Positive electrode active material
By introducing a metal element concentration gradient into the lithium composite oxide, the structural instability problems caused by the unstableness of the positive electrode material of the lithium secondary battery at high temperature and the increase in nickel content are solved, and the thermal stability and electrochemical performance of the battery are improved, and the thermal stability and electrochemical performance of the battery are extended. Battery life.
Patent Information
- Application Number
- CN202410983614.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2020-10-27
- Filing Date
- 2021-08-25
- Publication Date
- 2024-11-12
AI Technical Summary
The existing lithium secondary battery positive electrode materials are unstable at high temperatures, and the increase in nickel content leads to structural instability, affecting battery life and capacity.
By introducing a concentration gradient of metal elements, especially the concentration gradient of nickel and cobalt, into the lithium composite oxide, changes from the surface to the center to improve the thermal stability and electrochemical properties of the material.
It significantly improves the thermal stability and electrochemical properties of high-nickel positive electrode active materials, reduces the side reactions of lithium secondary batteries during charging and discharging, and extends the battery life.
Smart Images

Figure CN118943358A_ABST
Abstract
Description
[0001] This application is a divisional application with an application date of August 25, 2021, application number 202110979237.9, and invention name “Positive electrode active material and lithium secondary battery comprising the same”. Technical Field
[0002] The present invention relates to a positive electrode active material which can improve the electrochemical characteristics and stability of the positive electrode active material comprising the lithium composite oxide by adjusting the concentration gradient direction of metal elements in the lithium composite oxide. Background Art
[0003] Batteries store electricity using materials capable of electrochemical reactions at the positive and negative electrodes. A representative example of such batteries is a lithium secondary battery that stores electrical energy by changes in chemical potential during the insertion / extraction of lithium ions at the positive and negative electrodes.
[0004] The lithium secondary battery is manufactured by using a material that can reversibly intercalate or deintercalate lithium ions as a positive electrode active material and a negative electrode active material, and filling an organic electrolyte or a polymer electrolyte between the positive electrode and the negative electrode.
[0005] As a positive electrode active material of a lithium secondary battery, a lithium composite oxide has been used, and for example, composite oxides of LiCoO 2 , LiMn 2 O 4 , LiNiO 2 , LiMnO 2 , etc. are being studied.
[0006] Among the above-mentioned positive electrode active materials, although LiCoO 2 having excellent life characteristics and charge and discharge efficiency is widely used, the above-mentioned material has limitations in price competitiveness due to the limited resources of cobalt used as a raw material and high price.
[0007] Although lithium manganese oxides such as LiMnO2 and LiMn2O4 have the advantages of good thermal stability and low price, they have problems such as small capacity and poor high temperature characteristics. In addition, although LiNiO2-based positive electrode active materials have battery characteristics of high discharge capacity, they are very difficult to synthesize due to the cation mixing problem between lithium and transition metals, and there are great problems in rate characteristics.
[0008] In addition, depending on the degree of cation mixing, a large amount of lithium by-products are produced.
[0009] Since most lithium byproducts are composed of LiOH and Li2CO3 compounds, there are problems of gelation during the manufacture of positive electrode slurry and gas generation during charge and discharge after the manufacture of electrodes. Residual Li2CO3 increases the expansion of the battery, which not only reduces the cycle but also causes the battery to swell.
[0010] In order to make up for these shortcomings, the demand for high-nickel positive active materials with a nickel content of 50% or more as secondary battery positive active materials has begun to increase. However, although high-nickel positive active materials exhibit high capacity characteristics, there is a problem of structural instability caused by lithium / nickel cation mixing as the nickel content in the positive active material increases. Due to the structural instability of the above-mentioned positive active materials, lithium secondary batteries may deteriorate rapidly not only at high temperatures but also at room temperature.
[0011] Therefore, there is a need to develop a positive electrode active material for compensating for the problems of the above-mentioned high-nickel type positive electrode active material. Summary of the invention
[0012] Technical issues
[0013] In the lithium secondary battery market, the growth of lithium secondary batteries for electric vehicles plays a leading role in the market, and the demand for positive electrode materials used in lithium secondary batteries is also changing.
[0014] For example, conventionally, lithium secondary batteries using LFP have been mainly used from the viewpoint of ensuring safety, but recently, the use of nickel-based lithium composite oxides having a larger energy capacity per unit weight than LFP has been expanding.
[0015] In view of such a trend in positive electrode materials, an object of the present invention is to provide a high-nickel lithium composite oxide for achieving a high capacity of automobile batteries or a positive electrode active material including the lithium composite oxide.
[0016] And, another object of the present invention is to provide a positive electrode comprising the positive electrode active material defined herein.
[0017] In addition, another object of the present invention is to provide a lithium secondary battery using the positive electrode defined herein.
[0018] Solutions to the problem
[0019] According to one aspect of the present invention, a positive electrode active material is provided, which includes a lithium composite oxide capable of lithium insertion and deinsertion, at least one metal element in the above-mentioned lithium composite oxide presents a concentration gradient including a first concentration gradient interval with a (+) slope from the outermost surface of the above-mentioned lithium composite oxide toward the center portion and a second concentration gradient interval with a (-) slope toward the inside of the above-mentioned first concentration gradient interval, and the above-mentioned first concentration gradient interval exists from the outermost surface of the above-mentioned lithium composite oxide to a depth of 0.10μm.
[0020] In one embodiment, when the average diameter of the lithium composite oxide is defined as d, the first concentration gradient region and the second concentration gradient region exist within a depth range of 0.05d to 0.33d from the outermost surface of the lithium composite oxide.
[0021] In one embodiment, the first concentration gradient region and the second concentration gradient region may exist from the outermost surface of the lithium composite oxide to a depth of 1 μm.
[0022] In one embodiment, the first concentration gradient region and the second concentration gradient region may exist within a range from the outermost surface of the lithium composite oxide to a depth of 0.50 μm.
[0023] In one embodiment, the first concentration gradient range and the second concentration gradient range may exist in the bulk particle.
[0024] In one embodiment, the lithium composite oxide may have a single bulk structure, and the first concentration gradient region and the second concentration gradient region exist in the single bulk structure.
[0025] In one embodiment, the concentration of nickel in the lithium composite oxide may decrease from the surface portion toward the center portion of the lithium composite oxide in the first concentration gradient interval, while the concentration of cobalt increases, and the concentration of nickel in the lithium composite oxide may increase from the surface portion toward the center portion of the lithium composite oxide in the second concentration gradient interval, while the concentration of cobalt decreases.
[0026] In one embodiment, the concentration of at least one selected from manganese and aluminum in the lithium composite oxide in the first concentration gradient interval increases from the surface of the lithium composite oxide toward the center, and the concentration of at least one selected from manganese and aluminum in the lithium composite oxide in the second concentration gradient interval decreases from the surface of the lithium composite oxide toward the center.
[0027] In one embodiment, the positive electrode active material may have a concentration retention zone, which is located inside the second concentration gradient zone and maintains the concentration of at least one metal element in the lithium composite oxide from the surface portion toward the center portion.
[0028] In one embodiment, the absolute value of the concentration change rate of the at least one metal element in the concentration maintaining range may be less than 5 mol %.
[0029] In one embodiment, the concentration of nickel in the lithium composite oxide in the concentration maintaining range may be greater than that in the first concentration gradient range and the second concentration gradient range.
[0030] In one embodiment, the concentration of at least one selected from cobalt, manganese and aluminum in the lithium composite oxide in the first concentration gradient range and the second concentration gradient range may be greater than that in the concentration maintaining range.
[0031] In one embodiment, the lithium composite oxide may be represented by the following chemical formula 1:
[0032] Li w Ni 1-(x+y+z) Co x M1 y M2 z O 2+δ
[0033] Among them, M1 is at least one selected from Mn or Al, M2 is at least one selected from P, Sr, Ba, B, Ti, Zr, Mn, Al, W, Ce, Hf, Ta, F, Mg, Cr, V, Fe, Zn, Si, Y, Ga, Sn, Mo, Ge, Nd, Gd and Cu, M1 and M2 are different elements, 0.5≤w≤1.5, 0≤x≤0.50, 0≤y≤0.20, 0≤z≤0.20, 0≤δ≤0.02.
[0034] In one embodiment, the lithium composite oxide may contain nickel at a concentration of 80 mol % or more in all elements other than lithium.
[0035] In one embodiment, the lithium composite oxide may have a core-shell structure, in which the first concentration gradient interval exists in the shell and the second concentration gradient interval exists in the core, or the first concentration gradient interval and the second concentration gradient interval exist in the core, or the first concentration gradient interval and the second concentration gradient interval exist in the shell.
[0036] According to one aspect of the present invention, there is provided a positive electrode active material, characterized in that it comprises a lithium composite oxide capable of lithium insertion and extraction, wherein at least one metal element in the lithium composite oxide presents a concentration gradient including a first concentration gradient interval having a (+) slope and a second concentration gradient interval having a (-) slope from an outermost surface toward a center of the lithium composite oxide.
[0037] The first concentration gradient interval and the second concentration gradient interval may exist continuously from the outermost surface of the lithium composite oxide. Furthermore, the first concentration gradient interval may exist from the outermost surface of the lithium composite oxide to a predetermined depth, and the second concentration gradient interval may be located inside the first concentration gradient interval.
[0038] The positive electrode active material according to the present invention is characterized in that, within the first concentration gradient interval, the concentration of nickel in the lithium composite oxide can decrease from the surface portion toward the center portion of the lithium composite oxide, and the concentration of at least one selected from cobalt, manganese and aluminum can increase; and within the second concentration gradient interval, the concentration of nickel in the lithium composite oxide can increase from the surface portion toward the center portion of the lithium composite oxide, and the concentration of at least one selected from cobalt, manganese and aluminum can present a decreasing concentration gradient.
[0039] The lithium composite oxide may be represented by Chemical Formula 1 below.
[0040] Li w Ni 1-(x+y+z) Co x M1 y M2 z O 2+δ
[0041] (wherein, M1 is at least one selected from Mn or Al, M2 is at least one selected from P, Sr, Ba, B, Ti, Zr, Mn, Al, W, Ce, Hf, Ta, F, Mg, Cr, V, Fe, Zn, Si, Y, Ga, Sn, Mo, Ge, Nd, Gd and Cu, M1 and M2 are different elements, 0.5≤w≤1.5, 0≤x≤0.50, 0≤y≤0.20, 0≤z≤0.20, 0≤δ≤0.02).
[0042] And, according to another aspect of the present invention, there is provided a cathode comprising the cathode active material defined herein.
[0043] In addition, according to yet another aspect of the present invention, there is provided a lithium secondary battery using the positive electrode defined herein.
[0044] Effects of the Invention
[0045] Generally, high-nickel positive electrode active materials used to achieve high capacity of lithium secondary batteries have the problem of low thermal stability. However, the positive electrode active material according to the present invention improves the low thermal stability of the high-nickel positive electrode active material by adjusting the concentration gradient direction of the metal elements in the lithium composite oxide constituting the above-mentioned positive electrode active material, and at the same time has the advantage of improving high temperature working characteristics.
[0046] On the other hand, in the case of a high-nickel type positive electrode active material, compared with a positive electrode active material with a relatively low nickel content, a large amount of lithium by-products such as LiOH and Li2CO3 are present, and the above-mentioned lithium by-products may become the cause of gelation when a positive electrode slurry is prepared using the above-mentioned positive electrode active material, or become the cause of gas generation during charging / discharging and / or storage of a lithium secondary battery.
[0047] However, when the metal elements in the above-mentioned lithium composite oxide contained in the positive electrode active material according to the present invention present a concentration gradient that simultaneously includes a first concentration gradient interval with a (+) slope from the outermost surface of the above-mentioned lithium composite oxide toward the center portion and a second concentration gradient interval with a (-) slope, the content of lithium by-products in the surface of the above-mentioned positive electrode active material can be reduced.
[0048] In addition, the surface of the positive electrode active material is an area where side reactions may occur with the electrolyte during the charge / discharge and / or storage process of the lithium secondary battery. The larger the surface area of the positive electrode active material (which can be represented by an index such as BET specific surface area), the greater the possibility of side reactions. Therefore, the crystal structure in the surface of the positive electrode active material may undergo a phase transformation (e.g., layered structure → rock salt structure). The phase transformation of the crystal structure in the surface of the positive electrode active material as described above is pointed out to be one of the reasons for reducing the life characteristics of the lithium secondary battery.
[0049] In the case of the positive electrode active material according to the present invention, it is confirmed that by making the metal elements in the above-mentioned lithium composite oxide present a concentration gradient that simultaneously includes a first concentration gradient interval with a (+) slope and a second concentration gradient interval with a (-) slope from the outermost surface of the above-mentioned lithium composite oxide toward the center, the surface area that undergoes side reactions with the electrolyte during the charging / discharging and / or storage of the lithium secondary battery can be reduced (for example, it can be represented by indicators such as BET specific surface area), thereby reducing the possibility of side reactions with the electrolyte during the charging / discharging and / or storage of the lithium secondary battery.
[0050] As a result, the positive electrode active material according to the present invention helps to improve not only the basic physical properties of the above-mentioned positive electrode active material, but also the electrochemical characteristics such as life characteristics and efficiency characteristics by adjusting the concentration gradient direction of the metal elements in the lithium composite oxide constituting the above-mentioned positive electrode active material. BRIEF DESCRIPTION OF THE DRAWINGS
[0051] Figure 1 is a cross-sectional SEM image obtained after the lithium composite oxide contained in the positive electrode active material according to Example 2 was subjected to cross-sectional processing using FIB (gallium ion source).
[0052] Figure 2 To show that through Figure 1 A graph (line sum spectrum) showing the contents of metal elements (Ni, Co, Mn) present in a direction from the outermost surface toward the center of the lithium composite oxide confirmed by EDX analysis of a cross-sectional SEM image.
[0053] Figure 3 is a cross-sectional SEM image obtained after the lithium composite oxide contained in the positive electrode active material according to Comparative Example 1 was subjected to cross-sectional processing using FIB (gallium ion source).
[0054] Figure 4 To show that through Figure 3 A graph (line and spectrum) showing the contents of metal elements (Ni, Co, Mn) in a direction from the outermost surface toward the center of the lithium composite oxide confirmed by EDX analysis of a cross-sectional SEM image.
[0055] Figure 5 Graph (line and spectrum) showing the contents of metal elements (Ni, Co, Mn) present in the direction from the outermost surface toward the center of the lithium composite oxide as confirmed by EDX analysis of the cross-sectional SEM image of Example 3.
[0056] Figure 6 Graph (line and spectrum) showing the contents of metal elements (Ni, Co, Mn) present in the direction from the outermost surface toward the center of the lithium composite oxide as confirmed by EDX analysis of the cross-sectional SEM image of Example 4.
[0057] Figure 7 Graph (line and spectrum) showing the contents of metal elements (Ni, Co, Mn) present in the direction from the outermost surface toward the center of the lithium composite oxide as confirmed by EDX analysis of the cross-sectional SEM image of Example 5.
[0058] Figure 8 Graph (line and spectrum) showing the contents of metal elements (Ni, Co, Mn) present in the direction from the outermost surface toward the center of the lithium composite oxide as confirmed by EDX analysis of the cross-sectional SEM image of Example 6. DETAILED DESCRIPTION
[0059] Hereinafter, the cathode active material according to the present invention and a lithium secondary battery using a cathode including the cathode active material will be described in further detail.
[0060] Positive electrode active material
[0061] According to one aspect of the present invention, a positive electrode active material including a lithium composite oxide capable of inserting and extracting lithium is provided. The lithium composite oxide may include primary particles having a layered crystal structure and secondary particles formed by agglomerating the primary particles.
[0062] Here, the primary particle refers to a crystal grain (grain or crystallite), and the secondary particle refers to an aggregate formed by agglomeration of a plurality of primary particles. There may be gaps and / or grain boundaries between the primary particles constituting the secondary particles.
[0063] For example, the primary particles may be spaced apart from adjacent primary particles in the secondary particles to form internal voids. In addition, the primary particles may form surfaces present inside the secondary particles by contacting the internal voids, rather than forming grain boundaries by contacting adjacent primary particles.
[0064] On the other hand, the surface of the primary particle present on the outermost surface of the secondary particle, which is exposed to the outside air, forms the surface of the secondary particle.
[0065] The average particle size of the primary particles is 0.1 μm to 5 μm, preferably 0.1 μm to 3 μm, so that the optimal density of the positive electrode prepared using the positive electrode active material according to various embodiments of the present invention can be achieved. In addition, the average particle size of the secondary particles may vary depending on the number of agglomerated primary particles, and may be 3 μm to 20 μm.
[0066] As for the above-mentioned lithium composite oxide contained in the positive electrode active material according to various embodiments of the present invention, at least one metal element in the above-mentioned lithium composite oxide can present a concentration gradient that simultaneously includes a first concentration gradient interval with a (+) slope and a second concentration gradient interval with a (-) slope from the outermost surface toward the center of the above-mentioned lithium composite oxide.
[0067] Wherein, regarding the concentration gradient presented by at least one metal element in the lithium composite oxide, for example, the (+) slope and the (-) slope can be derived from a concentration change curve of the metal element measured from the outermost surface toward the center of the lithium composite oxide by EDX analysis of a cross section of the lithium composite oxide. In addition, the ordinal number used to refer to the concentration gradient interval having a (+) and / or (-) slope is only used to distinguish between the concentration gradient interval having a (+) slope and the concentration gradient interval having a (-) slope.
[0068] From the concentration change or concentration gradient of the metal element measured from the outermost surface toward the center of the lithium composite oxide by EDX analysis of the cross section of the lithium composite oxide, the overall concentration gradient of the bulk lithium composite oxide, rather than the concentration gradient of the cross section, can be predicted.
[0069] The concentration gradient having a (+) slope from the outermost surface toward the center of the lithium composite oxide means that the concentration of at least one metal element in the lithium composite oxide increases from the outermost surface toward the center of the lithium composite oxide. Conversely, the concentration gradient having a (+) slope from the outermost surface toward the center of the lithium composite oxide means that the concentration of at least one metal element in the lithium composite oxide decreases from the outermost surface toward the center of the lithium composite oxide.
[0070] Furthermore, the concentration gradient having a (+) slope from the outermost surface toward the center of the lithium composite oxide means that the slope of the concentration value of the specific metal element between the start point and the end point of the concentration gradient having a (+) slope is sufficient, regardless of the (+) slope.
[0071] The slope change is caused by the slight difference in the concentration value of a specific metal element in a part of the interval between the starting point and the end point of the concentration gradient interval with a slope. At this time, the slight difference in the concentration value may mean that there is no concentration value in a part of the interval within the concentration gradient interval with a (+) slope that is less than the concentration value of the metal element at the starting point of the concentration gradient interval with a (+) slope or greater than the concentration value at the end point of the concentration gradient interval with a (+) slope.
[0072] Similarly, the concentration gradient having a (-) slope from the outermost surface toward the center of the above-mentioned lithium composite oxide should be understood as that the slope of the concentration value of the specific metal element between the starting point and the end point of the concentration gradient interval having the (-) slope is sufficient. Therefore, the slope change caused by the slight difference in the concentration value of the specific metal element in a part of the interval between the starting point and the end point of the above-mentioned concentration gradient interval having the (-) slope is not taken into account, which can mean that in a part of the interval within the above-mentioned concentration gradient interval having the (-) slope, there is no concentration value greater than the concentration value of the metal element at the starting point of the above-mentioned concentration gradient interval having the (-) slope or less than the concentration value at the end point of the above-mentioned concentration gradient interval having the (-) slope.
[0073] For example, presenting a concentration gradient having a (+) slope from the outermost surface toward the center of the above-mentioned lithium composite oxide may mean that the slope of the concentration value of the specific metal element between the starting point and the end point of the concentration gradient interval having the (+) slope is (+), and the absolute value of the difference in the concentration value of the specific metal element between the starting point and the end point of the above-mentioned concentration gradient having the (+) slope is greater than 5.0 mol%.
[0074] Furthermore, presenting a concentration gradient having a (-) slope from the outermost surface toward the center of the above-mentioned lithium composite oxide may mean that the slope of the concentration value of the specific metal element between the starting point and the end point of the concentration gradient interval having the (-) slope is (-), and the absolute value of the difference in the concentration value of the specific metal element between the starting point and the end point of the above-mentioned concentration gradient having the (-) slope is greater than 5.0 mol%.
[0075] In one embodiment, the concentration gradient in the lithium composite oxide may be present from the outermost surface of the lithium composite oxide. More specifically, the first concentration gradient region and the second concentration gradient region may exist continuously from the outermost surface of the lithium composite oxide.
[0076] That is, the lithium composite oxide according to the present invention presents a concentration gradient in which the concentration of at least one metal element in the lithium composite oxide increases and decreases from the outermost surface of the lithium composite oxide, thereby improving the electrochemical characteristics and stability of the lithium composite oxide. In addition, by presenting a concentration gradient in which the concentration of at least one metal element in the lithium composite oxide increases and decreases from the outermost surface of the lithium composite oxide, the surface side reaction of the lithium composite oxide is reduced by reducing the specific surface area of the lithium composite oxide.
[0077] Furthermore, according to the present invention, preferably, when the average particle size D50 of the above-mentioned lithium composite oxide (secondary particles) is defined as d, the above-mentioned first concentration gradient interval and the above-mentioned second concentration gradient interval exist in the depth range from the outermost surface of the above-mentioned lithium composite oxide to 0.05d to 0.33d.
[0078] Furthermore, the first concentration gradient interval and the second concentration gradient interval exist from the outermost surface of the lithium composite oxide to a depth of 1 μm, preferably, to a depth of 0.75 μm, preferably, to a depth of 0.50 μm. When the first concentration gradient interval and the second concentration gradient interval exist from the outermost surface of the lithium composite oxide to a depth greater than 1 μm, the crystal structure in the surface portion of the lithium composite oxide may be unstable.
[0079] At this time, even though the first concentration gradient region and the second concentration gradient region may exist from the outermost surface of the lithium composite oxide to a depth of 0.33d, the second concentration gradient region preferably exists from the outermost surface of the lithium composite oxide to a depth of 1 μm or less.
[0080] In this case, there may be a concentration maintaining interval from the end point of the second concentration gradient interval relatively close to the center of the lithium composite oxide (i.e., the inner side of the second concentration gradient interval), in which the concentration of at least one metal element in the lithium composite oxide is maintained from the surface of the lithium composite oxide toward the center.
[0081] The above-mentioned concentration maintenance interval may refer to an interval in which the absolute value of the concentration change rate of at least one metal element is 5.0 mol % or less, preferably 3.0 mol % or less, and more preferably 2.0 mol % or less.
[0082] Therefore, in the above-mentioned lithium composite oxide, the above-mentioned first concentration gradient interval and the above-mentioned second concentration gradient interval exist in sequence from the outermost surface of the above-mentioned lithium composite oxide to a predetermined depth, and there is a concentration retention interval inside the above-mentioned second concentration gradient interval, so that the crystal structure of the above-mentioned lithium composite oxide can be stabilized.
[0083] As described above, the first concentration gradient region exists from the outermost surface of the lithium composite oxide to a predetermined depth, and the second concentration gradient region is located inside the first concentration gradient region.
[0084] At this time, in the first concentration gradient interval, the concentration of nickel in the lithium composite oxide may decrease from the surface portion toward the center portion of the lithium composite oxide, and the concentration of at least one selected from cobalt, manganese and aluminum may increase; in the second concentration gradient interval, the concentration of nickel in the lithium composite oxide may increase from the surface portion toward the center portion of the lithium composite oxide, and the concentration of at least one selected from cobalt, manganese and aluminum may decrease.
[0085] As described above, there is an increase or decrease in the concentration of nickel in the lithium composite oxide in the area close to the outermost surface of the lithium composite oxide. More specifically, there is a concentration gradient in which the concentration of nickel in the lithium composite oxide decreases by a predetermined amount from the outermost surface of the lithium composite oxide and then increases. This has the advantage of reducing cation mixing of lithium ions and nickel ions on the surface of the lithium composite oxide.
[0086] In the case of a high-nickel type (nickel ≥ 80 mol%) lithium composite oxide in which the average composition of the above-mentioned lithium composite oxide contains a relatively high nickel content, the electrochemical properties are reduced due to the mixing of lithium / nickel cations occurring on the surface, and the crystal structure is unstable due to the excessively high nickel content in the above-mentioned lithium composite oxide.
[0087] However, as shown in the lithium composite oxide disclosed in this article, when there is a concentration gradient in which the concentration of nickel in the above-mentioned lithium composite oxide decreases by a predetermined amount from the outermost surface of the above-mentioned lithium composite oxide and then increases (in this case, at least one selected from cobalt, manganese and aluminum has a concentration gradient opposite to that of nickel), there is the following advantage, namely, the mixing of lithium / nickel cations is reduced in the surface portion of the above-mentioned lithium composite oxide, thereby achieving the stabilization of the overall crystal structure of the above-mentioned lithium composite oxide.
[0088] Furthermore, in one embodiment, in the case of the concentration of nickel in the lithium composite oxide, the concentration in the concentration maintaining interval may be greater than the concentration in the first concentration gradient interval and the second concentration gradient interval. Thus, as described above, even if the nickel content in the average composition of the lithium composite oxide is high (nickel ≥ 80 mol%), the possibility of lithium / nickel cation mixing in the surface portion can be reduced by adjusting the nickel content in the first concentration gradient interval and the second concentration gradient interval relatively close to the surface portion of the lithium composite oxide.
[0089] In this case, the concentration of at least one selected from cobalt, manganese and aluminum in the above-mentioned lithium composite oxide is adjusted so that the concentration in the above-mentioned first concentration gradient interval and the above-mentioned second concentration gradient interval is greater than the concentration in the above-mentioned concentration maintaining interval, thereby stabilizing the overall crystal structure of the above-mentioned lithium composite oxide.
[0090] On the other hand, the lithium composite oxide defined in this article may be an oxide having a core-shell structure. In this case, the first concentration gradient interval, the second concentration gradient interval, and the concentration retention interval are present in the core, and the coating described below may be present as a shell in at least a portion of the surface of the core. At this time, the first concentration gradient interval, the second concentration gradient interval, and the concentration retention interval may exist sequentially from the outermost surface of the core.
[0091] Furthermore, in another embodiment, in the core-shell structure, the first concentration gradient interval may exist in the shell, and the second concentration gradient interval and the concentration holding interval may exist in the core. In another embodiment, in the core-shell structure, the first concentration gradient interval and the second concentration gradient interval may exist in the shell, and the concentration holding interval may exist in the core. If the first concentration gradient interval or the first concentration gradient interval and the second concentration gradient interval exist in the shell, a coating described below may be selectively present on at least a portion of the surface of the shell.
[0092] In another embodiment, the lithium composite oxide is an oxide having a core-shell structure, and the first concentration gradient region and the second concentration gradient region may exist in the form of surrounding the surface of the shell.
[0093] In the lithium composite oxides having the various core-shell structures, the core and the shell may exist as independent layers distinguishable from each other, or the core and the shell may exist as substantially indistinguishable (eg, solid-dissolved) layers.
[0094] Furthermore, the lithium composite oxide defined herein may have a single bulk structure instead of a core-shell structure, and the first concentration gradient region, the second concentration gradient region, and the concentration retention region may exist in the single bulk structure.
[0095] The above-mentioned lithium composite oxide defined herein may be represented by Chemical Formula 1 below.
[0096] Li w Ni 1-(x+y+z) Co x M1 y M2 z O 2+δ
[0097] Among them, M1 is at least one selected from Mn or Al, M2 is at least one selected from P, Sr, Ba, B, Ti, Zr, Mn, Al, W, Ce, Hf, Ta, F, Mg, Cr, V, Fe, Zn, Si, Y, Ga, Sn, Mo, Ge, Nd, Gd and Cu, M1 and M2 are different elements, 0.5≤w≤1.5, 0≤x≤0.50, 0≤y≤0.20, 0≤z≤0.20, 0≤δ≤0.02.
[0098] In this case, the lithium composite oxide may be Ni, Co,
[0099] The concentrations (mol %) of M1 and M2 satisfy the following formula 1 for a high nickel type lithium composite oxide.
[0100] [Formula 1]
[0101] Ni / (Ni+Co+M1+M2)≥80.0
[0102] Also, the positive active material according to various embodiments of the present invention may include a coating layer covering at least a portion of the surface of the primary particles (eg, interfaces between the primary particles) and / or secondary particles formed by agglomerating the primary particles.
[0103] For example, the coating layer may exist in a manner of covering at least a portion of the exposed surface of the primary particle. In particular, the coating layer may exist in a manner of covering at least a portion of the exposed surface of the primary particle at the outermost periphery of the secondary particle.
[0104] Thus, the coating layer may exist as a layer that continuously or discontinuously coats the surface of the primary particles and / or the secondary particles formed by agglomerating the primary particles. When the coating layer exists discontinuously, it may exist in the form of islands.
[0105] The presence of the coating as above can help improve the physical and electrochemical characteristics of the positive electrode active material.
[0106] Furthermore, the coating layer may exist in the form of a solid solution without forming a boundary with the primary particles and / or the secondary particles formed by agglomerating the primary particles.
[0107] The coating layer may include at least one oxide represented by the following Chemical Formula 2. That is, the coating layer may be defined as a region where the oxide represented by the following Chemical Formula 2 exists.
[0108] [Chemical formula 2]
[0109] Li a M3 b O c
[0110] (Wherein, M3 is at least one selected from Ni, Mn, Co, Fe, Cu, Nb, Mo, Ti, Al, Cr, Zr, Zn, Na, K, Ca, Mg, Pt, Au, B, P, Eu, Sm, W, V, Ba, Ta, Sn, Hf, Ce, Gd and Nd, and 0≤a≤10, 0≤b≤8, 2≤c≤13)
[0111] Also, the coating layer may have a form in which different types of oxides are simultaneously present in the same layer or different types of oxides represented by the above Chemical Formula 2 may exist in separate layers, respectively.
[0112] The oxide represented by the above Chemical Formula 2 may be physically and / or chemically bonded to the primary particles represented by the above Chemical Formula 1. Also, the oxide may exist in a state of forming a solid solution with the primary particles represented by the above Chemical Formula 1.
[0113] The positive electrode active material according to the present embodiment includes a coating, and the coating covers at least a portion of the surface of the primary particles (e.g., the interface between the primary particles) and / or the secondary particles formed by agglomerating the primary particles, thereby improving the structural stability. Moreover, when the positive electrode active material is used in a lithium secondary battery, the high temperature storage stability and life characteristics of the positive electrode active material can be improved. Moreover, the oxide reduces the residual lithium in the positive electrode active material and serves as a path for the movement of lithium ions, thereby affecting the efficiency characteristics of the lithium secondary battery.
[0114] Furthermore, depending on circumstances, the oxide may exist not only at the interface between the primary particles and at least a portion of the surface of the secondary particles, but also in internal voids formed in the secondary particles.
[0115] The oxide is an oxide obtained by combining lithium and an element represented by A or an oxide of A. Examples of the oxide are Li a W b O c , Li a Zr b O c , Li a Ti b O c , Li a Ni b O c , Li a B b O c , W b O c 、Zr b O c 、Ti b O c or B b O c However, the above examples are only described for ease of understanding, and the above oxides defined in this article are not limited to the above examples.
[0116] In another embodiment, the oxide may be an oxide formed by compounding lithium and at least two elements represented by A or further includes an oxide formed by compounding lithium and at least two elements represented by A. Examples of the oxide formed by compounding lithium and at least two elements represented by A may be Li a (W / Ti) b O c , Li a (W / Zr) b O c , Li a (W / Ti / Zr) b O c Li a (W / Ti / B) b O c Etc., but the present invention is not limited thereto.
[0117] The oxide may present a concentration gradient that decreases from the surface of the secondary particle toward the center of the secondary particle. Thus, the concentration of the oxide may decrease from the outermost surface of the secondary particle toward the center of the secondary particle.
[0118] As described above, the oxide presents a concentration gradient that decreases from the surface of the secondary particle toward the center of the secondary particle, thereby effectively reducing the residual lithium present on the surface of the positive electrode active material to prevent side reactions caused by unreacted residual lithium. In addition, the oxide can also prevent the crystallinity of the inner surface area of the positive electrode active material from decreasing. In addition, the oxide can prevent the overall structure of the positive electrode active material from collapsing during the electrochemical reaction.
[0119] Furthermore, the coating layer may include a first oxide layer and a second oxide layer, the first oxide layer including at least one oxide represented by the chemical formula 2, and the second oxide layer including at least one oxide represented by the chemical formula 2 different from the oxide included in the first oxide layer.
[0120] For example, the first oxide layer may exist in a manner that covers at least a portion of the exposed surface of the primary particle present at the outermost periphery of the secondary particle, and the second oxide layer may exist in a manner that covers at least a portion of the exposed surface of the primary particle not covered by the first oxide layer and the surface of the first oxide layer.
[0121] Lithium secondary battery
[0122] According to another aspect of the present invention, a positive electrode including a positive electrode current collector and a positive electrode active material layer formed on the positive electrode current collector may be provided. The positive electrode active material layer may include a positive electrode active material according to various embodiments of the present invention. Therefore, since the content about the positive electrode active material is the same as the above description, the detailed description will be omitted for convenience, and only the remaining components not described above will be described below.
[0123] There is no particular limitation on the positive electrode collector as long as it has conductivity without causing chemical changes in the battery, and examples thereof may include: stainless steel, aluminum, nickel, titanium, sintered carbon, or aluminum or stainless steel whose surface has been treated with carbon, nickel, titanium, silver, etc. In addition, the positive electrode collector may generally have a thickness of 3 μm to 500 μm, or the adhesion of the positive electrode active material may be increased by forming micro-concave and convex on the surface of the collector. For example, various forms such as films, sheets, boxes, nets, porous materials, foams, and non-woven fabrics may be used.
[0124] The positive electrode active material layer may be prepared by coating a positive electrode slurry composition on the positive electrode current collector. The positive electrode slurry composition includes the positive electrode active material and a conductive material, and optionally includes a binder as required.
[0125] At this time, the content of the positive electrode active material may be 80 wt % to 99 wt %, more specifically, 85 wt % to 98.5 wt % relative to the total weight of the positive electrode active material layer. When the content of the positive electrode active material is within the above range, excellent capacity characteristics may be achieved, but the present invention is not necessarily limited thereto.
[0126] The above-mentioned conductive material is used to provide conductivity to the electrode, and can be used without limitation, as long as it has electronic conductivity and does not cause chemical changes in the assembled battery. Specific examples thereof may include: graphite such as natural graphite or artificial graphite; carbon materials such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, thermal black or carbon fiber; metal powder or metal fiber such as copper, nickel, aluminum or silver; conductive whiskers such as zinc oxide whiskers, potassium titanate whiskers; conductive metal oxides such as titanium oxide; or conductive polymers such as polyphenylene derivatives, etc., and these substances can be used as a single one or as a mixture of two or more. The content of the above-mentioned conductive material can be 0.1 wt% to 15 wt% relative to the total weight of the positive electrode active material layer.
[0127] The above-mentioned binder serves to adhere the positive electrode active material particles to each other and improve the adhesion of the positive electrode active material and the collector. Specific examples thereof may include: polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile (polyacrylonitrile), carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinyl pyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene monomer (EPDM), sulfonated EPDM, styrene-butadiene rubber (SBR), fluororubber or its various copolymers, etc., and these substances can be used as a single or as a mixture of two or more. Relative to the total weight of the positive electrode active material layer, the content of the above-mentioned binder can be 0.1% by weight to 15% by weight.
[0128] In addition to using the above-mentioned positive electrode active material, the above-mentioned positive electrode can be prepared using a common positive electrode preparation method. Specifically, the above-mentioned positive electrode can be prepared by coating a positive electrode slurry composition prepared by dissolving or dispersing the above-mentioned positive electrode active material and a selective binder and a conductive material in a solvent onto a positive electrode collector, and then drying and rolling the obtained product.
[0129] The above-mentioned solvent may be a solvent commonly used in the art, and may include dimethyl sulfoxide (DMSO), isopropyl alcohol, N-methylpyrrolidone (NMP), acetone, water, etc., and these substances may be used alone as a substance, or as a mixture of two or more. Considering the coating thickness and preparation yield of the slurry, as long as the above-mentioned solvent can dissolve or disperse the above-mentioned positive electrode active material, conductive material and binder and has a viscosity sufficient to obtain excellent thickness uniformity when it is used to prepare the positive electrode coating thereafter, the amount of the solvent used is sufficient.
[0130] Furthermore, in another embodiment, the positive electrode may be prepared by casting the positive electrode slurry composition on a separate support, and then laminating a film obtained by peeling off the support on a positive electrode collector.
[0131] In addition, according to another aspect of the present invention, an electrochemical device including the positive electrode may be provided. The electrochemical device may be specifically a battery, a capacitor, etc., and more specifically, may be a lithium secondary battery.
[0132] Specifically, the lithium secondary battery may include a positive electrode, a negative electrode positioned opposite to the positive electrode, and a separator and an electrolyte between the positive electrode and the negative electrode. Since the positive electrode is the same as the positive electrode described above, a detailed description will be omitted for convenience, and only the remaining components not described above will be described in detail below.
[0133] The lithium secondary battery may further include, optionally, a battery container that accommodates the electrode assembly of the positive electrode, the negative electrode, and the separator, and a sealing member that seals the battery container.
[0134] The negative electrode may include a negative electrode current collector and a negative electrode active material layer located on the negative electrode current collector.
[0135] There is no particular limitation on the negative electrode collector as long as it has high conductivity and does not cause chemical changes in the battery, and examples thereof may include: copper, stainless steel, aluminum, nickel, titanium, sintered carbon, or copper or stainless steel, aluminum-cadmium alloy, etc., whose surfaces are treated with carbon, nickel, titanium, silver, etc. In addition, the negative electrode collector may generally have a thickness of 3 μm to 500 μm, or may increase the binding force of the negative electrode active material by forming tiny concave-convex shapes on the surface of the collector, as with the positive electrode collector. For example, various forms such as films, sheets, boxes, nets, porous materials, foams, and non-woven fabrics may be used.
[0136] The negative electrode active material layer may be prepared by coating a negative electrode slurry composition on the negative electrode current collector. The negative electrode slurry composition includes the negative electrode active material and a conductive material, and optionally includes a binder as required.
[0137] The above-mentioned negative electrode active material can use a compound that can reversibly intercalate and deintercalate lithium. Specific examples thereof may include: carbon materials such as artificial graphite, natural graphite, graphitized carbon fiber and amorphous carbon; metal compounds that can be alloyed with lithium such as Si, Al, Sn, Pb, Zn, Bi, In, Mg, Ga, Cd, Si alloy, Sn alloy or Al alloy; metal oxides that can be doped and dedoped with lithium such as SiO β (0<β<2), SnO2, vanadium oxide and lithium vanadium oxide; or a composite comprising a metal compound and a carbon material such as a Si-C composite or a Sn-C composite, and any one of these substances or a mixture of two or more thereof can be used. In addition, a metallic lithium film can be used as the above-mentioned negative electrode active material. In addition, the carbon material can use both low-crystalline carbon and high-crystalline carbon. Low-crystalline carbon generally includes soft carbon and hard carbon, and high-crystalline carbon generally includes: amorphous, plate-like, scaly, spherical or fibrous natural graphite or artificial graphite, and high-temperature sintered carbon such as floating graphite (Kish graphite), pyrolytic carbon (pyrolytic carbon), mesophase pitch carbon fiber (mesophase pitch based carbon fiber), mesophase carbon microbeads (meso-carbon microbeads), mesophase pitch (Mesophase pitches) and petroleum or coal tar pitch derived coke (petroleum or coal tar pitch derived cokes).
[0138] The negative electrode active material may be included in an amount of 80 wt % to 99 wt % based on the total weight of the negative electrode active material layer.
[0139] The binder is a component that helps to bind the conductive material, the active material and the current collector, and its content is generally 0.1 wt % to 10 wt % based on the total weight of the negative electrode active material layer. Examples of the binder may include polyvinylidene fluoride (PVDF), polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinyl pyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene terpolymer (EPDM), sulfonated EPDM, styrene-butadiene rubber, nitrile-butadiene rubber, fluororubber and various copolymers thereof.
[0140] The above conductive material is a component for further improving the conductivity of the negative electrode active material, and the content of the conductive material can be 10% by weight or less, preferably 5% by weight or less, based on the total weight of the negative electrode active material layer. The above conductive material is not subject to any restrictions as long as it has conductivity and does not cause chemical changes in the battery, and conductive materials such as graphite such as natural graphite or artificial graphite; carbon black such as acetylene black, Ketjen black, channel black, furnace black, lamp black or thermal black can be used; conductive fibers such as carbon fibers or metal fibers; metal powders such as fluorocarbons, aluminum or nickel powders; conductive whiskers such as zinc oxide or potassium titanate; conductive metal oxides such as titanium oxide; and polyphenylene derivatives.
[0141] In one embodiment, the negative electrode active material layer can be prepared by: coating a negative electrode slurry composition prepared by dissolving or dispersing a negative electrode active material and a selective binder and a conductive material in a solvent on a negative electrode collector and drying the obtained product; or by casting the negative electrode slurry composition on a separate carrier and then laminating a film obtained by peeling off the carrier on the negative electrode collector.
[0142] On the other hand, in the above-mentioned lithium secondary battery, the separator separates the negative electrode and the positive electrode, and provides a migration channel for lithium ions, and there is no particular limitation, as long as it is generally used as a separator in a lithium secondary battery. In particular, a separator with low resistance to electrolyte ion migration and excellent ability to contain electrolyte liquid moisture is preferred. Specifically, it is possible to use: a porous polymer film, for example, a porous polymer film prepared from a polyolefin polymer such as an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer, and an ethylene / methacrylate copolymer; or a laminated structure of more than two layers thereof. In addition, commonly used porous non-woven fabrics such as non-woven fabrics made of high melting point glass fibers or polyethylene terephthalate fibers can be used. In addition, in order to ensure heat resistance and mechanical strength, a coated separator comprising a ceramic component or a polymer material can also be used, and can be selectively used in a single-layer or multilayer structure.
[0143] In addition, the electrolyte used in the present invention may include organic liquid electrolytes, inorganic liquid electrolytes, solid polymer electrolytes, gel polymer electrolytes, solid inorganic electrolytes, molten inorganic electrolytes, etc. that can be used in the preparation of lithium secondary batteries, but the present invention is not limited thereto.
[0144] Specifically, the electrolyte may include an organic solvent and a lithium salt.
[0145] The above-mentioned organic solvent can be used without particular limitation as long as it can function as a medium through which ions participating in the electrochemical reaction of the battery can migrate. Specific examples of the above-mentioned organic solvents may include: ester solvents such as methyl acetate, ethyl acetate, γ-butyrolactone or ε-caprolactone; ether solvents such as dibutyl ether or tetrahydrofuran; ketone solvents such as cyclohexanone; aromatic hydrocarbon solvents such as benzene or fluorobenzene; carbonate solvents such as dimethyl carbonate (DMC), diethyl carbonate (DEC), methylethyl carbonate (MEC), ethylmethyl carbonate (EMC), ethylene carbonate (EC) or propylene carbonate (PC); alcohol solvents such as ethanol or isopropanol; nitrile solvents such as R-CN (R is C2~C 20 Straight chain, branched or cyclic hydrocarbon group, and may contain double bond aromatic ring or ether bond); amide such as dimethylformamide; dioxolane such as 1,3-dioxolane; sulfolane, etc. Among them, carbonate solvents are preferred, and a mixture of cyclic carbonates (such as ethylene carbonate, propylene carbonate, etc.) with high ion conductivity and high dielectric constant that can enhance the charging and discharging performance of the battery and low viscosity linear carbonate compounds (such as ethyl methyl carbonate, dimethyl carbonate, diethyl carbonate, etc.) is more preferred. In this case, mixing cyclic carbonates and chain carbonates in a volume ratio of about 1:1 to 1:9 can produce excellent electrolyte performance.
[0146] The above-mentioned lithium salt can be used without particular limitation, as long as it is a compound capable of providing lithium ions in a lithium secondary battery. Specific examples of the above-mentioned lithium salts may include LiPF6, LiClO4, LiAsF6, LiBF4, LiSbF6, LiAlO4, LiAlCl4, LiCF3SO3, LiC4F9SO3, LiN(C2F5SO3)2, LiN(C2F5SO2)2, LiN(CF3SO2)2, LiCl, LiI, LiB(C2O4)2, etc. Preferably, the lithium salt can be used in a concentration range of 0.1M to 2.0M. When the lithium salt concentration is included in the above range, the electrolyte has appropriate conductivity and viscosity, thereby being able to exhibit excellent electrolyte performance, and lithium ions can be effectively migrated.
[0147] In the above electrolyte, in order to increase the battery life property, inhibit the decline of battery capacity, improve the battery discharge capacity, etc., in addition to the above electrolyte forming components, one or more additives may be further included, including, for example: halogenated alkylene carbonate compounds such as difluoroethylene carbonate, pyridine, triethyl phosphite, triethanolamine, cyclic ether, ethylenediamine, n-glyme, hexaphosphoric acid triamide, nitrobenzene derivatives, sulfur, quinone imine dyes, N-substituted oxazolidinone, N, N-substituted imidazolidine, ethylene glycol dialkyl ether, ammonium salt, pyrrole, 2-methoxyethanol or aluminum chloride. Wherein, relative to the total weight of the electrolyte, the content of the above additives can be 0.1% by weight to 5% by weight.
[0148] The lithium secondary battery containing the positive electrode active material according to the present invention as described above stably exhibits excellent discharge capacity, output characteristics and life characteristics, and is therefore used in the following fields: the field of portable devices such as mobile phones, laptop computers and digital cameras; and the field of electric vehicles such as hybrid electric vehicles (HEV) and the like.
[0149] The shape of the lithium secondary battery according to the present invention is not particularly limited, but may have a cylindrical, angular, pouch or coin shape using a can. And, preferably, the lithium secondary battery can be used as a battery cell for a power source of a small device, and can also be used as a unit battery of a medium and large battery module including a plurality of battery cells.
[0150] According to still another aspect of the present invention, a battery module including the above-mentioned lithium secondary battery as a unit battery and / or a battery pack including the same may be provided.
[0151] The battery module or the battery pack may be used in power tools (Power Tool); electric vehicles including electric vehicles (EV), hybrid vehicles and plug-in hybrid electric vehicles (PHEV); or as a power source for one or more medium and large devices in a system for storing electricity.
[0152] Hereinafter, the present invention will be described in more detail with reference to Examples. However, it should be understood that these Examples are for illustrative purposes only and should not be construed as limiting the scope of the present invention.
[0153] Preparation Example 1. Preparation of positive electrode active material
[0154] Example 1
[0155] After adding 20 liters of distilled water and 1 kg of ammonia to a batch reactor (90 L batch reactor), N2 gas was introduced into the reactor at a rate of 1.5 liters / minute, the reactor temperature was maintained at 45°C, and stirring was performed at 350 rpm. As a nucleation aqueous solution, 53 g of a 2.5 M aqueous solution prepared by mixing nickel sulfate, cobalt sulfate, and manganese sulfate in a molar ratio of 95:3.5:1.5 was added.
[0156] The 2.5M aqueous solution for nucleation prepared above was continuously added at a rate of 2.4 liters / hour, and 28% aqueous ammonia was continuously added at a rate of 0.3 liters / hour. In addition, the amount of 25% sodium hydroxide solution added was adjusted so that the pH value in the reactor was maintained at 11 to 12, and the reaction was continued. At this time, the stirring speed was adjusted to 350 rpm.
[0157] As an aqueous solution for shell formation, a 2.5 M concentration aqueous solution for shell formation was prepared by mixing nickel sulfate, cobalt sulfate and manganese sulfate in a molar ratio of 54:44.5:1.5. The prepared aqueous solution for shell formation was added to the above-mentioned batch reactor (90L batch reactor) at a rate of 2.4 L / hour, 28% ammonia water was added at a rate of 0.3 L / hour, and 25% sodium hydroxide solution was also added to make the pH value become 11 to 12.
[0158] After the nucleation and shell formation reactions were completed, a crystallization reaction was induced by increasing the internal pH of the batch reactor.
[0159] After the crystallization reaction was completed, a spherical metal composite hydroxide precipitate was obtained from the batch reactor. The metal composite hydroxide was filtered, washed with water, and then dried in a hot air dryer at 110° C. for 12 hours.
[0160] The dried metal composite hydroxide was mixed with LiOH (Li / (Ni+Co+Mn) molar ratio = 1.06), and then heated to 690°C at 2°C per minute in a sintering furnace while maintaining an O2 atmosphere. The mixture was heat treated (first heat treatment) for 10 hours to obtain a lithium composite oxide.
[0161] Next, Al2O3, TiO2 and ZrO2 were mixed with the lithium composite oxide, and the temperature was raised to 680°C at a rate of 2°C per minute while maintaining an O2 atmosphere, and then an additional heat treatment (second heat treatment) was performed for 10 hours. At this time, the Al2O3 was weighed so that the Al content in the mixture was 1600ppm, the TiO2 was weighed so that the Ti content in the mixture was 1600ppm, and the ZrO2 content was weighed so that the Zr content in the mixture was 500ppm.
[0162] After that, distilled water was added to the lithium composite oxide and washed for 1 hour, and the washed lithium composite oxide was filtered and dried to obtain a positive electrode active material. The average particle size D50 of the lithium composite oxide contained in the positive electrode active material was measured to be 16.5 μm.
[0163] Example 2
[0164] The positive electrode active material was prepared in the same manner as in Example 1 except that H3BO3 was mixed with the above-mentioned lithium composite oxide, the temperature was raised to 300°C at a rate of 2°C per minute while maintaining the O2 atmosphere, and then an additional heat treatment (third heat treatment) was performed for 8 hours. At this time, H3BO3 was weighed so that the content of B in the mixture was 400 ppm. The average particle size D50 of the above-mentioned lithium composite oxide contained in the above-mentioned positive electrode active material was measured to be 16.5 μm.
[0165] Example 3
[0166] A positive electrode active material was prepared in the same manner as in Example 1 except that a nucleation aqueous solution in which nickel sulfate, cobalt sulfate, and manganese sulfate were mixed at a molar ratio of 97:3:0 was used and a shelling aqueous solution in which nickel sulfate, cobalt sulfate, and manganese sulfate were mixed at a molar ratio of 40:50:10 was used. The average particle size D50 of the lithium composite oxide contained in the positive electrode active material was measured to be 16.5 μm.
[0167] Example 4
[0168] A positive electrode active material was prepared in the same manner as in Example 1, except that a nucleation aqueous solution in which nickel sulfate, cobalt sulfate and manganese sulfate were mixed at a molar ratio of 90:10:0 was used and a shelling aqueous solution in which the molar ratio of nickel sulfate, cobalt sulfate and manganese sulfate was changed from 65:15:20 to 40:20:40 by changing the concentration was used, the temperature was raised to 800° C. for 10 hours at a rate of 2° C. per minute in the first heat treatment, and the temperature was raised to 720° C. for 10 hours at a rate of 2° C. per minute in the second heat treatment. The average particle size D50 of the lithium composite oxide contained in the positive electrode active material was measured to be 13.0 μm.
[0169] Example 5
[0170] After adding 20 liters of distilled water and 1 kg of ammonia to a batch reactor (90 L batch reactor), N2 gas was introduced into the reactor at a rate of 1.5 liters / minute, the reactor temperature was maintained at 45°C, and stirring was performed at 350 rpm. 80 g of a 2.5 M aqueous solution of nickel sulfate, cobalt sulfate, and manganese sulfate mixed in a molar ratio of 80:10:10 was added.
[0171] The 2.5M aqueous precursor solution prepared above was continuously added to the reactor at a rate of 2.4 liters / hour, and 28% aqueous ammonia was continuously added at a rate of 0.3 liters / hour. In addition, the amount of 25% sodium hydroxide solution added was adjusted so that the pH value in the reactor was maintained at 11 to 12, and the reaction was continued. At this time, the stirring speed was adjusted to 350 rpm.
[0172] After the reaction was completed, the internal pH of the batch reactor was increased to perform a crystallization reaction, thereby obtaining a spherical metal composite hydroxide precipitate. The metal composite hydroxide was filtered, washed with water, and then dried in a hot air dryer at 110° C. for 12 hours.
[0173] The dried metal composite hydroxide was mixed with LiOH (Li / (Ni+Co+Mn) molar ratio = 1.06), and then heated to 800°C at 2°C per minute in a sintering furnace for 10 hours while maintaining an O2 atmosphere to obtain a lithium composite oxide.
[0174] After that, distilled water was added to the lithium composite oxide and washed for 1 hour, and the washed lithium composite oxide was filtered and dried to obtain a positive electrode active material. The average particle size D50 of the lithium composite oxide contained in the positive electrode active material was measured to be 13.0 μm.
[0175] Example 6
[0176] In addition to using a precursor aqueous solution of nickel sulfate, cobalt sulfate, and manganese sulfate mixed in a molar ratio of 92:8.0:0.0 to prepare Ni 0.92 Co 0.08 The positive electrode active material was prepared in the same manner as in Example 5 except that LiOH and 1.4 mol % Al(OH)3 were mixed with the lithium composite oxide as a metal composite hydroxide precursor of (OH)2, and the temperature was raised to 650°C at a rate of 2°C per minute in a sintering furnace maintaining an O2 atmosphere, and heat-treated for 10 hours to obtain the lithium composite oxide. The average particle size D50 of the lithium composite oxide contained in the positive electrode active material was measured to be 14.0 μm.
[0177] Comparative Example 1
[0178] A positive electrode active material was prepared in the same manner as in Example 1, except that the internal pH of the batch reactor was not increased to induce a crystallization reaction after the nucleation and shelling reactions were completed.
[0179] Comparative Example 2
[0180] A positive electrode active material was prepared in the same manner as in Example 3 except that the internal pH of the batch reactor was not increased to induce a crystallization reaction after the nucleation and shelling reactions were completed.
[0181] Comparative Example 3
[0182] A positive electrode active material was prepared in the same manner as in Example 4 except that the internal pH of the batch reactor was not increased to induce a crystallization reaction after the nucleation and shelling reactions were completed.
[0183] Comparative Example 4
[0184] A positive electrode active material was prepared in the same manner as in Example 5, except that the internal pH of the batch reactor was not increased to induce a crystallization reaction after the nucleation and shelling reactions were completed.
[0185] Comparative Example 5
[0186] A positive electrode active material was prepared in the same manner as in Example 6, except that the internal pH of the batch reactor was not increased to induce a crystallization reaction after the nucleation and shelling reactions were completed.
[0187] Preparation Example 2. Preparation of lithium secondary battery
[0188] A positive electrode slurry was prepared by dispersing 94 wt % of the positive electrode active material prepared according to Preparation Example 1, 3 wt % of artificial carbon black and 3 wt % of PVDF binder in 3.5 g of N-methyl-2-pyrrolidone (NMP). The positive electrode slurry was uniformly coated on an aluminum film having a thickness of 20 μm as a positive electrode collector and dried, and roll-pressed to prepare a positive electrode. The loading level of the positive electrode was 7 mg / cm 2 , the electrode density is 3.2g / cm 3 .
[0189] A button cell was prepared according to a conventional preparation procedure using lithium foil as the counter electrode of the positive electrode, a porous polyethylene film (Celgard 2300, thickness: 25 μm) as an isolation film, and a liquid electrolyte containing LiPF6 at a concentration of 1.15 M in a solvent prepared by mixing ethylene carbonate and ethyl methyl carbonate in a volume ratio of 3:7.
[0190] Experimental Example 1. SEM / EDX Analysis of Metal Composite Hydroxides and Positive Electrode Active Materials
[0191] Figure 1 is a cross-sectional SEM image obtained after cross-sectional processing of the lithium composite oxide contained in the positive electrode active material according to Example 2 using FIB (gallium ion source), Figure 2 To show that through Figure 1 A graph (line sum spectrum) showing the contents of metal elements (Ni, Co, Mn) present in a direction from the outermost surface toward the center of the lithium composite oxide confirmed by EDX analysis of a cross-sectional SEM image.
[0192] Figure 3 is a cross-sectional SEM image obtained after cross-sectional processing of the lithium composite oxide contained in the positive electrode active material according to Comparative Example 1 using FIB (gallium ion source), Figure 4 To show that through Figure 3 A graph (line and spectrum) showing the contents of metal elements (Ni, Co, Mn) in a direction from the outermost surface toward the center of the lithium composite oxide confirmed by EDX analysis of a cross-sectional SEM image.
[0193] Reference Figure 2 It can be confirmed that at least one metal element in the lithium composite oxide contained in the above-mentioned positive electrode active material presents a concentration gradient including a first concentration gradient interval with a (+) slope from the outermost surface of the above-mentioned lithium composite oxide toward the center and a second concentration gradient interval with a (-) slope.
[0194] More specifically, it can be confirmed that the first concentration gradient interval exists from the outermost surface of the lithium composite oxide to a predetermined depth (about 0.1 μm from the outermost surface), the second concentration gradient interval is located inside the first concentration gradient interval, and the second concentration gradient interval is located from the outermost surface of the lithium composite oxide to a depth of 1 μm (about 0.1 μm from the outermost surface). Figure 2 As a reference, at a depth of about 0.5 μm, the first concentration gradient interval and the second concentration gradient interval exist.
[0195] Furthermore, it can be confirmed that within the first concentration gradient interval, the concentration of nickel in the lithium composite oxide decreases from the surface portion toward the center portion of the lithium composite oxide, while the concentrations of cobalt and manganese increase, and within the second concentration gradient interval, the concentration of nickel in the lithium composite oxide increases from the surface portion toward the center portion of the lithium composite oxide, while the concentrations of cobalt and manganese decrease.
[0196] It can be confirmed that there is a concentration retention zone (roughly from the outermost surface of the lithium composite oxide at a depth of 0.5 μm to the center of the lithium composite oxide) in which the concentration of at least one metal element in the lithium composite oxide is maintained inside the second concentration gradient zone (i.e., a position deeper from the second concentration gradient zone toward the center). The absolute value of the concentration change rate of nickel, cobalt and / or manganese in the concentration retention zone is 5.0 mol% or less.
[0197] On the other hand, referring to the line and spectrum of the positive electrode active material according to Comparative Example 1 Figure 4 , and Figure 2 Unlike the graph shown, the first concentration gradient region and the second concentration gradient region that are clearly distinguished do not appear from the outermost surface of the lithium composite oxide to a predetermined depth.
[0198] Furthermore, no line sum spectra of the positive electrode active materials according to Comparative Examples 2 to 5 can be observed. Figure 2 The concentration gradient pattern is shown in FIG.
[0199] Figure 5 Graph (line and spectrum) showing the contents of metal elements (Ni, Co, Mn) present in the direction from the outermost surface toward the center of the lithium composite oxide as confirmed by EDX analysis of the cross-sectional SEM image of Example 3.
[0200] Figure 6 Graph (line and spectrum) showing the contents of metal elements (Ni, Co, Mn) present in the direction from the outermost surface toward the center of the lithium composite oxide as confirmed by EDX analysis of the cross-sectional SEM image of Example 4.
[0201] Figure 7Graph (line and spectrum) showing the contents of metal elements (Ni, Co, Mn) present in the direction from the outermost surface toward the center of the lithium composite oxide as confirmed by EDX analysis of the cross-sectional SEM image of Example 5.
[0202] Figure 8 Graph (line and spectrum) showing the contents of metal elements (Ni, Co, Mn) present in the direction from the outermost surface toward the center of the lithium composite oxide as confirmed by EDX analysis of the cross-sectional SEM image of Example 6.
[0203] Reference Figures 5 to 8 It can be confirmed that Figure 2 Similarly to the concentration gradient pattern shown in FIG. 1 , the first concentration gradient interval exists from the outermost surface of the lithium composite oxide to a predetermined depth (roughly from the outermost surface to a depth of 0.1 μm), and the second concentration gradient interval is located inside the first concentration gradient interval, from the outermost surface of the lithium composite oxide to a depth of 1 μm (roughly from the outermost surface to a depth of 0.1 μm). Figure 5 As the reference, at a depth of about 0.5 μm, Figure 6 As the reference, at a depth of about 0.4 μm, Figure 7 As the reference, at a depth of about 0.2 μm, Figure 8 The first concentration gradient interval and the second concentration gradient interval exist at a depth of about 0.2 μm as a reference.
[0204] Similarly, it can be confirmed that within the first concentration gradient interval, the concentration of nickel in the lithium composite oxide decreases from the surface portion toward the center portion of the lithium composite oxide, while the concentrations of cobalt and manganese increase, and that within the second concentration gradient interval, the concentration of nickel in the lithium composite oxide increases from the surface portion toward the center portion of the lithium composite oxide, while the concentrations of cobalt and manganese decrease.
[0205] It can be confirmed that there is a concentration retention zone in which the concentration of at least one metal element in the lithium composite oxide is maintained inside the second concentration gradient zone (i.e., a position deeper from the second concentration gradient zone toward the center). The absolute value of the concentration change rate of nickel, cobalt and / or manganese in the concentration retention zone is 5.0 mol% or less.
[0206] Experimental Example 2. XPS analysis of positive electrode active materials
[0207] XPS analysis was performed on the positive electrode active material prepared according to Preparation Example 1 to confirm whether there was a coating on the surface of the lithium composite oxide. XPS analysis was performed by using K-Alpha+ (ThermoFisher Scientific) (accelerating voltage: 0.5keV to 2keV, energy resolution: about 0.5eV, minimum analysis area: 30micro, monatomic and gas cluster ion source). The above XPS analysis results are shown in Table 1 below.
[0208] Table 1
[0209] Classification Al2P B1s C1s Co2p Li1s Mn2p Ni2p O1s Ti2p ZlUT Example 1 2.35 0.00 33.11 0.75 17.45 1.53 4.34 37.92 2.21 0.34 Example 2 1.47 3.51 34.26 0.69 20.33 1.41 3.13 32.95 1.97 0.28 Example 3 2.86 0.00 20.57 1.05 18.18 4.17 7.00 43.24 2.72 0.21 Example 4 2.62 0.00 20.67 0.96 17.04 4.12 8.08 43.44 2.69 0.38 Example 5 0.00 0.00 40.6 2.98 10.85 3.13 7.72 34.72 0.00 0.00 Example 6 2.03 0.00 34.59 1.93 6.52 0.00 15.36 39.57 0.00 0.00 Comparative Example 1 2.45 0.00 32.88 1.11 18.66 1.50 3.14 37.92 2.04 0.30 Comparative Example 2 2.87 0.00 22.48 1.32 19.63 4.29 5.97 40.89 2.33 0.22 Comparative Example 3 3.18 0.00 20.32 1.01 16.12 4.19 6.95 45.36 2.55 0.32 Comparative Example 4 0.00 0.00 37.68 2.58 19.78 2.84 5.29 31.83 0.00 0.00 Comparative Example 5 2.17 0.00 34.45 2.18 7.76 0.00 13.26 40.18 0.00 0.00
[0210] Referring to the results in Table 1 above, in the case of the positive electrode active materials according to Examples 1, 3 and 4, specific peaks were detected in Al, Zr and Ti. Based on this, it can be confirmed that in the positive electrode active materials according to Examples 1, 3 and 4, a coating containing Al, Zr and Ti exists on the surface of the lithium composite oxide.
[0211] Furthermore, in the case of the positive electrode active material according to Example 2, specific peaks were detected not only in Al, Zr and Ti, but also in B, thereby confirming that in the positive electrode active material according to Example 2, a coating containing Al, Zr and Ti and a coating containing B are present on the surface of the lithium composite oxide.
[0212] Experimental Example 3. Residual lithium and specific surface area determination of positive electrode active material
[0213] The residual lithium was determined by the amount of 0.1M HCl used by pH titration until pH 4. First, 5 g of the positive electrode active material was added to 100 ml of DIW, stirred for 15 minutes, and then filtered. Next, 50 ml of the filtrate was taken, 0.1M HCl was added, and the HCl consumption according to the pH value was measured to determine Q1 and Q2, and the residual LiOH and Li2CO3 were calculated according to the following calculation formula.
[0214] M1=23.94(LiOH molecular weight)
[0215] M2=73.89(Li2CO3 molecular weight)
[0216] LiOH (ppm) = ((Q1-Q2) × M1 × HCl con. × DIW (g)) / (solution (g) × powder (g)) × 10,000
[0217] Li2CO3(ppm)=(2×Q2×M2 / 2×HCl con.×DIW(g)) / (solution
[0218] Liquid (g) × Powder (g)) × 10,000
[0219] The BET specific surface area is calculated from the amount of nitrogen adsorbed at liquid nitrogen temperature (77 K) using a gas adsorption specific surface area measuring apparatus (BELSORP-mini II manufactured by Microtarac BEL).
[0220] The above-mentioned residual lithium and BET specific surface area measurement results are shown in Table 2 below.
[0221] Table 2
[0222]
[0223]
[0224] Referring to the results in Table 2, it can be confirmed that the positive electrode active materials according to Examples 1 and 3 to 6 have reduced residual lithium content and BET specific surface area compared with the corresponding positive electrode active materials according to Comparative Examples 1 to 5, respectively.
[0225] That is, it was confirmed that the residual lithium and the BET specific surface area of the cathode active material as the final product were reduced by an additional step of increasing the internal pH of the batch reactor to induce a crystallization reaction.
[0226] Experimental Example 4. Evaluation of capacity and life characteristics of lithium secondary batteries
[0227] The lithium secondary battery (button cell) prepared according to Preparation Example 2 was subjected to a charge / discharge test at 25° C. in the voltage range of 3.0 V to 4.3 V at a discharge rate of 0.1 C using an electrochemical analyzer (Toyo, Toscat-3100) to measure the charge capacity and discharge capacity.
[0228] Furthermore, the same lithium secondary battery was charged / discharged 50 times at 1C / 1C in the driving voltage range of 3.0V to 4.4V at 25°C, and then the ratio of the discharge capacity at the 50th cycle to the initial capacity (cycle capacity retention) was measured.
[0229] The above measurement results are shown in Table 3 below.
[0230] Table 3
[0231]
[0232] Referring to the results of Table 3 above, it can be confirmed that the positive electrode active materials according to Examples 1 and 3 to 6 have improved charge and discharge efficiency and cycle capacity retention rate compared with the corresponding positive electrode active materials according to Comparative Examples 1 to 5, respectively.
[0233] And, it can be confirmed that the positive electrode active material according to Example 2 additionally introduced with the boron-containing coating layer exhibits an improved effect in the cycle capacity retention ratio, compared with the positive electrode active materials according to Examples 1 and 3 to 6.
[0234] Although the embodiments of the present invention are described above, those skilled in the art will understand that various modifications and changes can be made to the present invention by adding, modifying, deleting, increasing, etc., without departing from the scope of the idea of the present invention as described in the claims, and these also fall within the scope of the rights of the present invention.
Claims
1. A positive electrode active material, in, including lithium composite oxides capable of lithium insertion and extraction, The at least one metal element in the lithium composite oxide presents a concentration gradient including a first concentration gradient zone having a (+) slope from the outermost surface toward the center of the lithium composite oxide and a second concentration gradient zone having a (-) slope toward the inside of the first concentration gradient zone, The first concentration gradient region exists from the outermost surface of the lithium composite oxide to a depth of 0.10 μm.
2. The positive electrode active material according to claim 1, in, When the average diameter of the lithium composite oxide is defined as d, the first concentration gradient region and the second concentration gradient region exist within a depth range of 0.05d to 0.33d from the outermost surface of the lithium composite oxide.
3. The positive electrode active material according to claim 1, in, The first concentration gradient region and the second concentration gradient region exist from the outermost surface of the lithium composite oxide to a depth of 1 μm.
4. The positive electrode active material according to claim 1, in, The first concentration gradient region and the second concentration gradient region exist within a range from the outermost surface of the lithium composite oxide to a depth of 0.50 μm.
5. The positive electrode active material according to claim 1, in, The first concentration gradient section and the second concentration gradient section exist in the bulk particle.
6. The positive electrode active material according to claim 1, in, The lithium composite oxide has a single bulk structure, and the first concentration gradient region and the second concentration gradient region exist in the single bulk structure.
7. The positive electrode active material according to claim 1, in, In the first concentration gradient region, the concentration of nickel in the lithium composite oxide decreases from the surface portion toward the center portion of the lithium composite oxide, and the concentration of cobalt increases. In the second concentration gradient region, the concentration of nickel in the lithium composite oxide increases from the surface portion toward the center portion of the lithium composite oxide, and the concentration of cobalt decreases.
8. The positive electrode active material according to claim 1, in, In the first concentration gradient region, the concentration of at least one selected from manganese and aluminum in the lithium composite oxide increases from the surface toward the center of the lithium composite oxide. In the second concentration gradient region, the concentration of at least one selected from manganese and aluminum in the lithium composite oxide decreases from the surface toward the center of the lithium composite oxide.
9. The positive electrode active material according to claim 1, in, The positive electrode active material has a concentration retention zone, the concentration retention zone is located inside the second concentration gradient zone, and retains the concentration of at least one metal element in the lithium composite oxide from the surface portion toward the center portion of the lithium composite oxide.
10. The positive electrode active material according to claim 9, in, The absolute value of the concentration change rate of at least one metal element in the concentration maintaining range is 5 mol % or less.
11. The positive electrode active material according to claim 9, in, The concentration of nickel in the lithium composite oxide in the concentration maintaining range is higher than that in the first concentration gradient range and the second concentration gradient range.
12. The positive electrode active material according to claim 9, in, The concentration of at least one selected from cobalt, manganese, and aluminum in the lithium composite oxide is greater in the first concentration gradient range and the second concentration gradient range than in the concentration maintaining range.
13. The positive electrode active material according to claim 1, in, The lithium composite oxide is represented by the following chemical formula 1: Li w Ni 1-(x+y+z) Co x M1 y M2 z O 2+δ in, M1 is at least one selected from Mn or Al, M2 is at least one selected from P, Sr, Ba, B, Ti, Zr, Mn, Al, W, Ce, Hf, Ta, F, Mg, Cr, V, Fe, Zn, Si, Y, Ga, Sn, Mo, Ge, Nd, Gd and Cu, M1 and M2 are different elements. 0.5≤w≤1.5, 0≤x≤0.50, 0≤y≤0.20, 0≤z≤0.20, 0≤δ≤0.
02.
14. The positive electrode active material according to claim 1, in, The lithium composite oxide contains nickel at a concentration of 80 mol % or more in all elements other than lithium.
15. The positive electrode active material according to claim 1, in, The above-mentioned lithium composite oxide has a core-shell structure. In the above-mentioned core-shell structure, the above-mentioned first concentration gradient interval exists in the above-mentioned shell and the above-mentioned second concentration gradient interval exists in the above-mentioned core, or the above-mentioned first concentration gradient interval and the above-mentioned second concentration gradient interval exist in the above-mentioned core, or the above-mentioned first concentration gradient interval and the above-mentioned second concentration gradient interval exist in the above-mentioned shell.