Positive electrode active material for sodium ion secondary battery
By adding Co components and amorphous phase to the positive electrode active substance of the sodium ion secondary battery, the problems of low discharge voltage and insufficient capacity in the prior art are solved, and a high voltage and high capacity sodium ion secondary battery is realized. Improves charge and discharge characteristics and cycle characteristics, and enhances the stability of the battery.
Patent Information
- Application Number
- CN202411332839.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2017-06-27
- Filing Date
- 2018-06-12
- Publication Date
- 2024-11-12
AI Technical Summary
The existing positive electrode active substances for sodium ion secondary batteries have problems such as low discharge voltage and insufficient discharge capacity, especially the discharge voltage of Na2FeP2O7 crystallization is as low as about 2.9V, and the discharge capacity of Na4Ni3(PO4)2(P2O7) crystallization is low.
The positive electrode active material containing a specific composition of Co components is used, and the specific components include 8 to 55% Na2O, 10 to 70% CoO, 0 to 60% CrO+FeO+MnO+NiO, 15 to 70% P2O5+SiO2 +B2O3 and contains an amorphous phase to increase discharge capacity and voltage.
A high voltage and high capacity sodium ion secondary battery is realized, which improves the charge and discharge characteristics and cycle characteristics. Through the existence of amorphous phase, a dense sintered body is formed, which enhances the interface ions between the positive electrode active material and the solid electrolyte. The conduction path inhibits the decomposition of the electrolyte.
Smart Images

Figure CN118943362A_ABST
Abstract
Description
[0001] (This application is a divisional application of application No. 201880025212.1, filed on June 12, 2018, entitled “POSITIVE ELECTRODE ACTIVE MATERIAL FOR SODIUM ION SECONDARY BATTERY”) Technical Field
[0002] The present invention relates to a positive electrode active material for a sodium ion battery used in portable electronic devices, electric vehicles and the like. Background Art
[0003] Lithium-ion secondary batteries have established their position as high-capacity and lightweight power sources that are indispensable for portable electronic terminals or electric vehicles, and as their positive electrode active materials, active materials containing olivine-type crystals represented by the general formula LiFePO4 have attracted much attention. However, due to concerns about the rising prices of raw materials for lithium worldwide, research has been conducted in recent years on sodium-ion secondary batteries that use sodium, such as Na2FeP2O7 crystals and Na4Ni3(PO4)2(P2O7) crystals, as substitutes for lithium (for example, see Patent Documents 1 and 2).
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: Japanese Patent No. 5673836
[0007] Patent Document 2: Japanese Patent Application Publication No. 2016-25067 Summary of the invention
[0008] Technical problem to be solved by the invention
[0009] The positive electrode active material for sodium ion secondary batteries containing Na2FeP2O7 crystals has a technical problem of low discharge voltage of about 2.9 V. The positive electrode active material for sodium ion secondary batteries containing Na4Ni3(PO4)2(P2O7) crystals has a technical problem of low discharge capacity despite relatively high discharge voltage.
[0010] In view of the above circumstances, an object of the present invention is to provide a novel positive electrode active material for a sodium ion secondary battery having high voltage and high capacity.
[0011] Technical solutions for solving technical problems
[0012] As a result of intensive studies, the inventors of the present invention have found that the above-mentioned technical problems can be solved by a positive electrode active material having a specific composition containing a Co component, and have proposed a solution as the present invention.
[0013] That is, the positive electrode active material for sodium ion secondary battery of the present invention is characterized in that: in terms of mole % converted into oxides, it contains 8 to 55% of Na2O, 10 to 70% of CoO, 0 to 60% of CrO+FeO+MnO+NiO, 15 to 70% of P2O5+SiO2+B2O3, and contains an amorphous phase. In addition, in this specification, "○+○+···" refers to the total amount of the corresponding components.
[0014] During charge and discharge, the valence of Co ions changes, causing a redox reaction, thereby playing a role as a driving force for the absorption and release of sodium ions. Therefore, by containing CoO as an essential component in a predetermined amount as described above, the discharge capacity can be improved.
[0015] In addition, the positive electrode active material for the sodium ion secondary battery of the present invention is characterized by containing an amorphous phase, whereby the diffusion path of the sodium ions is three-dimensionally expanded, so that the insertion and separation of the sodium ions accompanying the charge and discharge becomes easy, and high capacity can be achieved. In addition, the rapid charge and discharge characteristics or the cycle characteristics are easily improved. In addition, when used as a positive electrode active material for a solid sodium ion secondary battery, the amorphous phase softens and flows during firing to weld the positive electrode active material and the sodium ion conductive solid electrolyte, so it is easy to become a dense sintered body. Therefore, an ion conduction path is easily formed at the interface between the positive electrode active material and the solid electrolyte. In addition, if the positive electrode active material contains amorphous, it is also easy to suppress the decomposition of the electrolyte caused by the positive electrode active material.
[0016] The positive electrode active material for the sodium ion secondary battery of the present invention may contain a general formula of Na x (Co 1-a M a )A y O z (M is at least one selected from Cr, Fe, Mn and Ni, A is at least one selected from P, Si and B, 0.5≤x≤4.1, 0.65≤y≤6.5, 2.5≤z≤20, 0≤a≤0.9) The crystal structure is shown in Figure 1. If so, the redox potential accompanying charge and discharge is easily maintained at a high potential and stable, and the energy density is easily improved.
[0017] The positive electrode active material for a sodium ion secondary battery of the present invention preferably has at least one crystal structure selected from the group consisting of monoclinic, triclinic, orthorhombic and tetragonal.
[0018] The positive electrode active material for a sodium ion secondary battery of the present invention preferably has a crystal belonging to at least one space group selected from the group consisting of P-1, P1, Cm, Pna21 and P21 / n.
[0019] The positive electrode material for a sodium ion secondary battery of the present invention is characterized by containing the positive electrode active material for a sodium ion secondary battery described above.
[0020] The positive electrode material for a sodium ion secondary battery of the present invention preferably further contains a conductive auxiliary agent.
[0021] The positive electrode material for a sodium ion secondary battery of the present invention preferably further contains a sodium ion conductive solid electrolyte.
[0022] In the positive electrode material for a sodium ion secondary battery of the present invention, the sodium ion conductive solid electrolyte is preferably β-alumina or a sodium super ion conductor (NASICON) type crystal.
[0023] The positive electrode material for a sodium ion secondary battery of the present invention preferably contains, by mass%, 30 to 100% of a positive electrode active material for a sodium ion secondary battery, 0 to 20% of a conductive aid, and 0 to 70% of a sodium ion conductive solid electrolyte.
[0024] The positive electrode for a sodium ion secondary battery of the present invention is characterized by using the above-mentioned positive electrode material for a sodium ion secondary battery.
[0025] The sodium ion secondary battery of the present invention is characterized by comprising the above-mentioned positive electrode for sodium ion secondary battery.
[0026] The method for producing a positive electrode active material for a sodium ion secondary battery of the present invention is used to produce the above-mentioned positive electrode active material for a sodium ion secondary battery. The method is characterized in that it includes: a step of melting batches of raw materials to obtain a melt; and a step of obtaining a glass body by cooling the melt.
[0027] The method for producing a positive electrode active material for a sodium ion secondary battery of the present invention preferably further comprises a step of crystallizing the glass body by firing the glass body.
[0028] The method for producing a positive electrode active material for a sodium ion secondary battery of the present invention preferably comprises firing a glass body together with at least one selected from the group consisting of conductive carbon, a conductive carbon source, and a sodium ion conductive solid electrolyte.
[0029] Effects of the Invention
[0030] According to the present invention, a novel positive electrode active material for a sodium ion secondary battery having high voltage and high capacity can be provided. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 This is a diagram showing the XRD spectrum of sample No. 1 of Example.
[0032] Figure 2 This is an initial charge and discharge curve of the solid sodium ion secondary battery using the sample No. 1 of the example. DETAILED DESCRIPTION
[0033] (Positive electrode active material for sodium ion secondary battery)
[0034] The positive electrode active material for sodium ion secondary battery of the present invention is characterized in that it contains 8 to 55% Na2O, 10 to 70% CoO, 0 to 60% CrO+FeO+MnO+NiO, 15 to 70% P2O5+SiO2+B2O3, and contains an amorphous phase, calculated as mole % of oxides. The reasons for limiting each component in this way are described below. In addition, in the following description of the content of each component, "%" means "mole %" unless otherwise specified.
[0035] Na2O becomes the source of sodium ions that move between the positive electrode active material and the negative electrode active material during charge and discharge. The content of Na2O is 8-55%, preferably 15-45%, and particularly preferably 25-35%. If Na2O is too little, the sodium ions involved in absorption and release decrease, so the discharge capacity tends to decrease. On the other hand, if Na2O is too much, heterogeneous crystals such as Na3PO4 that do not participate in charge and discharge are easily precipitated, so the discharge capacity tends to decrease.
[0036] CoO undergoes a redox reaction by changing the valence of Co ions during charge and discharge, and plays a role as a driving force for the occlusion and release of sodium ions. The content of CoO is 10 to 70%, preferably 30 to 45%, and particularly preferably 34 to 41%. If CoO is too little, it is difficult for the redox reaction accompanying charge and discharge to occur, and since the sodium ions occluded and released decrease, there is a tendency for the discharge capacity to decrease. On the other hand, if CoO is too much, there is a tendency for heterogeneous crystals to precipitate and the discharge capacity to decrease.
[0037] CrO, FeO, MnO and NiO are similar to CoO. During charge and discharge, the valence of these transition metal element ions changes and redox reactions occur, thereby playing a role as a driving force for the absorption and release of sodium ions. MnO is preferred because it shows a high redox potential in particular. In addition, FeO has a high structural stabilization during charge and discharge, and the cycle characteristics are easily improved, so it is preferred. The content of CrO+FeO+MnO+NiO is 0-60%, preferably 0.1-50%, 0.5-45%, 1-40%, 3-30%, and particularly preferably 5-20%. If there is too much CrO+FeO+MnO+NiO, heterogeneous crystals of FeO, MnO, NiO, etc. that do not participate in charge and discharge are easily precipitated, so the discharge capacity tends to decrease. In addition, in the case of giving priority to increasing the redox potential, the content of CrO+FeO+MnO+NiO is as small as possible, and it is preferred to increase the content of CoO.
[0038] In addition, the transition metal elements in CrO, FeO, MnO and NiO are preferably low-valent ions in the glass, and are particularly preferably divalent ions. In this case, the redox potential accompanying charge and discharge is high, and the discharge capacity and discharge voltage are likely to increase.
[0039] P2O5, SiO2 and B2O3 form a three-dimensional grid structure, and therefore have the effect of stabilizing the structure of the positive electrode active material. In addition, by containing these components, the content of the amorphous phase can be increased. In particular, P2O5 and SiO2 have excellent ion conductivity, so they are preferred, and P2O5 is most preferred. The content of P2O5+SiO2+B2O3 is 15-70%, preferably 28-40%, and particularly preferably 30-38%. If P2O5+SiO2+B2O3 is too little, there is a tendency for the discharge capacity to decrease easily during repeated charge and discharge. On the other hand, if P2O5+SiO2+B2O3 is too much, heterogeneous crystals such as P2O5 that do not participate in charge and discharge tend to precipitate. In addition, the contents of each component of P2O5, SiO2 and B2O3 are preferably 0-70%, 15-70%, 28-40%, and particularly preferably 30-38%, respectively.
[0040] In addition, Na2O / CoO is 0.2 to 5, preferably 0.3 to 4, and particularly preferably 0.4 to 3. If Na2O / CoO is too small or too large, the discharge capacity tends to decrease. In addition, CoO / (P2O5+SiO2+B2O3) is 0.2 to 4, preferably 0.3 to 3, and particularly preferably 0.4 to 2. If CoO / (P2O5+SiO2+B2O3) is too small or too large, the discharge capacity tends to decrease. Among them, "Na2O / CoO" means the molar ratio of each content of Na2O and CoO. In addition, "CoO / (P2O5+SiO2+B2O3)" means the molar ratio of each content of CoO and P2O5+SiO2+B2O3.
[0041] In addition, in the range that does not impair the effect of the present invention, various components other than the above components can be contained to facilitate vitrification. Such components include MgO, CaO, SrO, BaO, ZnO, CuO, Al2O3, GeO2, Nb2O5, ZrO2, V2O5, and Sb2O5, which are marked as oxides. Al2O3 that acts as a network-forming oxide and / or V2O5 that becomes an active material component are particularly preferred. The content of the above components is 0 to 30% in total, preferably 0.1 to 20%, and particularly preferably 0.5 to 10%.
[0042] The positive electrode active material for a sodium ion secondary battery of the present invention is characterized by containing an amorphous phase, thereby achieving the effects of increased capacity, improved rapid charge and discharge characteristics, and improved cycle characteristics, as described above.
[0043] The positive electrode active material for the sodium ion secondary battery of the present invention may contain the general formula Na x (Co 1-a M a )A y O z (M is at least one selected from Cr, Fe, Mn and Ni, A is at least one selected from P, Si and B, 0.5≤x≤4.1, 0.65≤y≤6.5, 2.5≤z≤20, 0≤a≤0.9) shown in the crystal (working voltage 4~6V (vs.Na / Na + )). In this way, the oxidation-reduction potential accompanying charge and discharge is high and easy to be constant, and the energy density is easy to improve.
[0044] x is preferably in the range of 0.5≤x≤4.1, 0.5≤x≤4, 1.2≤x≤3.5, 1.35≤x≤2.5, and particularly preferably in the range of 1.4≤x≤1.95. If x is too small, the sodium ions involved in occlusion and release decrease, so there is a tendency for the discharge capacity to decrease. On the other hand, if x is too large, heterogeneous crystals such as Na3PO4 that do not participate in charge and discharge precipitate and there is a tendency for the discharge capacity to decrease.
[0045] y is preferably in the range of 0.65≤y≤6.5, 1.1≤y≤4, 1.35≤y≤2, and particularly preferably in the range of 1.4≤y≤1.9. If y is too small, the matrix component including the transition metal element decreases, so there is a tendency for the capacity to be easily reduced during repeated charge and discharge. On the other hand, if y is too large, heterogeneous crystals such as P2O5 that do not participate in charge and discharge are precipitated, and there is a tendency for the capacity to be reduced.
[0046] z is preferably in the range of 2.5≤z≤20, 3.5≤z≤15, 5<z<7, and particularly preferably in the range of 5.7≤z<7. If z is too small, the valence of the transition metal element is less than 2, and it is easy to precipitate as metal with charging and discharging. The precipitated metal dissolves in the electrolyte and precipitates as metal dendrites on the negative electrode side, so it may become the cause of internal short circuit. In addition, if z is too small, the release of sodium ions decreases, or the redox reaction of the transition metal is not easy to occur, so there is a tendency for the discharge capacity to decrease. On the other hand, if z is too large, the transition metal element will be greater than 2, and it will be difficult for the redox reaction accompanying charging and discharging to occur, and the sodium ions absorbed and released will decrease, so the discharge capacity is easy to decrease.
[0047] The transition metal element M can be at least one selected from Cr, Fe, Mn and Ni. Ni and Mn show particularly high redox potentials, so they are preferred. Ni with high operating voltage is particularly preferred. In addition, Fe has high structural stabilization during charge and discharge, and the cycle characteristics are easily improved, so it is preferred.
[0048] a is preferably 0≤a≤0.9, 0≤a≤0.5, 0≤a≤0.3, and particularly preferably a = 0. The smaller a is, the higher the oxidation-reduction potential is, and when used as a positive electrode active material for an electricity storage device, a high charge and discharge voltage is likely to be exhibited.
[0049] A, as a network-forming component, functions as an element that forms a skeleton of a crystal structure and may be at least one selected from P, Si and B. However, P and Si are preferred due to their excellent structural stability, and P is particularly preferred due to its excellent ion conductivity.
[0050] General formula Na x (Co 1-a M a )A y O z The crystal shown preferably has any crystal structure of monoclinic, triclinic, orthorhombic and tetragonal, and triclinic with excellent structural stability is particularly preferred due to its excellent cycle characteristics. In addition, the above crystal preferably belongs to at least one space group selected from P-1, P1, Cm, Pna21 and P21 / n, and is particularly preferably P-1 or P1.
[0051] Specific examples of crystals include NaCoPO4 (theoretical capacity 152 mAh / g, tetragonal P65), Na2CoSiO4 (theoretical capacity 136 mAh / g, monoclinic Pn), Na4Co3(PO4)2(P2O7)(=Na 1.33 CoP 1.33 O5, theoretical capacity 127mAh / g, orthorhombic crystal Pna21), Na 3.12 Co 2.44 (P2O7)2(=Na 1.28 CoP 1.64 O 5.74 、Theoretical capacity 116mAh / g、triclinic P-1)、Na4Co5(PO4)2(P2O7)2(=Na 0.8 CoP 1.2 O 4.4 , theoretical capacity 116mAh / g, monoclinic P21 / c), Na 3.64 Co 2.18 (P2O7)2(=Na 1.67 CoP 1.83 O 6.42, theoretical capacity 104mAh / g, triclinic P-1), Na 5.6 Co4P8O 28 (=Na 1.4 CoP2O7, theoretical capacity 103 mAh / g, triclinic P-1), Na4Co7(PO4)6(=Na 0.57 CoP 0.86 O 3.43 , theoretical capacity 100mAh / g, monoclinic Cm), Na2Co(P2O7) (theoretical capacity 96mAh / g, tetragonal P42 / mnm, orthorhombic Pna21 or P21cn, triclinic P1 or P-1), Na9Co3(PO4)5(=Na3CoP 1.67 O 6.67 , theoretical capacity 94mAh / g), Na2Co2(B 12 O 21 )(=NaCoB6O 10.5 、Theoretical capacity 85mAh / g、monoclinic I2 / a)、Na2Co(Si4O 10 )(theoretical capacity 71 mAh / g, triclinic P-1), Na3Co9(PO4)7(=Na 0.33 CoP 0.78 O 3.11 , theoretical capacity 64 mAh / g), NaCo4(PO4)3(=Na 0.25 CoP 0.75 O3, theoretical capacity 49 mAh / g, monoclinic P21 / n), Na4Co(PO3)6 (theoretical capacity 43 mAh / g, triclinic P-1), etc. In addition, each mark of the above crystal is an indicative formula, and the formula recorded in brackets represents the general formula when the coefficient of Co in the indicative formula is standardized to 1. When the general formula and the indicative formula are the same, the record is omitted.
[0052] Among them, Na 3.12 Co 2.44 (P2O7)2、Na 3.64 Co 2.18 (P2O7)2、Na 5.6 Co4P8O 28 , Na2Co(P2O7), especially Na2Co(P2O7) with high capacity and excellent cycle stability 3.64 Co 2.18 (P2O7)2、Na 5.6 Co4P8O 28 , Na is the most preferred due to its excellent cycle stability 3.64 Co 2.18 (P2O7)2.
[0053] In addition, the above-mentioned crystals may be precipitated into only one type (single phase) or two or more types (mixed crystal). In addition, the above-mentioned crystals may be precipitated as main crystals, and crystals other than the above-mentioned crystals may be precipitated.
[0054] The smaller the crystallite size of the crystal, the smaller the average particle size of the positive electrode active material particles can be, and the conductivity can be improved. Specifically, the crystallite size is preferably less than 100 nm, and particularly preferably less than 80 nm. There is no particular limitation on the lower limit of the crystallite size, but in reality it is more than 1 nm, and further more than 10 nm. The crystallite size can be obtained from the analytical results of powder X-ray diffraction according to the Scherrer formula.
[0055] The content of amorphous phase and crystal in the positive electrode active material is preferably appropriately selected according to the target characteristics. For example, the content of amorphous phase in the positive electrode active material is preferably 0.1% or more, 1% or more, 5% or more, 10% or more, 20% or more, 30% or more, 50% or more, 70% or more, and particularly preferably 90% or more (the content of crystal is 99.9% or less, 99% or less, 95% or less, 90% or less, 80% or less, 70% or less, 50% or less, 30% or less, and particularly 10% or less in mass %). If the content of amorphous phase is too small, it is difficult to obtain the above effect. In addition, if the proportion of amorphous in the positive electrode active material increases, the degree of freedom of composition design is high compared with the positive electrode active material composed of crystals, so it has the advantages of easily achieving high voltage and high capacity by appropriately adjusting the composition (for example, increasing the content of transition metal components). The upper limit of the content of the amorphous phase is not particularly limited, and can be 100% (the content of crystals is 0%), but in the case of actively precipitating crystals, it can be 99.9% or less, 99% or less, 95% or less, 90% or less, 80% or less, 70% or less, 50% or less, 30% or less, and especially 10% or less (the content of crystals is 0.1% or more, 1% or more, 5% or more, 10% or more, 20% or more, 30% or more, 50% or more, 70% or more, and especially 90% or more in terms of mass%). In this way, the above-mentioned effects obtained by containing crystals can also be enjoyed at the same time.
[0056] The content of amorphous phase and crystal in the positive electrode active material is obtained by peak separation of the crystalline diffraction line in the amorphous halo in the diffraction line spectrum at 10 to 60° at 2θ value obtained by powder X-ray diffraction using CuKα line. Specifically, in the total scattering curve obtained by subtracting the background from the diffraction line spectrum, the integrated intensity obtained by peak separation of the broad diffraction line (amorphous halo) at 10 to 50° is taken as Ia, the sum of the integrated intensities obtained by peak separation of the crystalline diffraction line of the crystalline phase represented by the above general formula detected at 10 to 60° is taken as Ic, and the sum of the integrated intensities obtained from the crystalline diffraction line from other crystals is taken as Io, the content of the amorphous phase and the content Xc of the Xg crystal are obtained from the following formula.
[0057] Xg = [Ia / (Ic+Ia+Io)] × 100 (mass %)
[0058] Xc = [Ic / (Ic+Ia+Io)] × 100 (mass %)
[0059] The positive electrode active material for the storage device of the present invention can be coated with conductive carbon or composited with conductive carbon. In this way, the electronic conductivity becomes higher and the high-speed charge and discharge characteristics are easily improved. As the conductive carbon, high-conductive carbon black such as acetylene black and ketjen black, carbon powder such as graphite, carbon fiber, etc. can be used. Among them, acetylene black with high electronic conductivity is preferred.
[0060] As a method for coating the positive electrode active material with conductive carbon, it is possible to cite a method in which the positive electrode active material and an organic compound as a conductive carbon source are mixed, and then fired in an inactive or reducing atmosphere to carbonize the organic compound. As an organic compound, any raw material can be used as long as it is an organic compound that is a carbon residue during the heat treatment, but preferably glucose, citric acid, ascorbic acid, phenolic resin, surfactant, etc. are used, and surfactants that are easily adsorbed on the surface of the positive electrode active material are particularly preferred. As a surfactant, any one of a cationic surfactant, an anionic surfactant, an amphoteric surfactant, and a nonionic surfactant can be used, and nonionic surfactants with excellent adsorption properties on the surface of the positive electrode active material are particularly preferred.
[0061] The mixing ratio of the positive electrode active material and the conductive carbon is preferably 80 to 99.5:0.5 to 20 by mass ratio, and more preferably 85 to 98:2 to 15. If the content of the conductive carbon is too small, there is a tendency for the electron conductivity to deteriorate. On the other hand, if the content of the conductive carbon is too large, the content of the positive electrode active material becomes relatively small, so there is a tendency for the discharge capacity to decrease.
[0062] In addition, when the surface of the positive electrode active material is coated with conductive carbon, the thickness of the conductive carbon film is preferably 1 to 100 nm, and particularly preferably 5 to 80 nm. If the thickness of the conductive carbon film is too small, the conductive carbon film disappears during the charge and discharge process, and the battery characteristics are easily reduced. On the other hand, if the thickness of the conductive carbon film is too large, it is easy to cause a decrease in discharge capacity, a voltage drop, etc.
[0063] The positive electrode active material for the sodium ion secondary battery of the present invention has a Raman spectroscopic range of 1300 to 1400 cm -1 The peak intensity D is relative to the peak at 1550-1650cm -1 The peak intensity ratio (D / G) of the peak intensity G is preferably 1 or less, particularly preferably 0.8 or less, and the peak intensity of the peak intensity G is preferably 0.8 or less at 800 to 1100 cm -1 The ratio of the peak intensity F to the peak intensity G (F / G) is preferably 0.5 or less, particularly preferably 0.1 or less. When these peak intensity ratios satisfy the above ranges, the electron conductivity of the positive electrode active material tends to be high.
[0064] The shape of the positive electrode active material for the storage device is not particularly limited, but if it is in powder form, the sites for the absorption and release of sodium ions increase, so it is preferred. At this time, the average particle size is preferably 0.1-20 μm, 0.3-15 μm, 0.5-10 μm, and particularly preferably 0.6-5 μm. In addition, the maximum particle size is preferably less than 150 μm, less than 100 μm, less than 75 μm, and particularly preferably less than 55 μm. If the average particle size or the maximum particle size is too large, the sites for the absorption and release of sodium ions during charge and discharge decrease, so there is a tendency for the discharge capacity to decrease. On the other hand, if the average particle size is too small, there is a tendency that the dispersion state of the powder deteriorates during paste formation and it is difficult to manufacture a uniform electrode.
[0065] The average particle size and the maximum particle size represent the median diameter of the primary particles, respectively. 50 (50% volume cumulative particle size) and D 99 (99% volume cumulative particle size) refers to a value measured using a laser diffraction particle size distribution analyzer.
[0066] (Method for producing positive electrode active material for sodium ion secondary battery)
[0067] The positive electrode active material for the sodium ion secondary battery of the present invention can be manufactured by the melt quenching method described below. First, the raw material powder is arranged in a manner to obtain batches of raw materials in a desired composition. Then, the obtained batches of raw materials are melted. The melting temperature can be appropriately adjusted in a manner that the batches of raw materials become homogeneous. Specifically, the melting temperature is preferably above 800°C, above 900°C, and particularly preferably above 1000°C. The upper limit is not particularly limited. If the melting temperature is too high, the sodium component evaporates or causes energy loss, so it is preferably below 1500°C, and particularly preferably below 1400°C.
[0068] However, when the positive electrode active material contains Fe, if sodium ions are released during the initial charge, Fe is used as charge compensation. 2+ →Fe 3+ Oxidation reaction. Therefore, by increasing the proportion of divalent ions in the positive electrode active material, the above-mentioned charge compensation oxidation reaction is easily generated, and the initial charge and discharge efficiency is easily improved. However, the glass containing divalent Fe ions (FeO) is easily oxidized to trivalent Fe ions (Fe2O3) by the melting conditions, and when melted in the atmosphere, it is easily oxidized to trivalent Fe ions (Fe2O3). Therefore, by melting in a reducing atmosphere or an inactive atmosphere, the increase in the valence of Fe ions in the glass can be suppressed, and a storage device with excellent initial charge and discharge efficiency is obtained.
[0069] In order to melt in a reducing atmosphere, it is preferred to supply a reducing gas in the melting tank. When H2 gas is used as the reducing gas, in order to reduce the risk of explosion during melting, a mixed gas to which an inert gas such as N2 is added is preferably used. Specifically, the mixed gas preferably contains 90 to 99.5% N2 and 0.5 to 10% H2 by volume, and more preferably contains 92 to 99% N2 and 1 to 8% H2. In the case of melting in an inert atmosphere, it is preferred to supply an inert gas in the melting tank. As the inert gas, it is preferred to use any of nitrogen, argon and helium. The reducing gas or the inert gas can be supplied in the upper atmosphere of the molten glass in the melting tank, or it can be directly supplied to the molten glass from a bubbling nozzle, or these two methods can be performed simultaneously.
[0070] When the positive electrode active material contains P, by using phosphates such as sodium metaphosphate (NaPO3) and trisodium phosphate (Na3PO4) in the starting raw material powder, it is easy to obtain a positive electrode active material with less devitrified foreign matter and excellent homogeneity. If the positive electrode active material is used as the positive electrode material, it is easy to obtain a secondary battery with stable discharge capacity.
[0071] The obtained melt is cooled and molded to obtain a glass body. The molding method is not particularly limited, for example, the melt can be poured between a pair of cooling rollers and molded into a film while being quenched, or the melt can be flowed into a mold and molded into an ingot. The glass body is preferably an amorphous body in terms of homogeneity, but it may also contain a part of a crystalline phase.
[0072] In addition, when the glass contains trivalent Fe ions, it is preferred to reduce them to divalent Fe ions by, for example, firing in a reducing atmosphere. As the reducing atmosphere, an atmosphere containing at least one reducing gas selected from H2, NH3, CO, H2S and SiH4 can be cited. From the viewpoint of effectively reducing the Fe ions in the glass from trivalent to divalent, H2, NH3 or CO is preferred, and H2 is particularly preferred. In addition, when H2 is used, in order to reduce the risk of explosion during firing, a mixed gas of N2 and H2 is preferably used. As the mixed gas, it is preferred to contain 90 to 99.9% of N2 and 0.1 to 10% of H2 by volume, more preferably 90 to 99.5% of N2 and 0.5 to 10% of H2, and even more preferably 92 to 99% of N2 and 1 to 4% of H2.
[0073] The firing temperature (maximum temperature) is preferably above the glass transition temperature of the glass body, specifically preferably 350 to 900°C, 400 to 850°C, 425 to 800°C, and particularly preferably 450 to 750°C. If the firing temperature is too low, there is a tendency that the reduction of Fe ions becomes insufficient. On the other hand, if the firing temperature is too high, the glass bodies fuse to each other, the specific surface area decreases, and therefore there is a tendency that the discharge capacity of the positive electrode active material decreases.
[0074] The holding time of the highest temperature during firing is preferably 10 to 600 minutes, and particularly preferably 30 to 120 minutes. If the holding time is too short, the thermal energy imparted is small, so there is a tendency for insufficient reduction of Fe ions. On the other hand, if the holding time is too long, the glasses are welded to each other, and the specific surface area is reduced, so there is a tendency for the discharge capacity of the positive electrode active material to decrease.
[0075] Furthermore, the glass body obtained as described above can be sintered to be crystallized, thereby obtaining a positive electrode active material having both an amorphous phase and a crystalline phase.
[0076] The firing temperature for crystallization is preferably above the glass transition temperature, more preferably above the crystallization temperature. The glass transition temperature and the crystallization temperature can be obtained by DSC (differential scanning calorimetry) or DTA (differential thermal analysis). If the firing temperature is too low, there is a tendency that the precipitation of the crystalline phase is insufficient. On the other hand, if the firing temperature is too high, the glass bodies are fused to each other, and the specific surface area is reduced, so there is a tendency that the discharge capacity of the positive electrode active material is reduced. Therefore, the firing temperature is preferably below 900°C, below 800°C, below 700°C, and particularly preferably below 600°C.
[0077] The firing time is appropriately adjusted so that crystallization of the glass body proceeds sufficiently, and specifically, it is preferably 20 to 300 minutes, and more preferably 30 to 240 minutes.
[0078] The above-mentioned firing can be performed using an electric heating furnace, a rotary kiln, a microwave heating furnace, a high-frequency heating furnace, etc. In addition, the reduction and crystallization of Fe ions in the glass body can also be performed simultaneously.
[0079] In addition, as required, the glass and the conductive carbon can also be mixed while being crushed, thereby imparting conductivity. As a method of mixing while crushing, a method using a common pulverizer such as a mortar, a pestle, a ball mill, an ultrafine grinder, a vibrating ball mill, a satellite ball mill, a planetary ball mill, a jet mill, a bead mill, etc. can be cited. Among them, a planetary ball mill is preferably used. The planetary ball mill rotates while the tank rotates on its own axis and the plate rotates on the other side, and very high impact energy can be efficiently generated. Therefore, the conductive carbon can be uniformly dispersed in the glass to improve the electronic conductivity.
[0080] In addition, as described above, after mixing the glass body and the organic compound as the conductive carbon source, the glass body can be coated with conductive carbon by firing in an inactive or reducing atmosphere to carbonize the organic compound. In addition, the firing can be performed simultaneously with a heat treatment step for reducing Fe ions or a heat treatment step for crystallizing the glass body.
[0081] In addition, when using a general solid phase reaction method to make a positive electrode active material, the charge and discharge potential sometimes becomes too high undesirably. Therefore, when applied to a sodium ion secondary battery using a non-aqueous electrolyte as an electrolyte, the charge and discharge potential is likely to reach the decomposition potential of the electrolyte. As a result, with repeated charge and discharge, it is easy to produce a reduction in discharge capacity or charge and discharge efficiency caused by decomposition of the electrolyte. In addition, the positive electrode active material obtained by the solid phase reaction method is usually free of amorphous substances, so it is difficult to enjoy the effect of the above-mentioned present invention obtained by containing amorphous substances.
[0082] (Positive electrode materials for sodium ion secondary batteries)
[0083] By mixing the positive electrode active material for a sodium ion secondary battery of the present invention with a conductive auxiliary agent, a binder, etc., a positive electrode material for a sodium ion secondary battery can be obtained.
[0084] Examples of the conductive auxiliary agent include highly conductive carbon black such as acetylene black and Ketjen black, and conductive carbon in powder or fiber form such as graphite, etc. Among them, acetylene black is preferred because it can improve conductivity by adding a small amount.
[0085] Binders are components added to bind the materials constituting the positive electrode material to each other and prevent the positive electrode active material from detaching from the positive electrode due to the volume change accompanying charge and discharge. Specific examples of binders include thermoplastic linear polymers such as polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVDF), fluorine rubber, styrene-butadiene rubber (SBR), etc.; thermosetting resins such as thermosetting polyimide, polyamide-imide, polyamide, phenolic resin, epoxy resin, urea-formaldehyde resin, melamine resin, unsaturated polyester resin, polyurethane, etc.; cellulose derivatives such as carboxymethyl cellulose (also including carboxymethyl cellulose salts such as sodium carboxymethyl cellulose. The same applies below.), hydroxypropyl methyl cellulose, hydroxypropyl cellulose, hydroxyethyl cellulose, ethyl cellulose and hydroxymethyl cellulose; water-soluble polymers such as polyvinyl alcohol, polyacrylamide, polyvinyl pyrrolidone and copolymers thereof. Among them, from the perspective of excellent bonding properties, thermosetting resins, cellulose derivatives, and water-soluble polymers are preferred, and thermosetting polyimide or carboxymethyl cellulose, which are widely used in industry, are more preferred. In particular, carboxymethyl cellulose is most preferred because it is inexpensive and has low environmental impact and does not require an organic solvent when preparing an electrode-forming paste. These binders may be used alone or in combination of two or more.
[0086] When the positive electrode active material for the sodium ion secondary battery of the present invention is used as a solid sodium ion secondary battery, it is preferred to add a sodium ion conductive solid electrolyte as a constituent component of the positive electrode material for the sodium ion secondary battery. The sodium ion conductive solid electrolyte is a component responsible for the sodium ion conduction between the positive electrode and the negative electrode in a fully solid-state storage device. When the sodium ion conductive solid electrolyte is β-alumina or a sodium superion conductor type crystal, it is preferred because of its excellent sodium ion conductivity. β-alumina exists in two crystal forms: β-alumina (theoretical composition formula: Na2O·11Al2O3) and β” alumina (theoretical composition formula: Na2O·5.3Al2O3). β” alumina is a quasi-stable substance, so a substance with Li2O and / or MgO added as a stabilizer is usually used. Compared with β-alumina, β” alumina has a higher sodium ion conductivity, so it is preferred to use β” alumina alone, or to use a mixture of β” alumina and β” alumina, and it is more preferred to use Li2O stabilized β” alumina (Na 1.6 Li 0.34 Al10.66 O 17 ) or MgO stabilized β” alumina ((Al 10.32 Mg 0.68 O 16 )(Na 1.68 O)).
[0087] As the sodium superion conductor type crystal, Na3Zr2Si2PO 12 、Na 3.2 Zr 1.3 Si 2.2 P 0.8 O 10.5 、Na3Zr 1.6 Ti 0.4 Si2PO 12 、Na3Hf2Si2PO 12 、Na 3.4 Zr 0.9 Hf 1.4 Al 0.6 Si 1.2 P 1.8 O 12 、Na3Zr 1.7 Nb 0.24 Si2PO 12 、Na 3.6 Ti 0.2 Y 0.8 Si 2.8 O9、Na3Zr 1.88 Y 0.12 Si2PO 12 、Na 3.12 Zr 1.88 Y 0.12 Si2PO 12 、Na 3.6 Zr 0.13 Yb 1.67 Si 0.11 P 2.9 O 12 etc., especially Na 3.12 Zr 1.88 Y 0.12 Si2PO 12 Since sodium ion conductivity is excellent, it is preferred.
[0088] Average particle size D of sodium ion conductive solid electrolyte 50 It is preferably 0.3 to 25 μm, 0.5 to 20 μm, and particularly preferably 1.2 to 15 μm. 50If the average particle size D of the sodium ion conductive solid electrolyte is too small, it is not only difficult to mix uniformly with the positive electrode active material, but also absorbs moisture or carbonates, so that the ion conductivity is easily reduced. As a result, there is a tendency for the internal resistance to increase, and the charge and discharge voltage and discharge capacity to decrease. On the other hand, if the average particle size D of the sodium ion conductive solid electrolyte is 50 If it is too large, the softening and flow of the positive electrode active material is significantly hindered during sintering for forming the positive electrode layer, so that the smoothness of the obtained positive electrode layer is poor, the mechanical strength is reduced, or the internal resistance tends to increase.
[0089] The composition of the positive electrode material is preferably appropriately selected according to the type of electrolyte used. For example, in a sodium ion secondary battery using an aqueous or non-aqueous liquid electrolyte, it is preferably composed of 70 to 95% of a positive electrode active material, 1 to 15% of a conductive aid, and 3 to 15% of a binder in terms of mass %, preferably 80 to 95% of a positive electrode active material, 2 to 10% of a conductive aid, and 3 to 10% of a binder. If the content of the positive electrode active material is too little, the discharge capacity of the sodium ion secondary battery is easily reduced. If it is too much, the content of the conductive aid and the binder will be relatively reduced, so the electronic conductivity or cycle characteristics are easily reduced. If the content of the conductive aid is too little, the electronic conductivity is poor. If it is too much, the bonding between the constituent components of the positive electrode material is reduced, and the internal resistance is increased, so there is a tendency for the charge and discharge voltage and discharge capacity to decrease. If the content of the binder is too little, the bonding between the constituent materials of the positive electrode material is reduced, and the cycle characteristics are easily reduced. If it is too much, the electronic conductivity is reduced, so the rapid charge and discharge characteristics are easily reduced.
[0090] In the case of a solid sodium ion secondary battery using a sodium ion conductive solid electrolyte as the electrolyte, it is preferably calculated by mass %, containing 30 to 100% of a positive electrode active material, 0 to 20% of a conductive aid, and 0 to 70% of a solid electrolyte, more preferably containing 34.5 to 94.5% of a positive electrode active material, 0.5 to 15% of a conductive aid, and 5 to 65% of a solid electrolyte, and more preferably containing 40 to 92% of a positive electrode active material, 1 to 10% of a conductive aid, and 7 to 50% of a solid electrolyte. If the content of the positive electrode active material is too little, the discharge capacity of the sodium ion secondary battery is easily reduced. If the content of the conductive aid or the solid electrolyte is too much, the bonding between the constituent components of the positive electrode material is reduced and the internal resistance is increased, so there is a tendency for the charge and discharge voltage and discharge capacity to decrease.
[0091] The mixing of the constituent components of the positive electrode material can use a mixer such as a rotary revolution mixer, a drum mixer, a mortar, a mortar crusher, a ball mill, an attritor, a vibration ball mill, a satellite ball mill, a planetary ball mill, a jet mill, a bead mill, and other common pulverizers. In particular, by using a planetary ball mill, the constituent materials can be uniformly dispersed.
[0092] The positive electrode material for sodium ion secondary battery of the present invention is applied on a collector formed of a metal foil such as aluminum, copper, gold, etc., dried, and then fired as needed, and used as a positive electrode for sodium ion secondary battery. Alternatively, the positive electrode material for sodium ion secondary battery of the present invention can be formed into a sheet, and then a collector including a metal coating is formed by sputtering or plating.
[0093] (Sodium ion secondary battery)
[0094] The sodium ion secondary battery of the present invention includes a negative electrode as a counter electrode and an electrolyte in addition to the positive electrode for the sodium ion secondary battery described above.
[0095] The negative electrode contains a negative electrode active material that can absorb and release sodium ions during charge and discharge. As the negative electrode active material, metal materials such as metal Na, metal Sn, metal Bi, metal Zn, Sn-Cu alloy, Bi-Cu alloy, carbon materials such as hard carbon, oxide materials containing Ti and / or Nb as elements, etc. can be used. Among them, oxide materials containing Ti and / or Nb as elements have high safety and are abundant in resources, so they are preferred. In particular, it is preferred to use a material containing a redox potential of 1.5V (vs. Na / Na) during charge and discharge. + ) or an oxide material of a crystalline phase represented by Na4TiO(PO4)2 or Na5Ti(PO4)3. At this time, the operating voltage of the sodium ion secondary battery is high, and the precipitation of metal Na dendrites during repeated charge and discharge can be suppressed.
[0096] As electrolyte, aqueous electrolyte, non-aqueous electrolyte, solid electrolyte etc. can be used. The potential window of non-aqueous electrolyte or solid electrolyte is wide, so the phenomenon of gas generation accompanying the decomposition of electrolyte during charge and discharge hardly occurs, which can improve the safety of sodium ion secondary battery. Among them, non-flammable solid electrolyte is preferred.
[0097] Aqueous electrolytes include electrolyte salts that can be dissolved in water. Examples of electrolyte salts include NaNO3, Na2SO4, NaOH, NaCl, CH3COONa, etc. These electrolyte salts can be used alone or in combination of two or more. The electrolyte salt concentration is generally adjusted appropriately within the range of 0.1M to saturation concentration.
[0098] When an aqueous electrolyte is used, the positive electrode active material for a sodium ion secondary battery of the present invention can be used as long as the oxidation-reduction potential thereof is within the range of the potential window of water.
[0099] The non-aqueous electrolyte includes an organic solvent and / or an ionic liquid as a non-aqueous solvent, and an electrolyte salt dissolved in the non-aqueous solvent. The organic solvent as the non-aqueous solvent is not particularly limited, and examples thereof include: propylene carbonate (PC), ethylene carbonate (EC), 1,2-dimethoxyethane (DME), γ-butyrolactone (GBL), tetrahydrofuran (THF), 2-methyltetrahydrofuran (2-MeHF), 1,3-dioxolane, cyclopentane, acetonitrile (AN), diethyl carbonate (DEC), dimethyl carbonate (DMC), ethyl methyl carbonate (MEC), dipropyl carbonate (DPC), etc. These non-aqueous solvents can be used alone or in combination of two or more. Among them, propylene carbonate with excellent low temperature properties is preferred.
[0100] The ionic liquid is not particularly limited as long as it can dissolve the electrolyte salt used. Specifically, examples thereof include aliphatic quaternary ammonium salts such as N,N,N-trimethyl-N-propylammonium bis(trifluoromethanesulfonyl)imide [abbreviation: TMPA-TFSI], N-methyl-N-propylpiperidinium bis(trifluoromethanesulfonyl)imide [abbreviation: PP13-TFSI], N-methyl-N-propylpyrrolidinium bis(trifluoromethanesulfonyl)imide [abbreviation: P13-TFSI], N-methyl-N-butylpyrrolidinium bis(trifluoromethanesulfonyl)imide [abbreviation: P14-TFSI], etc.; 1-methyl-3-ethylimidazolium tetrafluoroborate [abbreviation: EMIBF4], Alkyl imidazolium quaternary salts such as 1-methyl-3-ethylimidazolium bis(trifluoromethanesulfonyl)imide [abbreviation: EMITFSI], 1-allyl-3-ethylimidazolium bromide [abbreviation: AEImBr], 1-allyl-3-ethylimidazolium tetrafluoroborate [abbreviation: AEImBF4], 1-allyl-3-ethylimidazolium bis(trifluoromethanesulfonyl)imide [abbreviation: AEImTFSI], 1,3-diallylimidazolium bromide [abbreviation: AAImBr], 1,3-diallylimidazolium tetrafluoroborate [abbreviation: AAImBF4], and 1,3-diallylimidazolium bis(trifluoromethanesulfonyl)imide [abbreviation: AAImTFSI].
[0101] As the electrolyte salt, PF 6- , BF 4- 、(CF3SO2)2N - (bis(trifluoromethanesulfonylamide; commonly known as TFSI), CF3SO 3- (commonly known as TFS), (C2F5SO2)2N - (bispentafluoroethanesulfonylamide; commonly known as BETI), ClO 4- , AsF 6- , SbF 6- , Bis(oxalatoborate) (B(C2O4)2- ; commonly known as BOB), difluoro(trifluoro-2-oxide-2-trifluoro-methylpropionate (2-)-0,0)boric acid (BF2OCOOC(CF3) 3- , commonly known as sodium salts of B (HHIB)). These electrolyte salts can be used alone or in combination of two or more. Inexpensive PF 6- , BF 4- The electrolyte salt concentration is usually adjusted appropriately within the range of 0.5 to 3M.
[0102] In addition, the non-aqueous electrolyte may contain additives such as vinylene carbonate (VC), vinylene acetate (VA), vinylene butyrate, vinylene caproate, vinylene crotonate, catechol carbonate, etc. These additives have the effect of forming a protective film on the surface of the active material. The concentration of the additive is preferably 0.1 to 3 parts by mass, particularly preferably 0.5 to 1 part by mass, relative to 100 parts by mass of the non-aqueous electrolyte.
[0103] As a solid electrolyte, the above-mentioned solid electrolyte can be used. Since the solid electrolyte has a wider potential window than aqueous electrolytes and non-aqueous electrolytes, there is almost no occurrence of gas associated with decomposition, which can improve the safety of the sodium ion secondary battery. Therefore, the positive electrode active material for the sodium ion secondary battery of the present invention is also most preferably used as a positive electrode active material for an all-solid sodium ion secondary battery using a solid electrolyte.
[0104] In the case of a sodium ion secondary battery using an aqueous electrolyte or a non-aqueous electrolyte electrolyte system, a separator is preferably provided between the electrodes. The separator is composed of an insulating material, specifically a porous film or non-woven fabric obtained from a polymer such as polyolefin, cellulose, polyethylene terephthalate, vinylon, etc., a glass non-woven fabric containing fibrous glass, a glass cloth woven from fibrous glass, a film-like glass, etc. can be used.
[0105] Example
[0106] Hereinafter, the present invention will be described in detail based on examples, but the present invention is not limited to the following examples at all.
[0107] Table 1 and Table 2 show Examples (No. 1 to 5) and Comparative Examples (No. 6 to 9) of the present invention.
[0108] [Table 1]
[0109]
[0110] [Table 2]
[0111]
[0112] Sodium ion secondary batteries using non-aqueous electrolytes (electrolyte batteries)
[0113] (1) Preparation of positive electrode active material (1-a) No. 1 to 7 (preparation by melting method)
[0114] Sodium carbonate, sodium metaphosphate, cobalt oxide (CoO), iron oxide (Fe2O3), nickel oxide (NiO), and orthophosphoric acid were used as raw materials to prepare raw material powders in a manner to obtain the compositions described in No. 1 to 7 shown in Tables 1 and 2. The raw material powders were put into a quartz crucible and melted in an electric furnace at 1250° C. for 60 minutes in the atmosphere. Then, the molten glass was poured between a pair of rotating rollers and formed while being quenched to obtain a film-like glass body with a thickness of 0.1 to 2 mm. The film-like glass body was crushed with a ball mill and air-classified to obtain a glass powder with an average particle size of 2 μm.
[0115] With respect to 100 parts by mass of the glass powder obtained above, 21.4 parts by mass (equivalent to 12 parts by mass in terms of carbon conversion) of a nonionic surfactant polyethylene oxide nonylphenyl ether (HLB value: 13.3, mass average molecular weight: 660) as a carbon source and 10 parts by mass of ethanol were fully mixed and dried at 100°C for about 1 hour. Then, by sintering at 700°C for 1 hour in a nitrogen atmosphere, carbonization of the nonionic surfactant and crystallization of the powder were simultaneously performed to obtain a positive electrode active material with a surface coated with carbon. After crushing it with a ball mill, air classification was performed to obtain a positive electrode active material powder with an average particle size of 2 μm.
[0116] The obtained positive electrode active material powder was subjected to powder X-ray diffraction measurement and Rietveld analysis to determine the crystal structure and space group. In addition, the amorphous content was calculated using the above method. The results are shown in Tables 1 and 2. In addition, Figure 1 The XRD pattern of sample No. 1 is shown. Figure 1 The lower part also shows the XRD pattern of the crystalline phase. The lattice parameter obtained by the refinement of Rietveld analysis is a: b: c: α: 93.980°, β: 104.04°, γ: 92.07°.
[0117] (1-b) No.8, No.9 (made by solid phase reaction method)
[0118] Sodium carbonate, sodium metaphosphate, cobalt oxide, nickel oxide, and orthophosphoric acid were weighed to obtain the compositions described in No. 8 and No. 9 of Table 2 to prepare batches of raw materials. The batches of raw materials were mixed in ethanol using a planetary ball mill and then dried at 100°C. The dried batches of raw materials were pre-calcined in an electric furnace at 900°C for 6 hours to degas. The pre-calcined batches of raw materials were heated at 500 kgf / cm 2 After pressure molding, the sintered body was fired at 800°C for 12 hours in an atmosphere. The ZrO2 grinding balls were crushed in a ball mill for 12 hours and air classified to obtain an average particle size D 50 The solid phase reaction product is a powder of 2 μm.
[0119] For 100 parts by mass of the powdered solid phase reaction product obtained above, 21.4 parts by mass (equivalent to 12 parts by mass in terms of carbon conversion) of a nonionic surfactant polyethylene oxide nonylphenyl ether (HLB value: 13.3, mass average molecular weight: 660) as a carbon source and 10 parts by mass of ethanol were fully mixed and dried at 100° C. for about 1 hour. Then, the mixture was calcined at 700° C. for 1 hour under a nitrogen atmosphere to carbonize the nonionic surfactant and obtain a positive electrode active material powder whose surface was coated with carbon.
[0120] The crystal structure, space group, and amorphous content of the obtained positive electrode active material powder were determined by the same method as above. The results are shown in Table 2.
[0121] (2) Preparation of positive electrode
[0122] The positive electrode active material powder obtained above was weighed in a manner such that acetylene black (Super C65 manufactured by Timcal) as a conductive aid and polyvinylidene fluoride as a binder were positive electrode active material powder: conductive aid: binder = 90:5:5 (mass ratio), dispersed in N-methylpyrrolidone, and then fully stirred and slurried using a rotation / revolution mixer to obtain a positive electrode material.
[0123] Then, the obtained positive electrode material was coated on a 20 μm thick aluminum foil as a positive electrode collector using a scraper with a gap of 125 μm, and after vacuum drying in a dryer at 70°C, it was pressed between a pair of rotating rollers to obtain an electrode sheet. The electrode sheet was punched into a diameter of 11 mm using an electrode punching machine, and dried under reduced pressure at a temperature of 150°C for 8 hours to obtain a circular positive electrode.
[0124] (3) Preparation of test battery
[0125] The test cell for sodium ion secondary battery is made as follows. The positive electrode obtained above is placed on the lower cover of the button cell with the aluminum foil facing downward, and a 16 mm diameter diaphragm made of a polypropylene porous film dried at 70°C under reduced pressure for 8 hours, metallic sodium as a counter electrode, and the upper cover of the button cell are stacked thereon to make the test cell. As the electrolyte, 1M NaPF6 solution / EC:DEC=1:1 (EC=ethylene carbonate, DEC=diethyl carbonate) is used. In addition, the assembly of the test cell is carried out in an environment with a dew point temperature below -70°C.
[0126] (4) Charge and discharge test
[0127] CC (constant current) charging was performed from open circuit voltage to 5.1V at 30°C, and the amount of electricity charged to each unit mass of the positive electrode active material (initial charge capacity) and the average voltage were calculated. Then, CC discharge was performed from 5.1V to 2V, and the amount of electricity released from each unit mass of the positive electrode active material (initial discharge capacity) and the average voltage were calculated. The C rate was set to 0.1C.
[0128] The results of the charge and discharge characteristics are shown in Tables 1 and 2. In the tables, "discharge capacity" indicates the initial discharge capacity, "average voltage" indicates the average operating voltage at the initial discharge, and "energy density" indicates the product of the discharge capacity and the average voltage.
[0129] As can be seen from Table 1 and Table 2, the discharge capacity of No. 1 to 5 as examples is 78 to 89 mAh / g, the average voltage is 3.7 to 4.09 V, and the energy density is as high as 300 to 360 Wh / kg. On the other hand, the average voltage of No. 6 as a comparative example is as low as 2.87 V, and the discharge capacity of No. 7 to 9 is as low as 49 to 68 mAh / g. As a result, the energy density of No. 6 to 9 is 225 to 274 Wh / kg, which is worse than that of the examples.
[0130] Sodium ion secondary battery using solid electrolyte (all-solid-state battery)
[0131] (1) Preparation of positive electrode active material precursor powder
[0132] Raw material powders are prepared using sodium carbonate, sodium metaphosphate, cobalt oxide (CoO), iron oxide (Fe2O3), nickel oxide (NiO), and orthophosphoric acid as raw materials in a manner to obtain the compositions described in No. 1 to 3 and 6 to 7 shown in Tables 1 and 2. The raw material powders are placed in a quartz crucible and melted in an electric furnace at 1250°C in the atmosphere for 60 minutes. The molten glass is then poured between a pair of rotating rollers and shaped while being rapidly cooled to obtain a film-like glass body with a thickness of 0.1 to 2 mm. The film-like glass body is subjected to The glass coarse powder was pulverized in a ball mill with ZrO2 balls for 10 hours and passed through a resin sieve with an aperture of 120 μm to obtain a glass coarse powder with an average particle size of 7 μm. Furthermore, ethanol was used as a pulverizing aid to pulverize the glass coarse powder. The ZrO2 balls were used to grind the powder for 80 hours, thereby obtaining a glass powder (positive electrode active material precursor powder) with an average particle size of 0.5 μm. The XRD measurement results showed that the glass powder was amorphous.
[0133] (2) Preparation of sodium ion conductive solid electrolyte
[0134] For the composition Na 1.6 Li 0.34 Al 10.66 O 17 Li2O-stabilized β" alumina (manufactured by Ionotec) was dry-ground to a thickness of 0.2 mm to obtain a solid electrolyte sheet. In addition, the obtained solid electrolyte sheet was crushed using a planetary ball mill and air-classified to produce a solid electrolyte powder (average particle size 1.5 μm). The production of the above-mentioned solid electrolyte sheet and powder was carried out in an environment with a dew point below -50°C to prevent moisture absorption and deterioration.
[0135] (3) Fabrication of solid sodium ion secondary batteries
[0136] For No. 1 to 3 and No. 6 to 7, the positive electrode active material precursor powder, solid electrolyte powder, and acetylene black (Super C65 manufactured by Timcal) as a conductive aid obtained in (1) above were weighed in a ratio of 72:25:3 (mass ratio), and mixed for 60 minutes using an agate mortar and pestle to obtain a mixed powder. For No. 8 and No. 9, instead of the positive electrode active material precursor powder, a powdered solid phase reaction product prepared in the above-mentioned electrolyte battery was used to obtain a mixed powder. 10 parts by mass of polypropylene carbonate was added to 100 parts by mass of the obtained mixed powder, and 40 parts by mass of anhydrous N-methylpyrrolidone was further added, and the mixture was fully stirred using a rotation / revolution mixer to form a slurry.
[0137] The obtained slurry was spread over an area of 1 cm 2, 70μm thick, coated on one surface of the above solid electrolyte sheet, and dried at 70℃ for 3 hours. Then, put it into a carbon container, No.1 at 500℃ in a nitrogen atmosphere, No.2 at 550℃ in a nitrogen atmosphere, No.3 at 530℃ in a nitrogen atmosphere, No.6 at 550℃ in a nitrogen / hydrogen (=96 / 4 volume %) atmosphere, No.7 at 550℃ in a nitrogen atmosphere, No.8 and No.9 at 650℃ in a nitrogen atmosphere for 30 minutes, respectively, to crystallize the positive electrode active material precursor powder and form a positive electrode layer. In addition, all the above operations are carried out in an environment with a dew point below -50℃.
[0138] Powder X-ray diffraction patterns of the materials constituting the positive electrode layer were observed, and diffraction lines derived from the crystals listed in Tables 1 and 2 were observed. In addition, in all positive electrodes, crystalline diffraction lines derived from the solid electrolyte powders used were observed.
[0139] Then, a collector composed of a gold electrode with a thickness of 300 nm was formed on the surface of the positive electrode layer using a sputtering device (SC-701AT manufactured by Sanyu Electronics Co., Ltd.). Furthermore, in an argon atmosphere with a dew point below -70°C, metallic sodium, which will become a counter electrode, was pressed against the surface of the solid electrolyte layer opposite to the surface on which the positive electrode layer was formed. The obtained laminate was placed on the lower cover of the button battery, and then the upper cover was covered to make a CR2032 type test battery.
[0140] (4) Charge and discharge test
[0141] For the test battery produced, CC (constant current) charging was performed from the open circuit voltage to 5.0V at 60°C, and the amount of electricity charged to each unit mass of the positive electrode active material (initial charge capacity) and the average voltage were calculated. Then, CC discharge was performed from 5.0V to 2V, and the amount of electricity released from each unit mass of the positive electrode active material (initial discharge capacity) and the average voltage were calculated. In addition, in this test, the C rate was evaluated at 0.01C. The results are shown in Tables 1 and 2, and in Figure 2 3 shows the initial charge and discharge curve of the solid sodium ion secondary battery using the sample No. 1.
[0142] As can be seen from Tables 1 and 2, the discharge capacity of No. 1 to 3 as examples is 83 to 91 mAh / g, the average voltage is 4.3 to 4.31 V, and the energy density is as high as 357 to 391 Wh / kg. On the other hand, the average voltage of No. 6 as a comparative example is as low as 2.63 V, and the discharge capacity of No. 7 is as low as 51 mAh / g. As a result, the energy density of No. 6 and 7 is 171 to 238 Wh / kg, which is worse than that of the examples. In addition, the batteries of No. 8 and 9 did not work.
[0143] Industrial Applicability
[0144] The positive electrode active material for a sodium ion secondary battery of the present invention is suitable for sodium ion secondary batteries used in portable electronic devices, electric vehicles, electric tools, backup emergency power supplies, and the like.
Claims
1. A positive electrode active material for a sodium ion secondary battery, characterized in that: In terms of molar % converted into oxides, it contains 8 to 55% Na2O, 10 to 70% CoO, 0 to 60% CrO+FeO+MnO+NiO, 15 to 70% P2O5+SiO2+B2O3, and an amorphous phase, wherein the content of the amorphous phase is in the range of 4% to 18% by mass.
2. The positive electrode active material for a sodium ion secondary battery according to claim 1, wherein: Contains the general formula Na x (Co 1-a M a )A y O z The crystal composition shown is a crystal, wherein M is at least one selected from Cr, Fe, Mn and Ni, A is at least one selected from P, Si and B, 0.5≤x≤4.1, 0.65≤y≤6.5, 2.5≤z≤20, 0≤a≤0.
9.
3. The positive electrode active material for a sodium ion secondary battery according to claim 1 or 2, characterized in that: The crystal has at least one crystal structure selected from the group consisting of monoclinic, triclinic, orthorhombic and tetragonal.
4. The positive electrode active material for a sodium ion secondary battery according to claim 1 or 2, characterized in that: The crystals belong to at least one space group selected from the group consisting of P-1, P1, Cm, Pna21 and P21 / n.
5. A positive electrode material for a sodium ion secondary battery, characterized in that: The positive electrode active material for a sodium ion secondary battery according to any one of claims 1 to 4 is contained.
6. The positive electrode material for sodium ion secondary battery according to claim 5, characterized in that: Also contains a conductive additive.
7. The positive electrode material for sodium ion secondary battery according to claim 5 or 6, characterized in that: A sodium ion conductive solid electrolyte is also included.
8. The positive electrode material for sodium ion secondary battery according to claim 7, characterized in that: The sodium ion conductive solid electrolyte is β-alumina or sodium super ion conductor type crystal.
9. The positive electrode material for sodium ion secondary battery according to claim 5 or 6, characterized in that: The sodium ion secondary battery contains, by mass%, 30 to 100% of a positive electrode active material for a sodium ion secondary battery, 0 to 20% of a conductive auxiliary agent, and 0 to 70% of a sodium ion conductive solid electrolyte.
10. A positive electrode for a sodium ion secondary battery, characterized in that: The positive electrode material for a sodium ion secondary battery according to any one of claims 5 to 9 is used.
11. A sodium ion secondary battery, characterized in that: A positive electrode for a sodium ion secondary battery according to claim 10.
12. A method for producing a positive electrode active material for a sodium ion secondary battery, for producing the positive electrode active material for a sodium ion secondary battery according to any one of claims 1 to 4, the method comprising: The process of melting batches of raw materials to obtain a melt; and The process of obtaining a glass body by cooling the melt.
13. The method for producing a positive electrode active material for a sodium ion secondary battery according to claim 12, wherein: Also includes: The process of crystallizing a glass body by firing it.
14. The method for producing a positive electrode active material for a sodium ion secondary battery according to claim 13, wherein: The glass body is fired together with at least one selected from the group consisting of conductive carbon, a conductive carbon source, and a sodium ion conductive solid electrolyte.