Silicon carbide MOSFET power device terminal structure
By setting the slope field limit ring area in the terminal structure of the silicon carbide MOSFET power device, the problem of low breakdown voltage of traditional devices is solved, a more uniform electric field distribution and higher breakdown voltage are achieved, and the reliability of the device is improved .
Patent Information
- Application Number
- CN202411433347.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-15
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-10-15
AI Technical Summary
The breakdown voltage of traditional silicon carbide MOSFET power devices is lower than expected, mainly due to the concentrated electric field effect of the PN junction edge in the active region, which leads to early breakdown of the device.
In the terminal structure of the silicon carbide MOSFET power device, the N-type silicon carbide epitaxial layer in the field limit ring region is set as a slope structure, and the inclination angle between the slope structure and the horizontal plane is 2° to 6°, and several field limits are formed by ion implantation. The ring extends the depletion zone, uniform electric field distribution, and reduces the phenomenon of electric field concentration.
Through the design of the bevel structure, the depletion area of the field-limited loop region is extended, the breakdown voltage is increased, the breakdown voltage reduction amplitude caused by the increase in the fixed charge density of the interface is reduced, and the reliability of the device is improved.
Smart Images

Figure CN118943165A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of silicon carbide MOSFET power devices, and in particular relates to a terminal structure of a silicon carbide MOSFET power device. Background Art
[0002] Silicon carbide is a new generation of wide bandgap semiconductor material. Silicon carbide MOSFET power devices have no minority carrier storage effect, fast device switching speed, and low switching loss, and are widely used in the field of power electronics.
[0003] A traditional silicon carbide MOSFET power device includes an N-type silicon carbide substrate, a drain metal is formed on the bottom surface of the N-type silicon carbide substrate, an N-type silicon carbide epitaxial layer is grown on the surface of the N-type silicon carbide substrate, a P-type well region is formed on the surface of the N-type silicon carbide epitaxial layer, an N+ region and a first P+ region are formed inside the P-type well region, the N+ region and the first P+ region are adjacent to each other, and the above structure constitutes a PN junction of an active region, which belongs to a cell region of the silicon carbide MOSFET power device. Since the edge of the PN junction in the active region often has curvature, the electric field is concentrated in the region with higher curvature, resulting in a breakdown voltage of the silicon carbide MOSFET power device being lower than expected.
[0004] In order to alleviate the electric field concentration effect at the junction edge and avoid premature breakdown, when designing silicon carbide MOSFET power devices, a terminal protection structure must be designed. This type of technology is usually called junction terminal technology. The main terminal structures of traditional silicon carbide MOSFET power devices are field plates, junction terminal extensions and field limiting rings, and these three structures are often used in combination in silicon carbide MOSFET power devices. Specifically, the terminal structure of the traditional silicon carbide MOSFET power device includes: a junction terminal extension is formed on the surface of the N-type silicon carbide epitaxial layer, a second P+ region is also formed on the junction terminal extension, the junction terminal extension is located outside the P-type well region, and a number of field limiting rings are formed on the surface of the N-type silicon carbide epitaxial layer. The field limiting rings are located outside the junction terminal extension. The area where the junction terminal extension is located is the junction terminal extension area of the terminal structure, and the area where the field limiting ring is located is the field limiting ring area of the terminal structure. A gate oxide layer is formed on the surface of the N-type silicon carbide epitaxial layer at the junction of the cell area and the junction terminal extension area. One side of the gate oxide layer is in contact with the P-type well region, and the other side is in contact with the junction terminal extension. A polysilicon gate is deposited on the gate oxide layer. A silicon dioxide oxide layer is grown on the surface of the polysilicon gate, the surface of the N-type silicon carbide epitaxial layer containing the junction terminal extension, and the surface of the N-type silicon carbide epitaxial layer containing the field limiting ring. A source metal is deposited on the silicon dioxide oxide layer. A portion of the source metal is located in the cell region, and another portion is located in the junction terminal extension region. The source metal is located on one side of the cell region and contacts the N+ region and the first P+ region. The source metal is located on one side of the junction terminal extension region and contacts the second P+ region. The portion of the source metal located in the junction terminal extension region acts as a field plate.
[0005] In the above terminal structure, when the interface fixed charge density between the N-type silicon carbide epitaxial layer and the silicon dioxide oxide layer above it increases, the depletion region of the field limiting ring region will be significantly shortened, so that the breakdown voltage of the device is greatly reduced. Summary of the invention
[0006] In order to solve the above technical problems, the present invention provides a silicon carbide MOSFET power device terminal structure. Compared with the traditional silicon carbide MOSFET power device terminal structure, the N-type silicon carbide epitaxial layer in the field limiting ring area is a slope structure, and the inclination angle of the slope structure to the horizontal plane is 2° to 6°. Several field limiting rings are formed on the slope structure by ion implantation.
[0007] The present invention is specifically implemented through the following scheme.
[0008] A terminal structure of a silicon carbide MOSFET power device, comprising a junction terminal extension region and a field limiting ring region, wherein the junction terminal extension region is located outside a cell region of the silicon carbide MOSFET power device, and the field limiting ring region is located outside the junction terminal extension region, wherein the field limiting ring region contains a part of an N-type silicon carbide epitaxial layer, wherein the surface of the N-type silicon carbide epitaxial layer located in the field limiting ring region is a slope structure, wherein the inclination angle of the slope structure to the horizontal plane is 2° to 6°, and a plurality of field limiting rings are formed on the surface of the slope structure by ion implantation.
[0009] Compared with the terminal structure of the traditional silicon carbide MOSFET power device, the present invention sets the N-type silicon carbide epitaxial layer in the field limiting ring area as a bevel structure, which can make the depletion region of the cell area, the depletion region of the junction terminal extension area and the depletion region of the field limiting ring area better extend to the field limiting ring at the rear end, extend the depletion region of the field limiting ring area, make the electric field distribution of the cell area, the junction terminal extension area and the field limiting ring area more uniform, reduce the curvature of the depletion region of the cell area, the junction terminal extension area and the field limiting ring area, and alleviate the phenomenon of electric field concentration.
[0010] In a preferred embodiment of the present invention, before the bevel structure is formed, the thickness of the N-type silicon carbide epitaxial layer in the junction terminal extension region and the field limiting ring region is 10 μm, and the doping concentration is 1×10 16 cm −3 .
[0011] In a preferred embodiment of the present invention, the bevel structure is made by a dry etching process or a V-cutting process. In the bevel structure, the etching depth at one end away from the junction terminal extension area is 3.5μm to 10μm. It should be noted that the etching depth here corresponds to different inclination angles. The larger the inclination angle, the greater the etching depth at one end of the bevel structure away from the junction terminal extension area. For example, when the inclination angle is 2°, the etching depth at one end of the bevel structure away from the junction terminal extension area is 3.5μm, when the inclination angle is 4°, the etching depth at one end of the bevel structure away from the junction terminal extension area is 7μm, and when the inclination angle is 6°, the etching depth at one end of the bevel structure away from the junction terminal extension area is 10μm.
[0012] In a preferred embodiment of the present invention, the number of field limiting rings is 15 to 25, the width of each field limiting ring is 2 μm to 3 μm, and the distance between two adjacent field limiting rings is 0.5 μm to 2.5 μm. Preferably, the number of field limiting rings is 20, the width of each field limiting ring is 2.5 μm, and the distance between two adjacent field limiting rings is 1 μm.
[0013] In a preferred embodiment of the present invention, the junction terminal extension region contains a portion of the N-type silicon carbide epitaxial layer, a junction terminal extension is formed on the surface of the N-type silicon carbide epitaxial layer in the junction terminal extension region, and the junction terminal extension and a plurality of field limiting rings are simultaneously formed by 2 to 3 ion implantations, and each time the ion implantation is performed, the junction terminal extension and the plurality of field limiting rings are simultaneously ion implanted, the implantation element is aluminum, the energy of each implantation is 100 keV to 800 keV, and the dose of each implantation is 2×10 13 cm −2 .
[0014] In a preferred embodiment of the present invention, the length of the junction terminal extension is 10 μm to 30 μm, preferably 20 μm.
[0015] In a preferred embodiment of the present invention, a second P+ region is formed on the junction terminal extension surface, and the second P+ region and the first P+ region located in the cell region are formed simultaneously by 3 to 4 ion implantations. During each ion implantation, the second P+ region and the first P+ region are simultaneously ion implanted. The implanted element is aluminum, the energy of each implantation is 100 keV to 200 keV, and the dose of each implantation is 1×10 14 cm −2 ~3×10 14 cm −2 .
[0016] In a preferred embodiment of the present invention, a gate oxide layer is formed on the surface of the N-type silicon carbide epitaxial layer at the junction of the cell region and the junction terminal extension region, one side of the gate oxide layer is in contact with the P-type well region in the cell region, and the other side is in contact with the junction terminal extension, and a polysilicon gate is deposited on the gate oxide layer.
[0017] In a preferred embodiment of the present invention, a silicon dioxide oxide layer is grown on the surface of the polysilicon gate, the surface of the N-type silicon carbide epitaxial layer containing the junction terminal extension, and the surface of the N-type silicon carbide epitaxial layer containing the field limiting ring, and a source metal is deposited on the silicon dioxide oxide layer, a part of the source metal is in contact with the N+ region and the first P+ region in the cell region, and another part is located in the junction terminal extension region and in contact with the second P+ region. The part of the source metal located in the junction terminal extension region acts as a field plate.
[0018] Compared with the prior art, the present invention has the following beneficial effects: The present invention provides a terminal structure of a silicon carbide MOSFET power device, in which an N-type silicon carbide epitaxial layer in a field limiting ring region is a bevel structure, the inclination angle of the bevel structure to the horizontal plane is 2° to 6°, and a plurality of field limiting rings are formed on the bevel structure. The bevel structure can make the depletion region of the cell region, the depletion region of the junction terminal extension region and the depletion region of the field limiting ring region better extend to the field limiting ring at the rear end, extend the depletion region of the field limiting ring region, make the electric field distribution of the cell region, the junction terminal extension region and the field limiting ring region more uniform, reduce the curvature of the depletion region of the cell region, the junction terminal extension region and the field limiting ring region, alleviate the phenomenon of electric field concentration, improve the breakdown voltage of the silicon carbide MOSFET power device, reduce the amplitude of the breakdown voltage reduction caused by the increase of the fixed charge density at the interface, and further improve the reliability of the device. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 Schematic diagram of the structure of a silicon carbide MOSFET power device with a traditional terminal structure.
[0020] Figure 2 It is a schematic diagram of the structure of a silicon carbide MOSFET power device containing the terminal structure of the present invention.
[0021] Figure 3 The figure is a comparison graph of breakdown voltage of silicon carbide MOSFET power devices with different tilt angles.
[0022] Figure 4 This is a graph showing the breakdown voltage of a silicon carbide MOSFET power device with a tilt angle of 6° and a traditional silicon carbide MOSFET power device as a function of the interface fixed charge density.
[0023] Description of reference numerals: 1. Drain metal, 2. N-type silicon carbide substrate, 3. N-type silicon carbide epitaxial layer, 4. Silicon dioxide oxide layer, 5. Source metal, 6. Polysilicon gate, 7. N+ region, 8. First P+ region, 9. P-type well region, 10. Junction terminal extension, 11. Field limiting ring, 12. Second P+ region, C1, cell region, C2, junction terminal extension region, C3, field limiting ring region. DETAILED DESCRIPTION
[0024] In order to enable those skilled in the art to better understand and implement the technical solution of the present invention, the present invention is further described below in conjunction with specific embodiments and drawings, but the embodiments are not intended to limit the present invention.
[0025] Traditional silicon carbide MOSFET power device terminal structure, such as Figure 1 As shown, it includes a junction terminal extension region C2 and a field limiting ring region C3, wherein the junction terminal extension region C2 is located outside the cell region C1 of the silicon carbide MOSFET power device, and the field limiting ring region C3 is located outside the junction terminal extension region C2, and the portion of the source metal 5 located in the junction terminal extension region C2 acts as a field plate, wherein the field limiting ring region C3 contains a portion of the N-type silicon carbide epitaxial layer 3, and the N-type silicon carbide epitaxial layer 3 located in the field limiting ring region C3 is a planar structure.
[0026] The present invention provides a silicon carbide MOSFET power device terminal structure, such as Figure 2 As shown, the terminal structure includes a junction terminal extension region C2 and a field limiting ring region C3. The junction terminal extension region C2 is located outside the cell region C1 of the silicon carbide MOSFET power device, and the field limiting ring region C3 is located outside the junction terminal extension region C2. The field limiting ring region C3 contains a portion of the N-type silicon carbide epitaxial layer 3. The surface of the N-type silicon carbide epitaxial layer 3 located in the field limiting ring region C3 is a bevel structure, and the inclination angle of the bevel structure to the horizontal plane is 2° to 6°. A plurality of field limiting rings 11 are formed on the surface of the bevel structure by ion implantation.
[0027] and Figure 1 Compared with the traditional terminal structure, the present invention improves the field limiting ring area C3. The N-type silicon carbide epitaxial layer 3 in the field limiting ring area C3 is a bevel structure, which can make the depletion region of the cell area C1, the depletion region of the junction terminal extension region C2 and the depletion region of the field limiting ring area C3 better extend to the field limiting ring 11 at the rear end, making the electric field intensity distribution more uniform and alleviating the phenomenon of electric field concentration.
[0028] The slope structure of the present invention is made by dry etching process or V-cutting process. In the slope structure, the etching depth of the end away from the junction terminal extension area C2 is 3.5μm to 10μm. The number of field limiting rings 11 is 15 to 25, the ring width of each field limiting ring 11 is 2μm to 3μm, and the ring spacing between two adjacent field limiting rings 11 is 0.5μm to 2.5μm.
[0029] The junction terminal extension region C2 of the present invention is configured as follows: a junction terminal extension 10 is formed on the surface of the N-type silicon carbide epitaxial layer 3 in the junction terminal extension region C2, and the junction terminal extension 10 and a plurality of field limiting rings 11 are simultaneously formed by 2 to 3 ion implantations. During each ion implantation, the junction terminal extension 10 and the plurality of field limiting rings 11 are simultaneously ion implanted, the implanted element is aluminum, the energy of each implantation is 100 keV to 800 keV, and the dose of each implantation is 2×10 13 cm −2 The length of the junction terminal extension 10 is 10 μm to 30 μm. A second P+ region 12 is formed on the surface of the junction terminal extension 10. The second P+ region 12 and the first P+ region 8 located in the cell region C1 are formed simultaneously by 3 to 4 ion implantations. During each ion implantation, the second P+ region 12 and the first P+ region 8 are simultaneously ion implanted. The implanted element is aluminum. The energy of each implantation is 100 keV to 200 keV. The dose of each implantation is 1×10 14 cm −2 ~3×10 14 cm −2 .
[0030] The terminal structure of the silicon carbide MOSFET power device provided by the present invention also includes a field plate structure, specifically, the part of the source metal 5 located in the junction terminal extension region C2 acts as a field plate. A gate oxide layer is formed on the surface of the N-type silicon carbide epitaxial layer 3 at the junction of the cell region C1 and the junction terminal extension region C2, one side of the gate oxide layer is in contact with the P-type well region 9 in the cell region C1, and the other side is in contact with the junction terminal extension 10, and a polysilicon gate 6 is deposited on the gate oxide layer. A silicon dioxide oxide layer 4 is grown on the surface of the polysilicon gate 6, the surface of the N-type silicon carbide epitaxial layer 3 containing the junction terminal extension 10, and the surface of the N-type silicon carbide epitaxial layer 3 containing the field limiting ring 11, and a source metal 5 is deposited on the silicon dioxide oxide layer 4, a part of the source metal 5 is in contact with the N+ region 7 and the first P+ region 8 in the cell region C1, and the other part is located in the junction terminal extension region C2 and in contact with the second P+ region 12.
[0031] The present invention is specifically described below through the following embodiments and comparative examples. In the following embodiments and comparative examples, the N-type silicon carbide substrate is specifically a 4H-silicon carbide substrate, and the N-type silicon carbide epitaxial layer is specifically a 4H-silicon carbide epitaxial layer.
[0032] Example 1 Embodiment 1 provides a terminal structure of a silicon carbide MOSFET power device, the terminal structure includes a junction terminal extension region C2 and a field limiting ring region C3, the field limiting ring region C3 contains a portion of an N-type silicon carbide epitaxial layer 3, the N-type silicon carbide epitaxial layer 3 has a thickness of 10 μm, and a doping concentration of 1×10 16 cm −3 The surface of the N-type silicon carbide epitaxial layer 3 in the field limiting ring region C3 is a bevel structure, and the inclination angle of the bevel structure to the horizontal plane is 2°. The bevel structure is made by a dry etching process, and the etching depth at the end away from the junction terminal extension region C2 is 3.5μm. 20 field limiting rings 11 are formed on the surface of the bevel structure by ion implantation, and the ring width of each field limiting ring 11 is 2.5μm, and the ring spacing between two adjacent field limiting rings 11 is 1μm.
[0033] The terminal structure of Example 1 is used in a silicon carbide MOSFET power device, and the overall structure is as follows: Figure 2 As shown, the preparation method comprises the following steps: (1) Providing a substrate containing a drain metal 1, an N-type silicon carbide substrate 2, and an N-type silicon carbide epitaxial layer 3, cleaning the N-type silicon carbide epitaxial layer 3, and marking the etching position. The thickness of the N-type silicon carbide epitaxial layer 3 is 10 μm, and the doping concentration is 1×10 16 cm −3 .
[0034] (2) Aluminum ions were implanted into the surface of the N-type silicon carbide epitaxial layer 3 for three times, with the energy of each implantation being 100 KeV, 500 KeV, and 800 KeV, and the dose of each implantation being 5×10 11 cm −2 , 1×10 12 cm −2 and 2×10 13 cm −2 , forming a P-type well region 9.
[0035] (3) Perform nitrogen ion implantation three times, with the energy of each implantation being 60 KeV, 100 KeV, and 120 KeV, and the implantation dose being 1.5×10 15 cm −2 , 2×10 15 cm −2 and 1.5×10 15 cm −2 , an N+ region 7 is formed inside the P-type well region 9.
[0036] (4) The N-type silicon carbide epitaxial layer 3 in the field limiting ring region C3 is etched to form a slope structure. The etching angle is 2°, and the etching depth at the end away from the junction terminal extension region C2 is 3.5 μm.
[0037] (5) Aluminum ion implantation was performed simultaneously on the surface of the N-type silicon carbide epitaxial layer 3 and the surface of the bevel structure in the junction terminal extension region C2. The number of implantations was 3 times, and the energy of each implantation was 100 KeV, 400 KeV, and 800 KeV, respectively. The dose of each implantation was 2×10 13 cm −2 , and a junction terminal extension 10 and 20 field limiting rings 11 are formed at the same time. The width of each field limiting ring 11 is 2.5 μm, the ring spacing between two adjacent field limiting rings 11 is 1 μm, and the length of the junction terminal extension 10 is 20 μm.
[0038] (6) Aluminum ion implantation is performed simultaneously on the inner side of the N+ region 7 and the surface of the junction terminal extension 10. The number of implantations is 3, and the implantation energies are 100 KeV, 150 KeV, and 200 KeV, respectively. The dose of each implantation is 1×10 14 cm −2 , 3×10 14 cm −2 and 3×10 14 cm −2 , forming a first P+ region 8 and a second P+ region 12.
[0039] (7) The structure prepared in step (6) is subjected to high temperature annealing to activate the implanted ions at a temperature of 1650° C. for 10 min.
[0040] (8) The structure prepared in step (7) is subjected to dry oxygen oxidation at 1200° C. for 2 hours and then to wet oxygen oxidation at 900° C. for 1 hour to form a gate oxide layer on the surface of the N-type silicon carbide epitaxial layer 3 at the junction of the cell region C1 and the junction terminal extension region C2.
[0041] (9) Using a low pressure chemical vapor deposition process, a polysilicon gate 6 with a thickness of 450 nm is deposited on the gate oxide layer formed in step (8) at a temperature of 600° C. and a growth time of 2 hours.
[0042] (10) Using a plasma enhanced chemical vapor deposition process, a silicon dioxide oxide layer 4 with a thickness of 1.2 μm is deposited on the structure prepared in step (9) at a temperature of 400° C., a radio frequency power of 1000 W, and a growth time of 12 min.
[0043] (11) The silicon dioxide oxide layer 4 above the N+ region 7, the first P+ region 8 and the second P+ region 12 is etched respectively, and a source metal 5 is deposited on the silicon dioxide oxide layer 4, wherein a portion of the source metal 5 is in contact with the N+ region 7 and the first P+ region 8, and another portion of the source metal 5 is located in the junction terminal extension region C2 and in contact with the second P+ region 12, and the source metal 5 is in ohmic contact with the drain metal 1, wherein both the source metal 5 and the drain metal 1 are nickel. After metallization, a silicon carbide MOSFET power device having the terminal structure of Example 1 is obtained.
[0044] Example 2 Embodiment 2 provides a terminal structure of a silicon carbide MOSFET power device, the terminal structure includes a junction terminal extension region C2 and a field limiting ring region C3, the field limiting ring region C3 contains a portion of an N-type silicon carbide epitaxial layer 3, the N-type silicon carbide epitaxial layer 3 has a thickness of 10 μm, and a doping concentration of 1×10 16 cm −3 The surface of the N-type silicon carbide epitaxial layer 3 in the field limiting ring region C3 is a bevel structure, and the inclination angle of the bevel structure to the horizontal plane is 4°. The bevel structure is made by a dry etching process, and the etching depth at the end away from the junction terminal extension region C2 is 7μm. 20 field limiting rings 11 are formed on the surface of the bevel structure by ion implantation, and the ring width of each field limiting ring 11 is 2.5μm, and the ring spacing between two adjacent field limiting rings 11 is 1μm.
[0045] The terminal structure of Example 2 is used in a silicon carbide MOSFET power device, and the preparation method of the overall structure includes the following steps: (1) Providing a substrate containing a drain metal 1, an N-type silicon carbide substrate 2, and an N-type silicon carbide epitaxial layer 3, cleaning the N-type silicon carbide epitaxial layer 3, and marking the etching position. The thickness of the N-type silicon carbide epitaxial layer 3 is 10 μm, and the doping concentration is 1×10 16 cm −3 .
[0046] (2) Aluminum ions were implanted into the surface of the N-type silicon carbide epitaxial layer 3 for three times, with the energy of each implantation being 100 KeV, 500 KeV, and 800 KeV, and the dose of each implantation being 5×10 11 cm −2 , 1×10 12 cm −2 and 2×10 13 cm −2 , forming a P-type well region 9.
[0047] (3) Perform nitrogen ion implantation for three times, with each implantation energy of 60 KeV, 100 KeV, and 120 KeV, and the implantation dose of 1.5 × 10 15 cm −2 , 2×1015 cm −2 and 1.5×10 15 cm −2 , an N+ region 7 is formed inside the P-type well region 9.
[0048] (4) The N-type silicon carbide epitaxial layer 3 in the field limiting ring region C3 is etched to form a slope structure. The etching angle is 4°, and the etching depth at the end away from the junction terminal extension region C2 is 7 μm.
[0049] (5) Aluminum ion implantation was performed simultaneously on the surface of the N-type silicon carbide epitaxial layer 3 and the surface of the bevel structure in the junction terminal extension region C2. The number of implantations was 3 times, and the energy of each implantation was 100 KeV, 400 KeV, and 800 KeV, respectively. The dose of each implantation was 2×10 13 cm −2 , and a junction terminal extension 10 and 20 field limiting rings 11 are formed at the same time. The width of each field limiting ring 11 is 2.5 μm, the ring spacing between two adjacent field limiting rings 11 is 1 μm, and the length of the junction terminal extension 10 is 20 μm.
[0050] (6) Aluminum ion implantation is performed simultaneously on the inner side of the N+ region 7 and the surface of the junction terminal extension 10. The number of implantations is 3, and the implantation energies are 100 KeV, 150 KeV, and 200 KeV, respectively. The dose of each implantation is 1×10 14 cm −2 , 3×10 14 cm −2 and 3×10 14 cm −2 , forming a first P+ region 8 and a second P+ region 12.
[0051] (7) The structure prepared in step (6) is subjected to high temperature annealing to activate the implanted ions; the temperature is 1650° C. and the annealing time is 10 min.
[0052] (8) The structure prepared in step (7) is subjected to dry oxygen oxidation at 1200° C. for 2 hours and then to wet oxygen oxidation at 900° C. for 1 hour to form a gate oxide layer on the surface of the N-type silicon carbide epitaxial layer 3 at the junction of the cell region C1 and the junction terminal extension region C2.
[0053] (9) Using a low pressure chemical vapor deposition process, a polysilicon gate 6 with a thickness of 450 nm is deposited on the gate oxide layer formed in step (8) at a temperature of 600° C. and a growth time of 2 hours.
[0054] (10) Using a plasma enhanced chemical vapor deposition process, a silicon dioxide oxide layer 4 with a thickness of 1.2 μm is deposited on the structure prepared in step (9) at a temperature of 400° C., a radio frequency power of 1000 W, and a growth time of 12 min.
[0055] (11) The silicon dioxide oxide layer 4 above the N+ region 7, the first P+ region 8 and the second P+ region 12 is etched respectively, and a source metal 5 is deposited on the silicon dioxide oxide layer 4. A portion of the source metal 5 is in contact with the N+ region 7 and the first P+ region 8 in the cell region C1, and another portion is located in the junction terminal extension region C2 and in contact with the second P+ region 12. The source metal 5 is in ohmic contact with the drain metal 1. Both the source metal 5 and the drain metal 1 are nickel. After metallization, a silicon carbide MOSFET power device having the terminal structure of Example 2 is obtained.
[0056] Example 3 Embodiment 3 provides a terminal structure of a silicon carbide MOSFET power device, the terminal structure includes a junction terminal extension region C2 and a field limiting ring region C3, the field limiting ring region C3 contains a portion of an N-type silicon carbide epitaxial layer 3, the N-type silicon carbide epitaxial layer 3 has a thickness of 10 μm and a doping concentration of 1×10 16 cm −3 The surface of the N-type silicon carbide epitaxial layer 3 in the field limiting ring region C3 is a bevel structure, and the inclination angle of the bevel structure to the horizontal plane is 6°. The bevel structure is made by a dry etching process, and the etching depth at the end away from the junction terminal extension region C2 is 10μm. 20 field limiting rings 11 are formed on the surface of the bevel structure by ion implantation, and the ring width of each field limiting ring 11 is 2.5μm, and the ring spacing between two adjacent field limiting rings 11 is 1μm.
[0057] The terminal structure of Example 3 is used in a silicon carbide MOSFET power device, and the preparation method of the overall structure includes the following steps: (1) Providing a substrate containing a drain metal 1, an N-type silicon carbide substrate 2, and an N-type silicon carbide epitaxial layer 3, cleaning the N-type silicon carbide epitaxial layer 3, and marking the etching position. The thickness of the N-type silicon carbide epitaxial layer 3 is 10 μm, and the doping concentration is 1×10 16 cm −3 .
[0058] (2) Aluminum ions were implanted into the surface of the N-type silicon carbide epitaxial layer 3 for three times, with the energy of each implantation being 100 KeV, 500 KeV, and 800 KeV, and the dose of each implantation being 5×10 11 cm −2 , 1×10 12 cm −2 and 2×10 13 cm −2 , forming a P-type well region 9.
[0059] (3) Perform nitrogen ion implantation three times, with the energy of each implantation being 60 KeV, 100 KeV, and 120 KeV, and the implantation dose being 1.5×10 15cm −2 , 2×10 15 cm −2 and 1.5×10 15 cm −2 , an N+ region 7 is formed inside the P-type well region 9.
[0060] (4) The N-type silicon carbide epitaxial layer 3 in the field limiting ring region C3 is etched to form a slope structure. The etching angle is 6°, and the etching depth at the end away from the junction terminal extension region C2 is 10 μm.
[0061] (5) Aluminum ion implantation was performed simultaneously on the surface of the N-type silicon carbide epitaxial layer 3 and the surface of the bevel structure in the junction terminal extension region C2. The number of implantations was 3 times, and the energy of each implantation was 100 KeV, 400 KeV, and 800 KeV, respectively. The dose of each implantation was 2×10 13 cm −2 , and at the same time, junction terminal extensions 10 and 20 field limiting rings 11 are formed, the width of each field limiting ring is 2.5 μm, the ring spacing between two adjacent field limiting rings is 1 μm, and the length of the junction terminal extension 10 is 20 μm.
[0062] (6) Aluminum ion implantation is performed simultaneously on the inner side of the N+ region 7 and the surface of the junction terminal extension 10. The number of implantations is 3, and the implantation energies are 100 KeV, 150 KeV, and 200 KeV, respectively. The implantation doses are 1×10 14 cm −2 , 3×10 14 cm −2 and 3×10 14 cm −2 , forming a first P+ region 8 and a second P+ region 12.
[0063] (7) The structure prepared in step (6) is subjected to high temperature annealing to activate the implanted ions at a temperature of 1650° C. for 10 min.
[0064] (8) The structure prepared in step (7) is subjected to dry oxygen oxidation at 1200° C. for 2 hours and then to wet oxygen oxidation at 900° C. for 1 hour to form a gate oxide layer on the surface of the N-type silicon carbide epitaxial layer 3 at the junction of the cell region C1 and the junction terminal extension region C2.
[0065] (9) Using a low pressure chemical vapor deposition process, a polysilicon gate 6 with a thickness of 450 nm is deposited on the gate oxide layer formed in step (8) at a temperature of 600° C. and a growth time of 2 hours.
[0066] (10) Using a plasma enhanced chemical vapor deposition process, a silicon dioxide oxide layer 4 with a thickness of 1.2 μm is deposited on the structure prepared in step (9) at a temperature of 400° C., a radio frequency power of 1000 W, and a growth time of 12 min.
[0067] (11) The silicon dioxide oxide layer 4 above the N+ region 7, the first P+ region 8 and the second P+ region 12 is etched respectively, and a source metal 5 is deposited on the silicon dioxide oxide layer 4. A portion of the source metal 5 is in contact with the N+ region 7 and the first P+ region 8 in the cell region C1, and another portion is located in the junction terminal extension region C2 and in contact with the second P+ region 12. The source metal 5 is in ohmic contact with the drain metal 1. Both the source metal 5 and the drain metal 1 are nickel. After metallization, a silicon carbide MOSFET power device having the terminal structure of Example 3 is obtained.
[0068] Comparative Example 1 Comparative Example 1 provides a terminal structure of a silicon carbide MOSFET power device, the terminal structure includes a junction terminal extension region C2 and a field limiting ring region C3, the field limiting ring region C3 contains a portion of an N-type silicon carbide epitaxial layer 3, the N-type silicon carbide epitaxial layer 3 has a thickness of 10 μm, and a doping concentration of 1×10 16 cm −3 The surface of the N-type silicon carbide epitaxial layer 3 located in the field limiting ring region C3 is a planar structure.
[0069] The terminal structure of Comparative Example 1 is used for a silicon carbide MOSFET power device, and the overall structure is as follows Figure 1 As shown, the preparation method comprises the following steps: (1) Providing a substrate containing a drain metal 1, an N-type silicon carbide substrate 2, and an N-type silicon carbide epitaxial layer 3, cleaning the N-type silicon carbide epitaxial layer 3, wherein the thickness of the N-type silicon carbide epitaxial layer 3 is 10 μm and the doping concentration is 1×10 16 cm −3 .
[0070] (2) Aluminum ions were implanted into the surface of the N-type silicon carbide epitaxial layer 3 for three times with injection energies of 100 KeV, 500 KeV, and 800 KeV, respectively. The dose of each implantation was 5×10 11 cm −2 , 1×10 12 cm −2 and 2×10 13 cm −2 , forming a P-type well region 9.
[0071] (3) Perform nitrogen ion implantation three times, with the energy of each implantation being 60 KeV, 100 KeV, and 120 KeV, and the implantation dose being 1.5×10 15 cm −2, 2×10 15 cm −2 and 1.5×10 15 cm −2 , an N+ region 7 is formed inside the P-type well region 9.
[0072] (4) Aluminum ion implantation was performed simultaneously on the surface of the N-type silicon carbide epitaxial layer 3 in the junction terminal extension region C2 and the field limiting ring region C3. The number of implantations was 3 times, and the implantation energy was 100 KeV, 400 KeV and 800 KeV respectively. The implantation dose was 2×10 13 cm −2 , forming a junction terminal extension 10 and 20 field limiting rings 11, the ring width of each field limiting ring 11 is 2.5μm, the ring spacing between two adjacent field limiting rings 11 is 1μm, and the length of the junction terminal extension 10 is 20μm.
[0073] (5) Aluminum ion implantation is performed simultaneously on the inner side of the N+ region 7 and the surface of the junction terminal extension 10. The number of implantations is 3, and the implantation energies are 100 KeV, 150 KeV, and 200 KeV, respectively. The implantation doses are 1×10 14 cm −2 , 3×10 14 cm −2 and 3×10 14 cm −2 , forming a first P+ region 8 and a second P+ region 12.
[0074] (6) The structure prepared in step (5) is subjected to high temperature annealing to activate the implanted ions at a temperature of 1650° C. for 10 min.
[0075] (7) The structure prepared in step (6) is subjected to dry oxygen oxidation at 1200° C. for 2 hours and then to wet oxygen oxidation at 900° C. for 1 hour to form a gate oxide layer on the surface of the N-type silicon carbide epitaxial layer 3 at the junction of the cell region C1 and the junction terminal extension region C2.
[0076] (8) Using a low pressure chemical vapor deposition process, a polysilicon gate 6 with a thickness of 450 nm is deposited on the gate oxide layer formed in step (7) at a temperature of 600° C. and a growth time of 2 hours.
[0077] (9) Using a plasma enhanced chemical vapor deposition process, a silicon dioxide oxide layer 4 with a thickness of 1.2 μm is deposited on the structure prepared in step (8) at a temperature of 400° C., a radio frequency power of 1000 W, and a growth time of 12 min.
[0078] (10) The silicon dioxide oxide layer 4 above the N+ region 7, the first P+ region 8 and the second P+ region 12 is etched respectively, and a source metal 5 is deposited on the silicon dioxide oxide layer 4, wherein a portion of the source metal 5 is in contact with the N+ region 7 and the first P+ region 8 in the cell region C1, and another portion of the source metal 5 is located in the junction terminal extension region C2 and in contact with the second P+ region 12, and the source metal 5 is in ohmic contact with the drain metal 1, and both the source metal 5 and the drain metal 1 are nickel. After metallization, a silicon carbide MOSFET power device having the terminal structure of comparative example 1 is obtained.
[0079] The performance of silicon carbide MOSFET power devices having the terminal structures of Examples 1 to 3 and Comparative Example 1 was tested respectively. The tilt angle in Example 1 was 2°, the tilt angle in Example 2 was 4°, the tilt angle in Example 3 was 6°, and there was no etching in Comparative Example 1, that is, the tilt angle was 0°.
[0080] Figure 3 The following is a comparison curve of the breakdown voltage of silicon carbide MOSFET power devices with different tilt angles, which is simulated by semiconductor process and device simulation software. Figure 3 As shown in the figure, when the inclination angles are 0°, 2°, 4°, and 6°, respectively, the interface fixed charge density is 1×10 12 cm −2 When the voltage of SiC MOSFET power device increases gradually, the breakdown voltage of SiC MOSFET power device with bevel structure in the field limiting ring area is significantly improved compared with the traditional SiC MOSFET power device without bevel structure.
[0081] Figure 4 The following is a graph showing the breakdown voltage of a 6° inclination silicon carbide MOSFET power device and a conventional silicon carbide MOSFET power device as a function of the interface fixed charge density, obtained by simulation using semiconductor process and device simulation software. Figure 4 As shown, the interface fixed charge density of the silicon carbide MOSFET power device is changed respectively. It can be seen that the breakdown voltage of the silicon carbide MOSFET power device with a tilt angle of 6° increases with the increase of the interface fixed charge density.
[0082] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A terminal structure of a silicon carbide MOSFET power device, the terminal structure comprising a junction terminal extension region (C2) and a field limiting ring region (C3), the junction terminal extension region (C2) being located outside a cell region (C1) of the silicon carbide MOSFET power device, the field limiting ring region (C3) being located outside the junction terminal extension region (C2), the field limiting ring region (C3) containing a portion of an N-type silicon carbide epitaxial layer (3), characterized in that: The surface of the N-type silicon carbide epitaxial layer (3) located in the field limiting ring region (C3) is a slope structure, the inclination angle of the slope structure to the horizontal plane is 2° to 6°, and a plurality of field limiting rings (11) are formed on the surface of the slope structure by ion implantation.
2. The silicon carbide MOSFET power device terminal structure according to claim 1, characterized in that: The inclined surface structure is manufactured by a dry etching process or a V-cutting process. In the inclined surface structure, the etching depth at one end away from the junction terminal extension region (C2) is 3.5 μm to 10 μm.
3. The silicon carbide MOSFET power device terminal structure according to claim 1, characterized in that: The number of the field limiting rings (11) is 15 to 25, the ring width of each field limiting ring (11) is 2 μm to 3 μm, and the ring spacing between two adjacent field limiting rings (11) is 0.5 μm to 2.5 μm.
4. The silicon carbide MOSFET power device terminal structure according to claim 1, characterized in that: The junction terminal extension region (C2) contains a portion of an N-type silicon carbide epitaxial layer (3), and a junction terminal extension (10) is formed on the surface of the N-type silicon carbide epitaxial layer (3) in the junction terminal extension region (C2). The junction terminal extension (10) and a plurality of field limiting rings (11) are simultaneously formed by 2 to 3 ion implantations. During each ion implantation, ion implantation is performed simultaneously on the junction terminal extension (10) and the plurality of field limiting rings (11). The implanted element is aluminum, the energy of each implantation is 100 keV to 800 keV, and the dose of each implantation is 2×10 13 cm −2 .
5. The silicon carbide MOSFET power device terminal structure according to claim 4, characterized in that: The length of the junction terminal extension (10) is 10 μm to 30 μm.
6. The silicon carbide MOSFET power device terminal structure according to claim 4, characterized in that: A second P+ region (12) is formed on the surface of the junction terminal extension (10), and the second P+ region (12) and the first P+ region (8) located in the cell region (C1) are simultaneously formed by 3 to 4 ion implantations. During each ion implantation, the second P+ region (12) and the first P+ region (8) are simultaneously ion implanted. The implanted element is aluminum, the energy of each implantation is 100 keV to 200 keV, and the dose of each implantation is 1×10 14 cm −2 ~3×10 14 cm −2 .
7. The silicon carbide MOSFET power device terminal structure according to claim 6, characterized in that: A gate oxide layer is formed on the surface of the N-type silicon carbide epitaxial layer (3) at the junction of the cell region (C1) and the junction terminal extension region (C2), one side of the gate oxide layer is in contact with the P-type well region (9) in the cell region (C1), and the other side of the gate oxide layer is in contact with the junction terminal extension (10), and a polysilicon gate (6) is deposited on the gate oxide layer.
8. The silicon carbide MOSFET power device terminal structure according to claim 7, characterized in that: A silicon dioxide oxide layer (4) is grown on the surface of a polysilicon gate (6), the surface of an N-type silicon carbide epitaxial layer (3) containing a junction terminal extension (10), and the surface of an N-type silicon carbide epitaxial layer (3) containing a field limiting ring (11); a source metal (5) is deposited on the silicon dioxide oxide layer (4); a portion of the source metal (5) is in contact with an N+ region (7) and a first P+ region (8) in a cell region (C1), and another portion of the source metal (5) is located in a junction terminal extension region (C2) and in contact with a second P+ region (12).
9. The silicon carbide MOSFET power device terminal structure according to claim 1, characterized in that: Before the bevel structure is formed, the thickness of the N-type silicon carbide epitaxial layer (3) in the junction terminal extension region (C2) and the field limiting ring region (C3) is 10 μm, and the doping concentration is 1×10 16 cm −3 .
Citation Information
Patent Citations
Semiconductor device terminal structure with slope and manufacturing method thereof
CN113299735A
Preparation method of silicon carbide composite terminal and composite terminal structure
CN117637450A
Semiconductor device, method for manufacturing semiconductor device, inverter circuit, drive device, vehicle, and elevator
US20240087897A1
Cited By
Steel plate pitting corrosion simulation method and system based on cellular automaton model
CN120180760A