Preparation method of composite positive electrode material
By using secondary spherical agglomerate composite materials in the positive electrode materials of lithium-ion batteries, combining transition metal oxides and phosphates, and introducing carbon nanomaterials, the problems of poor thermal stability and circulation performance of existing materials are solved. It realizes high-performance operation of lithium-ion batteries at high temperatures.
Patent Information
- Application Number
- CN202410983526.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-11-12
AI Technical Summary
Existing lithium-ion battery positive electrode materials such as lithium manganate, lithium manganese phosphate and lithium-rich manganese-based materials have problems such as low capacity, poor circulation performance, and poor thermal stability. The preparation method of composite materials cannot achieve effective synergistic effects between materials. and uniform surface coating, resulting in a significant reduction in battery performance in high temperature environments.
The secondary spherical agglomerate composite positive electrode material is used to combine transition metal oxides and phosphates through the recombination between primary grains, and carbon nanomaterials, fast ion conductors and preliminaries, and formed by spray drying and heat treatment processes. Uniform agglomerates to improve the conductivity and structural stability of the material.
The synergistic effect between different materials is achieved, the rate performance and cycle stability of lithium-ion batteries are improved, and the application scenarios of batteries are expanded, especially in high-temperature environments, which have significantly improved performance.
Smart Images

Figure BDA0004956754460000151 
Figure BDA0004956754460000161 
Figure HDA0004956754500000011
Abstract
Description
Technical field:
[0001] The invention relates to the field of lithium ion batteries, and in particular to a synthesis and preparation method of a composite positive electrode material. Background technology:
[0002] Lithium-ion batteries are ubiquitous in our daily lives, from energy storage in national power grids to electric vehicles, mobile phones and other mobile terminals. With the continuous development of energy technology, the importance of lithium-ion batteries in the energy field will continue to increase in the future. The performance of lithium-ion batteries mainly depends on the positive electrode material.
[0003] Compared with nickel and cobalt, metallic manganese has the advantages of abundant content, low cost and high completeness. Manganese-based positive electrode materials include lithium manganese oxide, lithium-rich manganese-based and lithium iron manganese phosphate and other positive electrode materials in which the transition metal layer Mn accounts for more than 50%.
[0004] Lithium manganese oxide is a relatively mature positive electrode material and is widely used in the two-wheel vehicle market due to its low cost. However, it has shortcomings such as low specific capacity and poor cycle performance, and its market popularity has gradually declined in recent years.
[0005] Transition metal layered oxides are highly favored because of their high energy density. For example, lithium-rich manganese-based cathode materials are considered to be the most promising next-generation cathode materials because of their ultra-high capacity (>250mAh / g). They have excellent low-temperature electrochemical properties, high compaction, and high rate performance. They also have good processing properties and are easy to mass-produce. However, the high capacity is accompanied by irreversible structural deterioration, gas production, and poor thermal stability. Among them, thermal stability is particularly important, which leads to a rapid and substantial capacity decay when the battery is operated in an environment greater than 45°C, which greatly limits the application scenarios of the battery.
[0006] Lithium iron manganese phosphate has the same olivine crystal configuration as lithium iron phosphate. Lithium iron phosphate has become the most commercially valuable cathode material due to its advantages of green environmental protection, good safety, low raw material cost, high abundance, and stable structure. It is widely used in power and energy storage scenarios. Compared with lithium iron phosphate, lithium iron manganese phosphate has a higher voltage platform and an energy density increase of more than 20%, which has a very broad application prospect. However, lithium iron manganese phosphate currently still has problems such as poor electronic conductivity, low lithium ion diffusion coefficient, low energy density, and difficulty in releasing capacity at low temperatures. In particular, due to its own low conductivity, the phosphate system has low electronic conductivity and poor lithium ion diffusion. The best solution to this problem is to coat the surface of the material with carbon material, but the uniform distribution of carbon material on the surface is the key to the good electrochemical performance of the material, which is one of the problems to be solved urgently; at the same time, the phosphate system cathode material also has the problem of low tap density, which is very challenging for its application in power batteries.
[0007] Therefore, whether it is lithium manganese oxide, lithium iron manganese phosphate or lithium-rich manganese-based positive electrode materials, a single material will always have the inevitable problems mentioned above. Therefore, introducing a second or even multiple materials to form a composite positive electrode material has become a breakthrough in solving the problem, and the synergistic effect of the composite materials can achieve the effect of complementary advantages between the materials.
[0008] In recent years, the construction method of composite cathode materials usually adopts the traditional blending form or surface coating form. The idea is based on the composite of secondary particles outside the bulk phase. On the one hand, it is impossible to achieve a stable construction of the material on the surface of the main material. On the other hand, taking the blending form as an example, the surface uniformity of the composite material is poor and the synergistic effect between multiple materials cannot be truly brought into play. Therefore, the form in which the composite cathode material is presented is of utmost importance. The composite between primary particles in the bulk phase is the key starting point to bring into play the advantages of multiple materials.
[0009] At the same time, the above technical solutions cannot form an "organic" whole by compounding two or more materials at the same time, and cannot truly avoid the shortcomings of each component material while expanding the advantages between the components. From the perspective of preparation methods and processes, neither blending nor coating can perfectly solve the problems of composite materials.
[0010] In view of the deficiencies in the prior art, the present invention provides a composite positive electrode material and a preparation method thereof. Summary of the invention:
[0011] In view of the problems existing in the background technology, the present invention proposes a composite positive electrode material and a preparation method thereof.
[0012] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:
[0013] One of the purposes of the present invention is to provide a composite positive electrode material, wherein the composite positive electrode material is a secondary spherical agglomerate, wherein the secondary spherical particle agglomerate is formed by uniform agglomeration of primary crystals, and the primary crystals include a transition metal oxide positive electrode material and a phosphate.
[0014] As a preferred technical solution of the present invention, the transition metal oxide positive electrode material includes any one of a ternary positive electrode material, a lithium-rich positive electrode material or a lithium nickel manganese oxide spinel material, or a combination of at least two of them. The combination can be a ternary positive electrode material and a lithium-rich positive electrode material, a lithium-rich positive electrode material and a lithium nickel manganese oxide spinel material, or a ternary positive electrode material and a lithium nickel manganese oxide spinel material, etc., but not only the existing listed combinations, but also other unlisted combinations within the scope of the combination are equally applicable.
[0015] Preferably, the phosphate is LiB (1-x) Mn xPO4, wherein 0≤x≤1, B is selected from any one of Ni, Co, Fe, Al, Ca, Zn, Mg, Mo, Pb, V or Zr, or a combination of at least two of them, wherein the element combination can be a combination of Ni and Fe, a combination of Fe and Al, a combination of Ca and Mg, a combination of Mo and Pb, a combination of V and Zr or a combination of Zn and Co, etc., but not only the combinations listed herein, but also other combinations not listed within the scope of the combination are equally applicable.
[0016] As a preferred technical solution of the present invention, based on the mass of the composite positive electrode material as 100%, the mass fraction of the transition metal oxide is 0.5%-99.5%, wherein the mass fraction can be 0.5%, 1%, 5%, 8%, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75%, 80%, 85%, 90%, 95%, 99% or 99.5%, etc., but not only the existing listed values, but also other unlisted values within the numerical range are also applicable, preferably 85%-95%. If the content of transition metal oxide is too large, the proportion of phosphate in the composite positive electrode material will be too small, and the phosphate will not be able to play a role in stabilizing the structure. If the content of transition metal oxide is too small, the specific capacity of the composite positive electrode material will decrease.
[0017] As a preferred technical solution of the present invention, based on the mass of the composite positive electrode material as 100%, the mass percentage content of the phosphate in the composite material is 0.5%-99.5%, wherein the mass fraction can be 0.5%, 1%, 5%, 8%, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75%, 80%, 85%, 90%, 95%, 99% or 99.5%, etc., but not only the existing listed values, but also other unlisted values within the numerical range are also applicable, preferably 0.2%-15%. When the phosphate content is too large, the conductivity of the composite positive electrode material will decrease, and when it is too small, the transition metal oxide structure cannot be protected from the damage of the electrolyte side reaction.
[0018] As a preferred technical solution of the present invention, the composite positive electrode material also includes any one or a combination of at least two of carbon nanomaterials, fast ion conductors, pre-lithium agents or inactive substances;
[0019] Due to their high electronic conductivity, carbon nanomaterials can improve the electron transfer rate of composite positive electrode materials, which helps the transfer of electrons during rapid charging and discharging; fast ion conductors can improve the lithium ion transfer rate of composite positive electrode materials due to their high ion conductivity, which helps the transfer of lithium ions during rapid charging and discharging; the low electrochemical activity of inactive substances helps to reduce the attack of byproducts produced by electrolyte decomposition on positive electrode materials.
[0020] Preferably, the carbon nanomaterial includes any one of conductive carbon black, graphene, graphyne or carbon nanotubes, or a combination of at least two thereof.
[0021] Preferably, the fast ion conductor includes any one of LATP, LLZO or LGPS, or a combination of at least two of them, wherein the combination may be a combination of LATP and LLZO, a combination of LGPS and LATP, or a combination of LLZO and LGPS, etc., but not only the existing listed combinations but also other unlisted combinations within the scope of the combination are equally applicable.
[0022] Preferably, the pre-lithium agent includes any one of Li5FeO4, Li2NiO2, Li2C2O4, Li6CoO4, Li2CuO2, LiF, Li2O, Li3N, Li8ZrO6 or Li2C4O4, or a combination of at least two thereof, wherein the combination may be a combination of Li5FeO4 and Li2NiO2, a combination of Li2C2O4 and Li6CoO4, a combination of Li2CuO2 and LiF, or a combination of Li3N and Li2O, etc., but not only the combinations listed in the existing list, but also other combinations not listed in the combination range are also applicable. Preferably, the inactive material includes any one of Al2O3, Fe2O3, TiO2 or ZrO2, or a combination of at least two thereof, wherein the combination may be a combination of Al2O3 and Fe2O3, a combination of TiO2 and ZrO2, a combination of Fe2O3 and ZrO2, or a combination of Al2O3 and ZrO2, etc., but not only the combinations listed in the existing list, but also other combinations not listed in the combination range are also applicable.
[0023] As a preferred technical solution of the present invention, based on the mass of the composite positive electrode material as 100%, the mass percentage content of the carbon nanomaterial in the composite material is 0%-20%, wherein the mass fraction can be 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 1%, 5%, 8%, 10%, 15% or 20%, etc., but not only the existing listed values, but also other unlisted values within the numerical range are also applicable, preferably 0%-5%. The introduction of the carbon nanomaterial of the present invention can improve the conductivity of the material and thus improve the rate performance of the battery system, but too much carbon nanomaterial will cause a decrease in the compaction density of the composite positive electrode material.
[0024] Preferably, based on the mass of the composite positive electrode material as 100%, the mass percentage content of the fast ion conductor in the composite material is 0-20%, wherein the mass fraction can be 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 1%, 5%, 8%, 10%, 15% or 20%, etc., but not only the existing listed values, but also other unlisted values within the numerical range are also applicable, preferably 0-5%. The introduction of the fast ion conductor of the present invention can increase the lithium ion transmission rate in the electrochemical process, thereby improving the rate performance of the battery system, but when there are too many fast ion conductors, the specific capacity of the composite positive electrode material decreases.
[0025] Preferably, based on the mass of the composite positive electrode material as 100%, the mass percentage content of the pre-lithium agent in the composite material is 0-20%, wherein the mass fraction can be 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 1%, 5%, 8%, 10%, 15% or 20%, etc., but not only the existing listed values, but also other unlisted values within the numerical range are also applicable, preferably 0-5%. The introduction of the pre-lithium agent of the present invention can supplement the loss of lithium ions during the battery cycle, thereby improving the stability of electrochemical cycle performance, but when the pre-lithium agent is too much, the specific capacity of the composite positive electrode material decreases.
[0026] Preferably, based on the mass of the composite positive electrode material as 100%, the mass percentage content of the inactive substance in the composite material is 0-20%, wherein the mass fraction can be 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 1%, 5%, 8%, 10%, 15% or 20%, etc., but not only the existing listed values, but also other unlisted values within the numerical range are also applicable, preferably 0-5%. The introduction of inactive substances can further reduce the contact between the positive electrode material and the decomposition byproducts of the electrolyte, reduce the occurrence of malignant side reactions, and improve the battery cycle performance. When there are too many inactive substances, the conductivity of the material will be reduced, resulting in a decrease in the rate performance.
[0027] Compared with the traditional coating method on the surface of secondary spherical particles, the advantages of different materials can be better utilized through the composite between primary crystals. Transition metal oxides have high specific capacity and working voltage, but their structure is easily attacked and destroyed by electrolyte during electrochemical cycles. Phosphates have good structural stability due to their olivine structure, and composite with transition metal oxides to stabilize the structure, thereby improving cycle stability.
[0028] The second object of the present invention is to provide a method for preparing a composite positive electrode material as described in the first object, the preparation method comprising the following steps: mixing a transition metal oxide material, a phosphate and a solvent, grinding them to obtain an intermediate slurry, spray drying the intermediate slurry, and then heat treating them to obtain the composite positive electrode material.
[0029] The spray drying method adopted in the present invention has the following advantages: first, the drying speed is fast. Spray drying can complete the drying process in a very short time, significantly reducing the heating time of the material, which is especially important for heat-sensitive materials. The structure and surface morphology of the positive electrode material can be well maintained. Moreover, since it is carried out in a closed space, the product is not easily contaminated and has a low impurity content. Second, the production efficiency is high. The spray drying process is simple, easy to operate and control, and is particularly suitable for continuous, automated and large-scale production. Compared with traditional drying methods, spray drying reduces the steps of concentration, filtration, and crushing, thereby improving production efficiency.
[0030] As a preferred technical solution of the present invention, the mixture also includes any one or a combination of at least two of carbon nanomaterials, fast ion conductors, pre-lithium agents or inactive substances.
[0031] Preferably, the grinding speed is 2000rpm-2700rpm.
[0032] Preferably, the grinding time is 5h-10h.
[0033] Preferably, the solvent is an alcohol solvent, such as ethanol, propanol, butanol or ethylene glycol.
[0034] Preferably, the grinding is followed by ultrasonic treatment to obtain an intermediate slurry.
[0035] As a preferred technical solution of the present invention, the feed rate of the spray drying is 5ml / min-70ml / min, preferably 20ml / min-50ml / min.
[0036] Preferably, the spray drying pressure is 0.5MPa-1.7MPa, wherein the pressure value may be 0.5MPa, 0.7MPa, 0.8MPa, 1MPa, 1.5MPa or 1.7MPa, etc., but not only the existing listed values, but also other unlisted values within the numerical range are also applicable, preferably 1MPa-1.2MPa. If the spray drying pressure of the present invention is too high, the nucleation size of the composite positive electrode material will be uneven, and if the pressure is too low, the density of the composite positive electrode material will decrease.
[0037] Preferably, the spray drying temperature is 150°C-190°C, wherein the temperature may be 150°C, 160°C, 170°C, 180°C or 190°C, etc., but not only the existing listed values, but also other unlisted values within the numerical range are equally applicable, preferably 150°C-170°C; if the spray drying temperature of the present invention is too high, the solution will evaporate too quickly, the primary grains of the input material will not have enough time to agglomerate, and the size of the composite positive electrode material will be too small; if the spray temperature is too low, the solution will evaporate too slowly, the primary grain agglomeration time will be too long, and the size of the composite positive electrode material will be too large, which is not conducive to lithium ion transmission.
[0038] Preferably, the spray-dried slurry has a solid content of 5%-50%, wherein the solid content may be 5%, 8%, 10%, 15%, 20%, 30%, 40% or 50%, etc., but not only the existing listed values, but also other unlisted values within the numerical range are also applicable, preferably 20%-40%.
[0039] The solid content of the spray-dried slurry of the present invention is too high, the primary grain agglomeration phenomenon is serious before spray drying, and a composite positive electrode material with uniformly distributed primary grains cannot be formed after spray drying. The excessive solid content reduces production efficiency.
[0040] Preferably, the spraying temperature of the spray drying is 100°C-250°C, wherein the temperature can be 100°C, 120°C, 150°C, 160°C, 180°C, 190°C, 220°C or 250°C, etc., but not only the existing listed values, but also other unlisted values within the numerical range are also applicable, preferably 120°C-200°C.
[0041] If the spray temperature of the spray drying of the present invention is too high, the solution evaporates too quickly, the primary crystal grains of the input material do not have enough time to agglomerate, and the size of the composite positive electrode material is too small. If the spray temperature is too low, the solution evaporates too slowly, the primary crystal grain agglomeration time is too long, and the size of the composite positive electrode material is too large, which is not conducive to lithium ion transmission.
[0042] As a preferred technical solution of the present invention, the composite positive electrode material is subjected to heat treatment, and the heat treatment includes: heat treatment in an oxygen atmosphere, the temperature of the heat treatment is 300°C-500°C, and the time of the heat treatment is 1-5h. The heat treatment of the present invention can make the interface between the primary grains more compact, which is conducive to the transmission of lithium ions between the interfaces. When the temperature is too high or the time is too long, it will affect the structure of the material phase. When the temperature is too low or the time is too short, it cannot play the role of interface fusion.
[0043] The third object of the present invention is to provide an application of the composite positive electrode material as described in the first object, wherein the composite positive electrode material is applied in the field of lithium ion batteries.
[0044] The present invention can achieve uniform compounding of different materials. Starting from the dimension of primary particles, the synergistic effect of different component materials can be fully exerted, thus truly realizing the "organic" integration of multiple materials.
[0045] Compared with the prior art, the present invention has the following beneficial effects:
[0046] (1) Compared with the traditional blending or coating, the present invention proposes a composite positive electrode material based on primary particles of different materials, which makes it possible for multiple materials to play a synergistic role, making it a truly composite material rather than just a simple blend.
[0047] (2) The process of the present invention is simple, the conditions are mild, it is easy to scale up and industrialize, and the performance is significantly improved. Description of the drawings:
[0048] Figure 1 Schematic diagram of composite cathode material aggregates.
[0049] Figure 2 This is the SEM morphology of transition metal layered oxide after sand grinding.
[0050] Figure 3 This is the SEM image of lithium manganese iron phosphate (LMFP) after sand grinding.
[0051] Figure 4 This is the SEM image of the composite positive electrode material of Example 1.
[0052] Figure 5 It is a comparison chart of the cycle performance of Comparative Example 1 and Examples 1-3 at room temperature.
[0053] Figure 6 It is a comparison chart of the cycle performance under high temperature of Comparative Example 1 and Examples 1-3.
[0054] Figure 7 It is a comparison chart of the cycle performance of Comparative Example 2 and Examples 4-6 at room temperature.
[0055] Figure 8 It is a comparison chart of the rate performance of Comparative Example 2 and Example 4 at room temperature. Specific implementation method:
[0056] The present invention is described in further detail below in conjunction with specific embodiments. However, it should be understood that these embodiments are only for illustration and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms also fall within the scope defined by the claims of the present application. If specific techniques or conditions are not specified in the embodiments, they are carried out according to the techniques or conditions described in the literature in this field, or according to the product manual. If the manufacturer is not specified for the instruments used, conventional products can be purchased through regular channels. The chemical raw materials used in the present invention can be easily purchased in the domestic chemical product market.
[0057] Embodiment 1:
[0058] A commercial NCM811 positive electrode material and lithium iron manganese phosphate with a mass ratio of 99:1 are selected, an ethanol solution is added, and the mixture is mixed by rapid stirring with a magnetic device to obtain a mixture, the mixture is placed in a sand mill, sand milled at 2700 rpm for 10 hours, and ultrasonically treated for 10 minutes to obtain an intermediate slurry with an average primary grain of 1 micron, the intermediate slurry is placed in a spray dryer, and the intermediate slurry is spray-dried to obtain the composite positive electrode material, wherein the feed rate of the spray drying is 20 ml / mi, the pressure of the spray drying is 1 MPa, the temperature of the spray drying is 150°C, the solid content of the spray-dried slurry is 20%, and the spraying temperature of the spray drying is 150°C.
[0059] The schematic diagram of the composite positive electrode material agglomerate of this embodiment is as follows: Figure 1 The secondary spherical agglomerates of the composite positive electrode material are formed by uniform distribution and agglomeration of primary crystals of different materials. The SEM image of NCM811 after sand grinding without spray drying in this embodiment is as follows: Figure 2 The NCM811 is broken into primary crystals of about 1 micron. The SEM image of the LMFP after sand grinding without spray drying in this embodiment is as follows: Figure 3 The LMFP agglomerates shown in the figure are broken up to form primary crystals of about 500 nm. Figure 4 The composite cathode material shown is a secondary spherical agglomerate. When magnified, it can be seen that it is formed by the agglomeration of multiple primary crystals, which is consistent with Figure 1 Schematic diagram of the composite cathode material shown Figure 1 To.
[0060] Embodiment 2:
[0061] A lithium cobalt oxide single crystal positive electrode material (LiCoO2), lithium iron manganese phosphate and conductive carbon black with a mass ratio of 98:1:1 are selected, an ethanol solution is added, and the mixture is mixed by rapid stirring with a magnetic device to obtain a mixture, the mixture is placed in a sand mill, and sand milled at 2700rpm for 10 hours, and ultrasonically treated for 10 minutes to obtain an intermediate slurry with an average primary grain of 1 micron, the intermediate slurry is placed in a spray dryer, and the intermediate slurry is spray-dried to obtain the composite positive electrode material, wherein the feed rate of the spray drying is 20ml / mi, the pressure of the spray drying is 1MPa, the temperature of the spray drying is 150°C, the solid content of the spray-dried slurry is 20%, and the spraying temperature of the spray drying is 150°C.
[0062] Embodiment 3:
[0063] The lithium-rich cathode material (Li 1.08 Ni 0.22 Co 0.22 Mn 0.45 O2) and lithium manganese iron phosphate, add ethanol solution, mix by rapid stirring with a magnetic particle to obtain a mixture, put the mixture into a sand mill, perform sand milling at 2700rpm for 10 hours, and perform ultrasonic treatment for 10 minutes to obtain an intermediate slurry with an average primary grain of 1 micron, place the intermediate slurry in a spray dryer, and perform spray drying on the intermediate slurry to obtain the composite positive electrode material, wherein the feed rate of the spray drying is 20ml / mi, the pressure of the spray drying treatment is 1MPa, the temperature of the spray drying treatment is 150°C, the solid content of the spray drying treatment slurry is 20%, and the spraying temperature of the spray drying treatment is 150°C. Collect the dried material, transfer it to a tubular furnace, and heat it at 300°C for 3h.
[0064] The room temperature electrochemical data of the composite positive electrode material of this embodiment, embodiments 1-2 and comparative example 1 are as follows: Figure 5 As shown, the composite positive electrode materials of Examples 1-3 are compared with Comparative Example 1, under 1C test conditions, the rate performance is improved to a certain extent, because the introduction of carbon nanomaterials improves the conductivity of the composite positive electrode materials. The high temperature electrochemical data of the composite positive electrode materials of this embodiment and the composite positive electrode materials of Examples 1-2 and Comparative Example 1 are as follows Figure 6 As shown, the rate performance of the composite positive electrode material is significantly improved compared with that of comparative example 1. Under 1C test conditions, the discharge specific capacity is increased by 10mah / g. At the same time, after multiple cycles at room temperature, the capacity retention rate of Examples 1-3 is significantly improved compared with that of Comparative Example 1, among which the capacity retention rate of Example 1 is close to 100% after 100 cycles.
[0065] Embodiment 4:
[0066] The lithium-rich cathode material (Li 1.10 Ni 0.22 Co 0.22 Mn 0.45 O2) and lithium manganese iron phosphate, add ethanol solution, mix by rapid stirring with a magnetic particle to obtain a mixture, put the mixture into a sand mill, perform sand milling at 2700rpm for 10 hours, and perform ultrasonic treatment for 10 minutes to obtain an intermediate slurry with an average primary grain of 1 micron, place the intermediate slurry in a spray dryer, and perform spray drying on the intermediate slurry to obtain the composite positive electrode material, wherein the feed rate of the spray drying is 20ml / mi, the pressure of the spray drying treatment is 1MPa, the temperature of the spray drying treatment is 150°C, the solid content of the spray drying treatment slurry is 20%, and the spraying temperature of the spray drying treatment is 150°C. Collect the dried material, transfer it to a tubular furnace, and heat it at 300°C for 3h.
[0067] The room temperature rate performance test results of this embodiment and comparative example 2 are Figure 7 As shown, the composite positive electrode exhibits a higher discharge specific capacity than that of Comparative Example 2 under high rate test conditions, demonstrating the excellent rate performance of the composite positive electrode material.
[0068] Embodiment 5:
[0069] The NCM622 positive electrode material (LiNi 0.6 Mn 0.2 Co 0.2 O2) and lithium manganese iron phosphate, add ethanol solution, mix by rapid stirring with a magnetic particle to obtain a mixture, put the mixture into a sand mill, perform sand milling at 2700rpm for 10 hours, and perform ultrasonic treatment for 10 minutes to obtain an intermediate slurry with an average primary grain of 1 micron, place the intermediate slurry in a spray dryer, and perform spray drying on the intermediate slurry to obtain the composite positive electrode material, wherein the feed rate of the spray drying is 20ml / mi, the pressure of the spray drying treatment is 1MPa, the temperature of the spray drying treatment is 150°C, the solid content of the spray drying treatment slurry is 20%, and the spraying temperature of the spray drying treatment is 150°C. Collect the dried material, transfer it to a tubular furnace, and heat it at 300°C for 3h.
[0070] Embodiment 6:
[0071] The NCM622 positive electrode material (LiNi 0.6 Mn 0.2 Co 0.2O2) and lithium manganese iron phosphate, add ethanol solution, mix by rapid stirring with a magnetic particle to obtain a mixture, put the mixture into a sand mill, perform sand milling at 2700rpm for 10 hours, and perform ultrasonic treatment for 10 minutes to obtain an intermediate slurry with an average primary grain of 1 micron, place the intermediate slurry in a spray dryer, and perform spray drying on the intermediate slurry to obtain the composite positive electrode material, wherein the feed rate of the spray drying is 20ml / mi, the pressure of the spray drying treatment is 1MPa, the temperature of the spray drying treatment is 150°C, the solid content of the spray drying treatment slurry is 20%, and the spraying temperature of the spray drying treatment is 150°C. Collect the dried material, transfer it to a tubular furnace, and heat it at 300°C for 3h.
[0072] The room temperature electrochemical test comparison of this embodiment, embodiment 4-5 and comparative example 2 is as follows: Figure 8 As shown, Examples 4-6 all exhibited higher discharge specific capacity than Comparative Example 2 under 1C test conditions, proving that the composite positive electrode material has excellent rate performance.
[0073] Comparative Example 1:
[0074] Select commercial NCM811 cathode material (LiNi 0.8 Mn 0.1 Co 0.1 O2), which is the positive electrode material of Comparative Example 1.
[0075] Comparative Example 2:
[0076] The hydroxide precursor was prepared by coprecipitation method, and the lithium-rich cathode material (Li 1.10 Ni 0.22 Co 0.22 Mn 0.45 O2)). It is the positive electrode material of comparative example 2.
[0077] The positive electrode material, conductive agent (acetylene black) and binder (polyvinylidene fluoride, PVDF) in the embodiment and comparative example are weighed in a mass ratio of 8:1:1, and then PVDF is dissolved into a solution with a certain proportion of N-methylpyrrolidone (NMP), and the three are evenly mixed and stirred with a magnetic stirrer for 8-10 hours to obtain a uniformly mixed slurry. The slurry is evenly applied on both sides of a clean and flat aluminum foil, and after standing for 0.5 hours, it is placed in a 120°C vacuum constant temperature drying oven for 16 hours. The dried pole piece is punched into a disc with a diameter of 10mm and maintained at a pressure of 10MPa for 3 minutes on a hydraulic press, and then a secondary drying treatment is performed and dried in a 120°C vacuum drying oven for 8 hours to obtain a positive pole piece; then, a lithium sheet is used as a negative pole piece, and a 1mol / L hexafluorophosphoric acid ethylene carbonate (EC) and dimethyl carbonate (DMC) solution (the volume ratio of EC to DMC is 1:1) is used as an electrolyte, and assembled in a glove box to obtain a lithium-ion battery.
[0078] The lithium-ion battery was tested for cycle performance using an electrochemical tester. The normal temperature test temperature was 25°C, the high temperature test temperature was 45°C, the current density was 0.1C (1C = 200mA / g), the charge and discharge voltage range was 2.8 to 4.4V, and the battery's initial charge and discharge performance was tested. The cycle performance was tested at a rate system of 2.8-4.4V, 1C or 0.5C.
[0079] The lithium-ion battery was rate tested using an electrochemical tester. At room temperature of 25°C, the battery was cycled at 0.1C (1C = 200 mA / g) for 5 cycles, 0.2C for 5 cycles, 0.5C for 5 cycles, 1C for 5 cycles, 2C for 5 cycles, 5C for 5 cycles, and 0.1C for 5 cycles.
[0080] Table 1
[0081]
[0082]
[0083] It can be seen from Table 1 that compared with Comparative Example 1, the discharge specific capacity of 1C of Examples 1-3 is improved, indicating that the rate performance of the composite positive electrode materials of Examples 1-3 is improved relative to that of Comparative Example 1, which is due to the introduction of carbon nanomaterials; the room temperature and high temperature capacity retention rates of the composite positive electrode materials of Examples 1-3 are improved relative to that of Comparative Example 1 within 100 cycles, indicating that the introduction of phosphate helps to stabilize the material structure and improve the cycle retention rate; compared with Comparative Example 2, the discharge specific capacity of 1C of Examples 4-6 is improved, indicating that the rate performance of the composite positive electrode materials of Examples 4-6 is improved relative to that of Comparative Example 2, which is due to the introduction of carbon nanomaterials; the room temperature retention rate of the composite positive electrode materials of Examples 4-6 is not significantly improved relative to that of Comparative Example 2 within 100 cycles, but the advantages of the composite positive electrode materials at high temperatures gradually emerge, indicating that the stable structure of phosphate at high temperatures helps to improve the cycle performance of the composite positive electrode materials.
[0084] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations. In addition, the various different embodiments of the present invention can also be combined arbitrarily, as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.
[0085] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Any simple modification, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention are still within the scope of the technical solution of the present invention.
Claims
1. A composite positive electrode material, characterized in that: The composite positive electrode material is a secondary spherical agglomerate, and the secondary spherical particle agglomerate is formed by uniform agglomeration of primary crystal particles, and the primary crystal particles include a transition metal oxide positive electrode material and phosphate.
2. A composite positive electrode material according to claim 1, characterized in that: The transition metal oxide positive electrode material includes any one of a ternary positive electrode material, a lithium-rich positive electrode material or a lithium nickel manganese oxide spinel material or a combination of at least two thereof; the phosphate is LiB (1-x) Mn x PO4, wherein 0≤x≤1, and B is selected from any one or a combination of at least two of Ni, Co, Fe, Al, Ca, Zn, Mg, Mo, Pb, V or Zr; Taking the mass of the composite positive electrode material as 100%, the mass fraction of the transition metal oxide is 0.5%-99.5%, and the mass percentage content of the phosphate in the composite material is 0.5%-99.5%.
3. A composite positive electrode material according to claim 1, characterized in that: The composite positive electrode material also includes any one or a combination of at least two of a carbon nanomaterial, a fast ion conductor, a pre-lithium agent or an inactive substance; the mass percentage content of the carbon nanomaterial in the composite material is 0%-20%; the mass percentage content of the fast ion conductor in the composite material is 0-20%; The mass percentage content of the pre-lithium agent in the composite material is 0-20%; the mass percentage content of the inactive substance in the composite material is 0-20%; Furthermore, the mass percentage of the carbon nanomaterial in the composite material is 0-5%; the mass percentage of the fast ion conductor in the composite material is 0-5%; the mass percentage of the pre-lithium agent in the composite material is 0-5%; and the mass percentage of the inactive substance in the composite material is 0-5%.
4. A composite positive electrode material according to claim 2, characterized in that: The mass fraction of the transition metal oxide in the composite material is 85%-95%.
5. A composite positive electrode material according to claim 2, characterized in that: The mass percentage content of phosphate in the composite material is 0.2%-15%.
6. A composite positive electrode material according to claim 3, characterized in that: The carbon nanomaterial includes any one of conductive carbon black, graphene, graphyne or carbon nanotubes, or a combination of at least two thereof; The fast ion conductor includes any one of LATP, LLZO or LGPS or a combination of at least two thereof; The pre-lithium agent includes any one of Li5FeO4, Li2NiO2, Li2C2O4, Li6CoO4, Li2CuO2, LiF, Li2O, Li3N, Li8ZrO6 or Li2C4O4, or a combination of at least two thereof; The inactive material includes any one of Al2O3, Fe2O3, TiO2 or ZrO2 or a combination of at least two thereof.
7. A method for preparing a composite positive electrode material according to any one of claims 1 to 6, characterized in that: The transition metal oxide positive electrode material, phosphate and solvent are mixed and ground to obtain an intermediate slurry, and the intermediate slurry is spray-dried to obtain the composite positive electrode material.
8. The method according to claim 7, characterized in that The mixture also includes any one or a combination of at least two of carbon nanomaterials, fast ion conductors, pre-lithium agents or inactive substances; the grinding rotation speed is 2000rpm-2700rpm; the grinding time is 5h-10h; the solvent is an alcohol solvent, and ultrasonic treatment is performed after grinding to obtain an intermediate slurry; the feed rate of the spray drying is 5ml / min-70ml / min, preferably 20ml / min-50ml / min; the pressure of the spray drying is 0.5MPa-1.7MPa, preferably 1MPa-1.2Mpa; the temperature of the spray drying is 150℃-190℃, preferably 150℃-170℃; the solid content of the spray-dried slurry is 5%-50%, preferably 20%-40%; the spraying temperature of the spray drying is 100℃-250℃, preferably 120℃-200℃.
9. The method according to claim 7, characterized in that The composite positive electrode material is subjected to heat treatment, wherein the heat treatment comprises: heat treatment in an oxygen atmosphere, the heat treatment temperature is 300° C.-500° C., and the heat treatment time is 1-5 hours.
10. Use of a composite positive electrode material according to any one of claims 1 to 6, characterized in that: The composite positive electrode material is applied in the field of lithium ion batteries.