unit. In addition, the polysilicon layer formed once is etched twice to form an ONO gate structure and a logic gate structure respectively, which reduces the number of polysilicon layer growths, can effectively improve production efficiency, and reduce manufacturing costs.
[0048] In order to enable those skilled in the art to better understand the solution of the present application, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.
[0049] See also Figure 1 , which is a flow chart of a method for manufacturing an eflash storage unit provided in an embodiment of the present application, and is applied to manufacturing an eflash storage unit including a logic device and a SONOS structure, the method comprising:
[0050] S101: providing a substrate.
[0051] Specifically, see Figure 2A The substrate includes a logic region i and a SONOS region ii, wherein the substrate of the logic region i includes a substrate 10, a gate oxide layer 11, and a first portion 12 of a polysilicon layer stacked in sequence; the substrate of the SONOS region ii includes a substrate 10, an ONO layer 21 formed by stacking a first oxide layer 211, a first nitride layer 212, and a second oxide layer 213, and a second portion 22 of a polysilicon layer stacked in sequence.
[0052] Optionally, a silicon substrate 10 may be provided, and an ONO layer 21 consisting of a first oxide layer 211, a first nitride layer 212, and a second oxide layer 213 stacked in sequence may be first formed on the silicon substrate 10; the ONO layer 21 located in the logic area may be etched to expose the silicon substrate 10 in the logic area; then, a gate oxide layer 11 may be formed on the surface of the silicon substrate 10 in the logic area; finally, a polysilicon layer may be grown on a side of the gate oxide layer 11 and the ONO layer 21 facing away from the substrate 10 to form a first portion 12 of the polysilicon layer located in the logic area i and a second portion 22 of the polysilicon layer located in the SONOS area ii, thereby obtaining a base.
[0053] Exemplarily, in the ONO layer 21, the thickness of the first oxide layer 211 is in the range of The thickness of the first nitride layer 212 is in the range of The thickness of the second oxide layer 213 is in the range of The first oxide layer 211 is a tunneling oxide layer, the first nitride layer 212 is a storage medium, and the second oxide layer 213 is a scheduling oxide layer. During the programming process, electrons are excited and enter the first nitride layer 212 through the first oxide layer 211, and the second oxide layer 213 can prevent charge loss, thereby realizing data storage. Optionally, the first oxide layer 211 and the second oxide layer 213 are both silicon oxide layers, and the first nitride layer 212 is a silicon nitride layer.
[0054] S102 : forming a hard mask 51 .
[0055] Optionally, the hard mask 51 may be a nitride layer or a stack of an oxide layer and a nitride layer. For example, the hard mask 51 is a stack of silicon oxide and silicon nitride, wherein silicon oxide is located on a side of the hard mask 51 close to the substrate 10, and silicon nitride is located on a side of the hard mask 51 away from the substrate 10.
[0056] As an example, silicon oxide and silicon nitride may be deposited in sequence on the side of the base facing away from the substrate 10 to form a stack of silicon oxide and silicon nitride; then, the stack of silicon oxide and silicon nitride is etched to expose the second portion of the polysilicon layer located in the formation area of the non-ONO gate structure to obtain a hard mask 51.
[0057] S103 : etching the second portion 22 of the polysilicon layer and the ONO layer 21 to form an ONO gate structure 31 .
[0058] See also Figure 2B , the hard mask 51 shown in the figure is a nitride layer. As an example, the non-ONO gate structure 31 formation area in the second portion 22 of the polysilicon layer can be dry-etched first to obtain a control gate 311; then, the non-ONO gate structure 31 formation area in the ONO layer 21 is dry-etched to the exposed substrate 10 to form an ONO gate structure 31 including the etched ONO layer and the control gate 311.
[0059] S104 : forming an oxide layer spacer 41 on the first portion 12 of the polysilicon layer and the sidewall of the ONO gate structure 31 .
[0060] Specifically, see Figure 2C , a third oxide layer may be formed on the side of the base away from the substrate 10; and then the first portion 12 of the polysilicon layer and the surface of the ONO gate structure 31 away from the substrate 10 and the third oxide layer on the surface of the substrate 10 are removed to form an oxide layer sidewall 41. Optionally, after the oxide layer sidewall is formed, the remaining hard mask 51 may be removed first.
[0061] Optionally, a third oxide layer can be formed by, for example, chemical vapor deposition or thermal oxidation, and the first portion 12 of the polysilicon layer and the surface of the ONO gate structure 31 facing away from the substrate 10 and the third oxide layer located on the surface of the substrate 10 are removed by, for example, dry etching to form an oxide layer sidewall 41.
[0062] Alternatively, if Figure 2D After the oxide layer sidewall 41 is formed, the hard mask 51 can be removed first, and then silicon oxide and silicon nitride can be deposited again on the side of the substrate facing away from the substrate 10 to form a stack of silicon oxide and silicon nitride; or silicon oxide and silicon nitride can be deposited again on the side of the substrate facing away from the substrate 10 directly on the basis of the original hard mask. In this way, in the subsequent process of forming the logic gate structure 61, the part that does not need to be etched can be more comprehensively protected.
[0063] S105 : etching the first portion 12 of the polysilicon layer and the gate oxide layer 11 to form a logic gate structure 61 .
[0064] The hard mask 51 is photolithographically defined in the logic region i where the logic gate structure 61 is to be formed and the hard mask 51 is etched in the region other than the region where the logic gate structure 61 is to be formed.
[0065] As an example, the hard mask 51 can be etched first to expose the first portion 12 of the polysilicon layer located in the non-logic gate structure 61 formation area; then, under the mask of the etched hard mask, the first portion 12 of the polysilicon layer and the gate oxide layer 11 are etched to form the logic gate structure 61.
[0066] Specifically, a photoresist mask may be formed on the surface of the formation region of the logic gate structure 61 in the logic region i by a photolithography process; then, the hard mask 51 in the formation region other than the logic gate structure 61 may be removed by wet etching such as a hydrofluoric acid solution or dry etching such as plasma etching, such as Figure 2E Therefore, the etched hard mask 51 can provide protection for the formation region of the logic gate structure 61 during the process of forming the logic gate structure 61 to ensure the etching accuracy of the dry etching.
[0067] Optionally, after wet etching the hard mask 51 in the non-logic gate structure 61 formation area, the photoresist may be removed first and then the step of forming the logic gate structure 61 by etching is performed, or the photoresist may be removed after the step of forming the logic gate structure 61 by etching is performed.
[0068] As an example, the non-logic gate structure 61 formation region in the first portion 12 of the polysilicon layer may be dry-etched first to obtain a select transistor 611; and then the non-logic gate structure 61 formation region of the gate oxide layer 11 may be dry-etched to the exposed substrate 10 to form a logic gate structure 61 including the etched gate oxide layer and the select gate 611, as shown in FIG. Figure 2F .
[0069] S106 : removing the hard mask 51 .
[0070] Optionally, the hard mask 51 is removed by wet etching. For example, a hot phosphoric acid solution having a high etching rate for silicon nitride and silicon oxide can be used to etch the silicon nitride as a hard mask to remove the hard mask. Figure 2G .
[0071] S107: forming a lightly doped drain region and a source-drain implantation region by ion implantation to obtain an eflash storage unit.
[0072] Optionally, the substrate provided in the embodiment of the present application is a substrate having a deep N-well DNW. Before step S101, the DNW may be formed by performing N-type ion implantation on a P-type substrate, thereby reducing substrate coupling noise.
[0073] For example, after removing the hard mask 51, a source Drain, a drain Source and a lightly doped drain region LDD may be formed by ion doping. Figure 2H As shown, in the SONOS region ii, an N+ source, an N+ drain and an N-type lightly doped drain region (NLDD) can be formed by performing N-type ion implantation on the substrate 10; or a P+ source, a P+ drain and a P-type lightly doped drain region (PLDD) can be formed by performing P-type ion implantation on the substrate 10. The source and the drain are respectively located on both sides of the contact area between the substrate 10 and the ONO gate structure 31, and are in contact with the side of the oxide layer sidewall 41 close to the substrate 10; the doping depth of the lightly doped drain region is lower than that of the source and the drain, and the two lightly doped drain regions extend to the side of the source close to the contact area between the substrate 10 and the ONO gate structure 31 and the side of the gate close to the contact area between the substrate 10 and the ONO gate structure, and the two lightly doped drain regions are not in contact.
[0074] In an embodiment of the present application, first, a substrate is provided; the substrate includes a logic region and a SONOS region, the substrate of the logic region includes a substrate, a gate oxide layer, and a first part of a polysilicon layer stacked in sequence, and the substrate of the SONOS region includes a substrate, an ONO layer formed by stacking a first oxide layer, a first nitride layer, and a second oxide layer, and a second part of a polysilicon layer stacked in sequence; then, a hard mask is formed; the hard mask exposes the second part of the polysilicon layer located in the formation area of the non-logic gate structure; then, the second part of the polysilicon layer and the ONO layer are etched to form an ONO gate structure; then, an oxide layer sidewall is formed on the first part of the polysilicon layer and the sidewall of the ONO gate structure; then, the first part of the polysilicon layer and the gate oxide layer are etched to form a logic gate structure; finally, the hard mask is removed; and a lightly doped drain region and a source-drain injection region are formed by ion implantation to obtain an eflash storage unit. Thus, after forming the ONO gate structure, the sidewall of the ONO layer is protected by the oxide layer sidewall, which not only ensures the etching accuracy of the logic gate structure of the logic device, but also avoids the ONO layer being lateral etched and causing defects in the subsequent hard mask removal process because the ONO layer and the hard mask have the same composition, thereby reducing the damage to the ONO layer in the manufacturing process of the eflash storage unit and improving the reliability of the eflash storage unit. In addition, the polysilicon layer formed once is etched twice to form the ONO gate structure and the logic gate structure respectively, reducing the number of polysilicon layer growth times, and effectively reducing the manufacturing cost.
[0075] In addition, the present application also provides a storage unit, which is manufactured using the manufacturing method of the eflash storage unit described in the above embodiment, and includes a logic device and a SONOS structure.
[0076] The terms "first", "second", "third" and "fourth" etc. in the specification, claims and drawings of this application are used to distinguish different objects rather than to limit a specific order.
[0077] In the embodiments of the present application, the words "as an example" or "for example" are used to indicate examples, illustrations or explanations. Any embodiment or design described as "as an example" or "for example" in the embodiments of the present application should not be interpreted as being more preferred or more advantageous than other embodiments or designs. Specifically, the use of the words "as an example" or "for example" is intended to present the relevant concepts in a specific way.
[0078] The terms used in the implementation section of this application are only used to explain the specific embodiments of this application and are not intended to limit this application.
[0079] It should be noted that each embodiment in this specification is described in a progressive manner, and the same or similar parts between the embodiments can be referred to each other, and each embodiment focuses on the differences from other embodiments. The method embodiments described above are only illustrative, and some or all of the steps can be selected according to actual needs to achieve the purpose of the embodiment scheme. Ordinary technicians in this field can understand and implement it without paying creative work.
[0080] The above is only a specific implementation of the present application, but the protection scope of the present application is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed in the present application should be included in the protection scope of the present application. Therefore, the protection scope of the present application should be based on the protection scope of the claims.
Claims
1. A method for manufacturing an eflash storage unit, characterized in that: The eflash storage unit includes a logic device and a SONOS structure, and the method includes: Providing a substrate; the substrate comprises a logic region and a SONOS region, the substrate of the logic region comprises a substrate, a gate oxide layer, and a first portion of a polysilicon layer stacked in sequence, and the substrate of the SONOS region comprises a substrate, an ONO layer formed by stacking a first oxide layer, a first nitride layer, and a second oxide layer, and a second portion of a polysilicon layer, stacked in sequence; forming a hard mask; the hard mask exposing a second portion of the polysilicon layer located in a non-ONO gate structure formation region; the hard mask comprising a nitride layer; Etching the second portion of the polysilicon layer and the ONO layer to form an ONO gate structure; Forming an oxide layer sidewall on the first portion of the polysilicon layer and the sidewall of the ONO gate structure; The first portion of the polysilicon layer and the gate oxide layer are etched to form a logic gate structure.
2. The method according to claim 1, characterized in that The step of forming an oxide layer sidewall on the first portion of the polysilicon layer and the sidewall of the ONO gate structure comprises: forming a third oxide layer on the first portion of the polysilicon layer and on the sidewalls of the ONO gate structure; The first portion of the polysilicon layer and the surface of the ONO gate structure facing away from the substrate and the third oxide layer located on the surface of the substrate are removed to form oxide layer sidewalls.
3. The method according to claim 2, characterized in that The third oxide layer is formed by chemical vapor deposition or thermal oxidation.
4. The method according to claim 1, characterized in that: The etching of the second portion of the polysilicon layer and the ONO layer to form an ONO gate structure includes: dry etching the second portion of the polysilicon layer to obtain a control gate; The ONO layer is dry-etched to expose the substrate, forming an ONO gate structure including the etched ONO layer and a control gate.
5. The method according to claim 1, characterized in that The etching of the first portion of the polysilicon layer and the gate oxide layer to form a logic gate structure includes: Etching the hard mask to expose a first portion of the polysilicon layer located in a formation area of a non-logic gate structure; Under the mask of the etched hard mask, the first portion of the polysilicon layer and the gate oxide layer are etched to form a logic gate structure.
6. The method according to claim 1, characterized in that The substrate is prepared by the following process: Providing a substrate; the substrate is a silicon substrate; forming an ONO layer consisting of a first oxide layer, a first nitride layer and a second oxide layer stacked in sequence on the substrate; Etching the ONO layer located in the logic area to expose the substrate; forming a gate oxide layer on the surface of the substrate in the logic region; A polysilicon layer is grown on the side of the gate oxide layer and the ONO layer away from the substrate to obtain a base; the polysilicon layer includes a first portion of the polysilicon layer located in the logic region and a second portion of the polysilicon layer located in the SONOS region.
7. The method according to claim 1, characterized in that After etching the first portion of the polysilicon layer and the gate oxide layer to form a logic gate structure, the method further includes: removing the hard mask; By ion implantation, a lightly doped drain region and a source-drain implantation region are formed.
8. The method according to claim 1, characterized in that In the ONO layer, the thickness of the first oxide layer is in the range of The thickness of the first nitride layer is in the range of The thickness of the second oxide layer is in the range of 9. The method according to claim 1, characterized in that: The removing of the hard mask comprises: The hard mask is removed by wet etching using a phosphoric acid solution.
10. A storage unit, characterized in that: The memory cell is manufactured by applying the method for manufacturing an eflash memory cell according to any one of claims 1 to 9.