Internal connection structure and manufacturing method thereof
By introducing an oxide adhesive layer and an ultra-low k dielectric layer into the inner connection structure, the problem of poor adhesion of the dielectric layer in the prior art is solved, the resistance-capacity retardation and mechanical properties of the semiconductor device are improved, and the membrane separation is avoided The layers and cracks improve product quality.
Patent Information
- Application Number
- CN202310939425.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-05-09
- Filing Date
- 2023-07-28
- Publication Date
- 2024-11-12
AI Technical Summary
The resistance-capacitance delay performance associated with the low-k barrier layer and the dielectric layer of the black diamond in the existing internal connection structure cannot meet the needs of next-generation semiconductor products, and the poor interface adhesion of the ultra-low-k dielectric layer leads to film during packaging. Layering issues.
The oxide glue layer is located between the barrier layer and the ultra-low k dielectric layer. The oxide glue layer provides interface adhesion, and self-assembly and cross-link to form an orderly and uniform pore configuration to reduce the The porosity of the ULK layer is to improve mechanical properties.
It effectively improves the resistance-capacity retardation performance of semiconductor devices, prevents film layering, improves product yield and reliability, and resists film rupture during chemical mechanical grinding.
Smart Images

Figure CN118943117A_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to an internal connection structure and a method for manufacturing the internal connection structure. Background Art
[0002] The manufacturing process of semiconductor integrated circuit (IC) includes front-end-of-line (FEOL), middle-end-of-line (MEOL) and back-end-of-line (BEOL). The front-end process includes wafer preparation, isolation, well formation, gate patterning, spacer, extension and source / drain implantation, silicide formation and dual stress pad formation. The middle process includes gate contact formation. The back-end process includes a series of wafer processing steps to interconnect the semiconductor components produced during the front-end process and the middle-end process. In addition, the successful manufacture of qualified semiconductor wafer products requires consideration of the interaction between materials and processes.
[0003] As the size of semiconductor devices decreases, the resistive-capacitive (RC) delay performance associated with the dielectric layer in the existing interconnect structure including the stack of low-k barrier layer and black diamond cannot meet the requirements of the next generation products. Although the ultra low-k (ULK) layer with high porosity and low-k dielectric constant can be used in the interconnect structure to improve the RC delay performance, the interface adhesion of the ULK layer is worse, which will lead to film delamination during packaging. In addition, even if a porogen is not added in the initial step of forming the ULK layer to reduce the porosity of the ULK layer, the interconnect structure still shows delamination due to the poor adhesion of the general precursor of the ULK layer. Summary of the invention
[0004] One aspect of the present disclosure provides an internal connection structure.
[0005] According to some embodiments of the present disclosure, an interconnect structure includes a barrier layer, an oxide glue layer, and an ultra-low-k dielectric layer. The oxide glue layer is located on the barrier layer. The ultra-low-k dielectric layer is located on the oxide glue layer, wherein the oxide glue layer is located between the barrier layer and the ultra-low-k dielectric layer, and the ultra-low-k dielectric layer has a porosity of less than 40%.
[0006] In some embodiments, the oxide glue layer contacts a top surface of the barrier layer and a bottom surface of the ultra low k dielectric layer.
[0007] In some embodiments, the porosity of the oxide glue layer is greater than 10%.
[0008] In some embodiments, the oxide glue layer is formed from a precursor including tetraethylorthosilicate (TEOS).
[0009] In some embodiments, the ultra low-k dielectric layer is formed from a precursor other than TEOS.
[0010] In some embodiments, the ultra low-k dielectric layer includes a plurality of pores arranged in an ordered and uniform distribution.
[0011] In some embodiments, the material of the oxide glue layer and the material of the ultra-low-k dielectric layer include silicon oxide.
[0012] In some embodiments, the ultra low k dielectric layer has a dielectric constant that is less than the dielectric constant of the barrier layer.
[0013] In some embodiments, the ultra low-k dielectric layer has a dielectric constant less than 2.5.
[0014] In some embodiments, the dielectric constant of the barrier layer is less than 4.0.
[0015] In some embodiments, the material of the barrier layer includes amorphous silicon carbide (a-SiC).
[0016] In some embodiments, the interconnect structure further includes a metal layer in contact with a top surface of the ultra low-k dielectric layer.
[0017] In some embodiments, the interconnect structure further includes another barrier layer in contact with the top surface of the ultra low-k dielectric layer.
[0018] In some embodiments, the interconnect structure further comprises a metal layer, wherein the barrier layer is located on the metal layer.
[0019] In some embodiments, the interconnect structure further includes a capping layer on the ultra low-k dielectric layer.
[0020] Another aspect of the present disclosure provides a method for manufacturing an inner connection structure.
[0021] According to some embodiments of the present disclosure, a method for manufacturing an internal connection structure includes: forming a barrier layer on a metal layer; forming an oxide glue layer on the barrier layer; and forming an ultra-low-k dielectric layer on the oxide glue layer, so that the oxide glue layer is located between the barrier layer and the ultra-low-k dielectric layer, wherein the ultra-low-k dielectric layer has a porosity of less than 40%.
[0022] In some embodiments, forming an oxide primer layer on the barrier layer includes using tetraethylorthosilicate (TEOS) as a precursor to form the oxide primer layer.
[0023] In some embodiments, the oxide glue layer and the ultra low-k dielectric layer are formed from a first precursor and a second precursor different from the first precursor, respectively.
[0024] In some embodiments, forming an ultra-low-k dielectric layer on the oxide glue layer includes: depositing a dielectric material having a porogen on the oxide glue layer; and curing the dielectric material using UV light to remove the porogen.
[0025] In some embodiments, the method for fabricating the interconnect structure further comprises: planarizing the ultra-low-k dielectric layer using chemical mechanical polishing; and forming at least one of a metal layer and another barrier layer on the planarized ultra-low-k dielectric layer.
[0026] In the above-described embodiments of the present disclosure, since the interconnect structure has an oxide glue layer between the barrier layer and the ultra low-k (ULK) dielectric layer, the oxide glue layer can provide interfacial adhesion to the underlying barrier layer and the overlying ultra low-k dielectric layer. Therefore, film delamination between the ultra low-k dielectric layer and the barrier layer does not occur during packaging, and cracking does not occur during chemical-mechanical polishing (CMP) performed on the interconnect structure. In addition, the ultra low-k dielectric layer can have a high porosity and a low-k dielectric constant to improve the resistive-capacitive (RC) delay performance of the semiconductor device including the interconnect structure. In addition, due to the self-assembly and cross-linking of the porogen, the ultra low-k dielectric layer has an ordered pore configuration and a uniform pore distribution, and thus the ultra low-k dielectric layer can have good mechanical properties even with its high porosity. Therefore, a cap layer on the ultra low-k dielectric layer can be omitted because the ultra low-k dielectric layer can release the stress caused by CMP to resist film cracking. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] The aspects of the present disclosure are best understood from the following detailed description when read in conjunction with the accompanying drawings. It should be noted that, in accordance with standard practice in the industry, various features are not drawn to scale. In practice, the sizes of various features may be arbitrarily increased or reduced for clarity of discussion.
[0028] Figure 1 FIG. 4 is a cross-sectional view of an inner connection structure according to an embodiment of the present disclosure.
[0029] Figure 2 FIG. 4 is a cross-sectional view of an inner connection structure according to another embodiment of the present disclosure.
[0030] Figure 3 FIG. 1 is a comparison diagram of film quality between an ultra-low-k dielectric layer according to an embodiment of the present disclosure and conventional black diamond.
[0031] Figure 4 FIG. 4 is a cross-sectional view of an inner connection structure according to another embodiment of the present disclosure.
[0032] Figure 5FIG. 4 is a cross-sectional view of an inner connection structure according to another embodiment of the present disclosure.
[0033] Figure 6 FIG. 4 is a cross-sectional view of an inner connection structure according to an embodiment of the present disclosure.
[0034] Figure 7 The figure is a flow chart of a method for manufacturing an inner connection structure according to an embodiment of the present disclosure. DETAILED DESCRIPTION
[0035] The following disclosure provides many different embodiments or examples for implementing the different features of the provided subject matter. The specific examples of components and configurations are described below to simplify the disclosure. Of course, these specific embodiments or examples are only examples and are not intended to be limiting. In addition, the disclosure may repeat reference numerals and / or letters in various examples. This repetition is for the purpose of simplicity and clarity, and does not itself indicate the relationship between the various embodiments and / or configurations discussed.
[0036] Additionally, for ease of description, spatially relative terms (such as "below," "beneath," "bottom," "above," "upper," and the like) may be used herein to describe the relationship of one component or feature to another component or feature as illustrated in the accompanying figures. The spatially relative terms are intended to encompass different orientations of the device in use or operation in addition to the orientation depicted in the figures. The device may be otherwise oriented (rotated 90 degrees or at other orientations) and the spatially relative descriptors used herein interpreted accordingly.
[0037] Figure 1 FIG. 1 is a cross-sectional view of an internal connection structure 100 according to an embodiment of the present disclosure. Figure 1 As shown, the interconnect structure 100 includes a barrier layer 110, an oxide glue layer 120, and an ultra low-k (ULK) dielectric layer 130. In this embodiment, the interconnect structure 100 further includes a capping layer 140 located on the ultra low-k dielectric layer 130. The oxide glue layer 120 is located on the barrier layer 110. The ultra low-k dielectric layer 130 is located on the oxide glue layer 120. In other words, the oxide glue layer 120 is located between the barrier layer 110 and the ultra low-k dielectric layer 130. The oxide glue layer 120 is configured to provide interfacial adhesion (e.g., adhesion force F1 and adhesion force F2) to the barrier layer 110 and the ultra low-k dielectric layer 130, thereby preventing the barrier layer 110 and the ultra low-k dielectric layer 130 from being delaminated. In more detail, the oxide glue layer 120 contacts the top surface 111 of the barrier layer 110 and the bottom surface 133 of the ultra low-k dielectric layer 130.
[0038] The interconnect structure 100 can be applied to a semiconductor device, such as a memory device having a logic region, but the present disclosure is not limited thereto. The interconnect structure 100 can be located between two metal layers (eg, copper layers), two dielectric layers, or a metal layer and a dielectric layer, depending on the design requirements of the semiconductor device.
[0039] In some embodiments, the ultra low k dielectric layer 130 has a porosity of less than 40% and at least greater than 10%. The ultra low k dielectric layer 130 includes a plurality of pores 132 that are arranged in an ordered manner and in a uniform distribution due to self-assembly and cross-linking of the porogen. The ultra low k dielectric layer 130 has a dielectric constant that is less than the dielectric constant of the barrier layer 110. For example, the dielectric constant of the ultra low k dielectric layer 130 is less than 2.5, and the dielectric constant of the barrier layer 110 is less than 4.0.
[0040] In some embodiments, the oxide glue layer 120 is formed of a precursor including tetraethyl orthosilicate (TEOS), and thus the oxide glue layer 120 can enhance the interfacial adhesion to the barrier layer 110 and the ultra-low-k dielectric layer 130. The ultra-low-k dielectric layer 130 can be formed of a precursor other than TEOS, such as silane (SiH 4 ) or silicon tetrachloride (SiCl 4 In addition, the material of the oxide glue layer 120, the material of the ultra-low-k dielectric layer 130, and the material of the cap layer 140 include oxides, such as silicon oxide (SiO 2 In addition, the material of the barrier layer 110 may include amorphous silicon carbide (a-SiC).
[0041] Specifically, since the interconnect structure 100 has the oxide glue layer 120 between the barrier layer 110 and the ultra low-k (ULK) dielectric layer 130, the oxide glue layer 120 can provide interface adhesion to the underlying barrier layer 110 and the overlying ultra low-k dielectric layer 130. Therefore, film delamination between the ultra low-k dielectric layer 130 and the barrier layer 110 does not occur during packaging, and does not crack during a chemical-mechanical polish (CMP) process performed on a semiconductor device having the interconnect structure 100. Therefore, the interconnect structure 100 having the oxide glue layer 120 can improve product yield and reliability. In addition, the ultra low-k dielectric layer 130 can have a high porosity and a low k dielectric constant to improve the resistive-capacitive (RC) delay performance of the semiconductor device including the interconnect structure 100.
[0042] It should be noted that the connection relationship, materials and advantages of the above components will not be repeated in the following description. In the following description, other types of internal connection structures will be explained.
[0043] Figure 2 FIG. 1 is a cross-sectional view of an interconnect structure 100a according to another embodiment of the present disclosure. The interconnect structure 100a includes a barrier layer 110, an oxide glue layer 120, and an ultra low-k (ULK) dielectric layer 130. Figure 1 The difference between the embodiments is that Figure 2 The interconnect structure 100a has no capping layer 140 on the ultra-low-k dielectric layer 130 (see Figure 1 In other words, the top surface 131 of the ultra low-k dielectric layer 130 is not covered by the capping layer 140 .
[0044] Due to the self-assembly and cross-linking of the porogen, the ultra-low-k dielectric layer 130 has an ordered pore configuration and a uniform pore distribution, and thus the ultra-low-k dielectric layer 130 can have good mechanical properties even with its high porosity. Figure 1 ) can be omitted because the ultra low-k dielectric layer 130 can release the stress caused by CMP to resist film cracking.
[0045] Figure 3 FIG. 1 is a comparison diagram of film quality between an ultra low-k (ULK) dielectric layer 130 according to an embodiment of the present disclosure and a conventional black diamond (BD). Figure 1 and Figure 2 The ultra-low-k dielectric layer 130 shown can replace black diamond in the technical field of the interconnect structure. The dielectric constant of the ultra-low-k dielectric layer 130 is less than 2.5, while the dielectric constant of black diamond is less than 3.0. The dielectric constant of the ultra-low-k dielectric layer 130 can be less than the dielectric constant of black diamond. The porosity of the ultra-low-k dielectric layer 130 is less than 40%, while the porosity of black diamond is less than 10%. The porosity of the ultra-low-k dielectric layer 130 can be greater than the porosity of black diamond. The pore configuration of the ultra-low-k dielectric layer 130 is ordered, while the pore configuration of black diamond is disordered. The pore distribution of the ultra-low-k dielectric layer 130 is uniform, while the pore distribution of black diamond is non-uniform. In addition, the ultra-low-k dielectric layer 130 can release stress caused by CMP, while black diamond enhances stress caused by CMP.
[0046] Figure 4 FIG. 1 is a cross-sectional view of an interconnect structure 100b according to another embodiment of the present disclosure. The interconnect structure 100b includes a barrier layer 110, an oxide glue layer 120, and an ultra low-k (ULK) dielectric layer 130. Figure 2The difference between the embodiments of the present invention is that the interconnect structure 100b further includes two metal layers 150a and 150b. Each of the two metal layers 150a and 150b can be a copper layer for transmitting electrical signals. The barrier layer 110 is located on the metal layer 150a. That is, the metal layer 150a is located below the barrier layer 110. In some embodiments, the metal layer 150b contacts the top surface 131 of the ultra low k dielectric layer 130.
[0047] Figure 5 FIG. 1 is a cross-sectional view of an interconnect structure 100c according to another embodiment of the present disclosure. The interconnect structure 100c includes a barrier layer 110, an oxide glue layer 120, and an ultra low-k (ULK) dielectric layer 130. Figure 4 The difference between the embodiments of the present invention is that the interconnect structure 100c further includes another barrier layer 110a, another oxide glue layer 120a and another ultra low k dielectric layer 130a sequentially stacked on the ultra low k dielectric layer 130. In some embodiments, the barrier layer 110a contacts the top surface 131 of the ultra low k dielectric layer 130.
[0048] Figure 6 FIG. 1 is a cross-sectional view of an interconnect structure 100d according to an embodiment of the present disclosure. The interconnect structure 100d includes a barrier layer 110, an oxide glue layer 120, and an ultra low-k (ULK) dielectric layer 130. Figure 4 and Figure 5 The difference between each of the embodiments is that the interconnect structure 100d includes a barrier layer 110a, an oxide glue layer 120a, an ultra-low-k dielectric layer 130a, and a metal layer 150b. The metal layer 150b and the barrier layer 110a are in contact with the top surface 131 of the ultra-low-k dielectric layer 130. In addition, the sidewall of the metal layer 150b is in contact with the barrier layer 110a, the oxide glue layer 120a, and the ultra-low-k dielectric layer 130a.
[0049] Figure 7The present invention is a flow chart of a method for manufacturing an internal connection structure according to an embodiment of the present disclosure. The method for manufacturing an internal connection structure includes the following steps. In step S1, a barrier layer is formed on the metal layer. Thereafter, in step S2, an oxide glue layer is formed on the barrier layer. Thereafter, in step S3, an ultra-low-k dielectric layer is formed on the oxide glue layer so that the oxide glue layer is located between the barrier layer and the ultra-low-k dielectric layer. Next, in step S4, the ultra-low-k dielectric layer is planarized using chemical-mechanical polish (CMP). Subsequently, in step S5, at least one of a metal layer and another barrier layer is formed on the planarized ultra-low-k dielectric layer. The method for manufacturing an internal connection structure is not limited to the above steps S1 to S5. For example, in some embodiments, the manufacturing method may further include other steps between two of the above steps, and may further include other steps before step S1 and after step S5.
[0050] In the following description, the above-mentioned steps of the method for manufacturing the inner connection structure will be explained in detail.
[0051] like Figure 6 As shown, a barrier layer 110 is formed on the metal layer 150a. Then, an oxide glue layer 120 is formed on the barrier layer 110. The formation of the oxide glue layer 120 includes using tetraethyl orthosilicate (TEOS) as a precursor to form the oxide glue layer 120. After the oxide glue layer 120 is formed, an ultra-low-k dielectric layer 130 is formed on the oxide glue layer 120, so that the oxide glue layer 120 is located between the barrier layer 110 and the ultra-low-k dielectric layer 130. The ultra-low-k dielectric layer 130 has a porosity of less than 40%. In addition, the oxide glue layer 120 and the ultra-low-k dielectric layer 130 are respectively made of a first precursor (e.g., TEOS) and a second precursor different from the first precursor (e.g., SiCl 4 ). Forming the ultra low k dielectric layer 130 on the oxide glue layer 120 may include depositing a dielectric material with a porogen on the oxide glue layer 120, and then curing the dielectric material to remove the porogen using UV light. Afterwards, chemical-mechanical polishing (CMP) may be used to planarize the ultra low k dielectric layer 130, and at least one of the metal layer 150b and the barrier layer 110a may be formed on the planarized ultra low k dielectric layer 130.
[0052] Through some or all of the above steps, the Figure 1 , Figure 2 , Figure 4 , Figure 5 and Figure 6 The inner connection structures 100, 100a, 100b, 100c and 100d are shown.
[0053] The foregoing summarizes the features of several embodiments so that those skilled in the art can better understand the aspects of the present disclosure. Those skilled in the art should understand that they can easily use the present disclosure as a basis for designing or modifying other processes and structures to achieve the same purposes and / or achieve the same advantages of the embodiments introduced herein. Those skilled in the art should also recognize that such equivalent constructions do not depart from the spirit and scope of the present disclosure, and those skilled in the art can make various changes, substitutions and modifications without departing from the spirit and scope of the present disclosure.
[0054]
Explanation of symbols
[0055] 100,100a,100b,100c,100d: internal connection structure
[0056] 110,110a: Barrier layer
[0057] 111,131: Top surface
[0058] 120,120a: Oxide glue layer
[0059] 130,130a: Ultra-low-k dielectric layer
[0060] 132: Hole
[0061] 133: Bottom surface
[0062] 140: Covering layer
[0063] 150a, 150b: metal layer
[0064] F1, F2: Adhesion
[0065] S1,S2,S3,S4,S5: steps.
Claims
1. An internal connection structure, It is characterized in that include: Barrier layer; an oxide glue layer, located on the barrier layer; and The ultra low k dielectric layer is located on the oxide glue layer, wherein the oxide glue layer is located between the barrier layer and the ultra low k dielectric layer, and the ultra low k dielectric layer has a porosity less than 40%.
2. The inner connection structure according to claim 1, It is characterized in that The oxide glue layer contacts the top surface of the barrier layer and the bottom surface of the ultra low k dielectric layer.
3. The inner connection structure according to claim 1, It is characterized in that The porosity of the oxide glue layer is greater than 10%.
4. The inner connection structure according to claim 1, It is characterized in that The oxide glue layer is formed from a precursor including tetraethylorthosilicate.
5. The inner connection structure according to claim 1, It is characterized in that The ultra low k dielectric layer is formed from a precursor other than tetraethyl orthosilicate.
6. The inner connection structure according to claim 1, It is characterized in that The ultra low k dielectric layer includes a plurality of pores arranged in an orderly manner and in a uniform distribution.
7. The inner connection structure according to claim 1, It is characterized in that The material of the oxide glue layer and the material of the ultra-low-k dielectric layer include silicon oxide.
8. The inner connection structure according to claim 1, It is characterized in that The ultra low-k dielectric layer has a dielectric constant that is less than a dielectric constant of the barrier layer.
9. The inner connection structure according to claim 8, It is characterized in that The dielectric constant of the ultra low-k dielectric layer is less than 2.
5. 10 . The interconnect structure as claimed in claim 8 , wherein the dielectric constant of the barrier layer is less than 4.
0.
11. The inner connection structure according to claim 1, It is characterized in that The material of the barrier layer includes amorphous silicon carbide.
12. The inner connection structure according to claim 1, It is characterized in that Further including: A metal layer contacts a top surface of the ultra low-k dielectric layer.
13. The inner connection structure according to claim 1, It is characterized in that Further including: Another barrier layer contacts the top surface of the ultra low k dielectric layer.
14. The inner connection structure according to claim 1, It is characterized in that Further including: A metal layer, wherein the barrier layer is located on the metal layer.
15. The inner connection structure according to claim 1, It is characterized in that Further including: A capping layer is located on the ultra low-k dielectric layer.
16. A method for manufacturing an inner connection structure, It is characterized in that The following steps are involved: forming a barrier layer on the metal layer; forming an oxide glue layer on the barrier layer; and An ultra low k dielectric layer is formed on the oxide glue layer so that the oxide glue layer is located between the barrier layer and the ultra low k dielectric layer, wherein the ultra low k dielectric layer has a porosity less than 40%.
17. The method for manufacturing the inner connection structure according to claim 16, It is characterized in that The step of forming the oxide glue layer on the barrier layer comprises: Tetraethyl orthosilicate is used as a precursor to form the oxide glue layer.
18. The method for manufacturing the inner connection structure according to claim 16, It is characterized in that The oxide glue layer and the ultra low k dielectric layer are respectively formed from a first precursor and a second precursor different from the first precursor.
19. The method for manufacturing the inner connection structure according to claim 16, It is characterized in that The step of forming the ultra low k dielectric layer on the oxide glue layer comprises: depositing a dielectric material having a porogen on the oxide glue layer; and The dielectric material is cured by ultraviolet light to remove the porogen.
20. The method for manufacturing the inner connection structure according to claim 16, It is characterized in that Further including: planarizing the ultra-low-k dielectric layer using chemical mechanical polishing; and At least one of the metal layer and another barrier layer is formed on the planarized ultra low k dielectric layer.