Broccoli-shaped MnWO4 electrocatalyst as well as preparation method and application thereof
By using polyoxygenate and trimethylolic acid in the ethanol-water system, broccoli-like MnWO4 electrocatalyst is prepared by solvothermal method, the problem of using highly toxic solvents and complex preparation processes in the prior art is solved, and the problem of using a high toxic solvent and complex preparation process is achieved. Efficient and environmentally friendly catalyst preparation, with excellent electrocatalytic performance and good electron transport capability.
Patent Information
- Application Number
- CN202411023258.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-11-12
AI Technical Summary
The existing preparation methods for MnWO4 electrocatalysts require the use of highly toxic organic solvents and surfactants, and the preparation process is cumbersome, making it difficult to achieve efficient and environmentally friendly catalyst preparation.
The broccoli-like MnWO4 electrocatalyst is prepared by solvothermal method using green material polyoxygenate as structural guide agent. In the ethanol-water system, using phenylagenic acid as the linking agent, using manganese salt and polyoxygenate salt The mixed solution in deionized water is subjected to a solvothermal reaction with the solution of the linking agent in an organic solvent, and the broccoli-like MnWO4 is obtained after calcination.
The prepared broccoli-shaped MnWO4 electrocatalyst has good electron transport capability and excellent electrocatalytic properties. It is suitable for a variety of electrochemical applications. It has a simple preparation method, environmentally friendly, high yield, and the reagents used are non-toxic.
Smart Images

Figure CN118943389A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of electrochemical applications, and in particular relates to a broccoli-shaped MnWO4 electrocatalyst and a preparation method and application thereof. Background Art
[0002] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention, and should not necessarily be regarded as an admission or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art.
[0003] Energy storage technology is one of the core technologies to promote the clean and efficient use of world energy, break through energy resources and environmental constraints, and achieve global energy transformation and upgrading. Among them, the electrocatalytic oxygen reduction reaction (ORR) and oxygen evolution reaction (OER) are key reactions that control the performance of fuel cells and reversible metal-air batteries. Therefore, improving the efficiency of the key reactions involved in such technologies is of great significance to the development and promotion of the above technologies, that is, exploring the preparation of efficient electrocatalysts is of great significance.
[0004] At present, catalysts based on manganese oxide are becoming more and more popular, and their catalytic activity is comparable to that of catalysts based on Pt group metals. Studies have found that the shape, structure and exposed surface activity of manganese oxide catalysts play a crucial role. Among them, MnWO4 has the remarkable characteristics of low toxicity, easy synthesis, high conductivity, good stability, outstanding catalytic, magnetic and electrochemical properties. It is a suitable electrode material for electrocatalytic and electrochemical applications and is widely used in optical fibers, photoluminescence, humidity sensors, supercapacitors, electrochemical sensors, batteries and photocatalysis.
[0005] The inventors have found that although there are studies that have prepared MnWO4 in various forms by using different types of synthesis methods, such as template method, surfactant-assisted precipitation method and hydrothermal method, most of the preparation methods require highly toxic organic solvents or surfactants, and also require precise control of the solution pH, and the preparation methods are relatively cumbersome. Summary of the invention
[0006] In view of the above problems, the purpose of the present invention is to provide a broccoli-shaped MnWO4 electrocatalyst and its preparation method and application. The present invention uses green material polyoxometalate (POM) as a structure directing agent, and in an ethanol-water system, trimesic acid (H3BTC) is used as a linker to prepare broccoli-shaped MnWO4 for the first time by a solvothermal method. The broccoli-shaped MnWO4 has good electron transmission ability and excellent electrocatalytic performance, and is suitable for a variety of electrochemical application fields.
[0007] Specifically, the present invention provides the following technical solutions:
[0008] The first aspect of the present invention provides a method for preparing a broccoli-shaped MnWO4 electrocatalyst, comprising the following steps:
[0009] S1, dissolving a manganese salt and a polyoxometalate in deionized water to form a solution A;
[0010] S2, the linker is dissolved in an organic solvent to form a solution B;
[0011] S3, mixing solution A and solution B, performing a solvothermal reaction, and preparing a MnWO4 precursor;
[0012] S4. calcining MnWO4 to obtain broccoli-shaped MnWO4.
[0013] Preferably, the molar ratio of the manganese salt, the polyoxometalate, and the linker is 2-3.5:0.02-0.05:1.5-2.5.
[0014] Further preferably, the molar ratio of the manganese salt, the polyoxometalate, and the linker is 3:0.04:2.
[0015] Preferably, in step S1, the manganese salt is selected from one or more of MnSO4, MnCl2, KMnO4, and Mn(Ac)2.
[0016] Preferably, in step S1, the polyoxometalate is selected from silicotungstic acid or phosphotungstic acid and other simple tungstate-based polyoxometalates.
[0017] Preferably, in step S2, the linking agent is trimesic acid (H3BTC).
[0018] Preferably, in step S2, the organic solvent is selected from one or more of methanol, ethanol and ethylene glycol.
[0019] More preferably, the organic solvent is ethanol.
[0020] Preferably, in step S3, the reaction temperature is 125-180° C. and the reaction time is 6 h to 30 h.
[0021] Preferably, in step S3, the product after the solvothermal reaction is washed with deionized water and ethanol, and then dried in a vacuum drying oven.
[0022] Preferably, in step S4, the calcination temperature is between 600 and 800°C.
[0023] Preferably, in step S4, the calcination is carried out in an inert atmosphere, and the inert atmosphere is one or a combination of hydrogen, nitrogen, and argon.
[0024] The second aspect of the present invention provides a broccoli-shaped MnWO4 electrocatalyst obtained by the preparation method described in the first aspect.
[0025] The third aspect of the present invention provides the use of the broccoli-shaped MnWO4 electrocatalyst described in the second aspect in the preparation of a reversible zinc-air battery.
[0026] One or more embodiments of the present invention have at least the following beneficial effects:
[0027] (1) The broccoli-shaped MnWO4 electrocatalyst prepared by the present invention has a regular and beautiful morphology, a high specific surface area, good electron transport capacity and excellent electrocatalytic performance, and is suitable for a variety of electrochemical application fields.
[0028] (2) The preparation method used in the present invention has high yield and large output, the reagents used are non-toxic, the morphology control parameters are simple and efficient, and the preparation process is simple and environmentally friendly. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] The accompanying drawings in the specification, which constitute a part of the present invention, are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute improper limitations on the present invention.
[0030] Figure 1 In Example 1 of the present invention, A is a scanning electron microscope image of the prepared sample, and B is an XRD pattern of the sample.
[0031] Figure 2 The scanning electron microscope images of the samples prepared in Example 2 of the present invention are shown in Figure 1. A is a morphology image of the product with a KMnO4 concentration of 1 mmol; B is a morphology image of the product with a KMnO4 concentration of 2 mmol; and C is a morphology image of the product with a KMnO4 concentration of 4 mmol.
[0032] Figure 3 The scanning electron microscope images of the samples prepared in Example 3 of the present invention are shown in Figure 1. A is the morphology of the product obtained when the manganese salt is manganese acetate; B is the morphology of the product obtained when the manganese salt is manganese sulfate; and C is the morphology of the product obtained when the manganese salt is manganese chloride.
[0033] Figure 4 This is a scanning electron microscope image of the sample prepared in Example 4 of the present invention.
[0034] Figure 5The scanning electron microscope images of the samples prepared in Example 5 of the present invention are shown in FIG. A is the morphology of the material after 6 hours of reaction; B is the morphology of the material after 12 hours of reaction; C is the morphology of the material after 18 hours of reaction; and D is the morphology of the material after 24 hours of reaction.
[0035] Figure 6 This is a scanning electron microscope image of the sample prepared in Example 6 of the present invention. A is the morphology of the material when the reaction temperature is 125°C; B is the morphology of the material when the reaction temperature is 180°C.
[0036] Figure 7 LSV curves of electrocatalytic ORR (A) and OER (B) of the samples prepared in Examples 1 and 2 of the present invention.
[0037] Figure 8 The charge and discharge cycle curve of the sample prepared in Example 1 of the present invention in a rechargeable zinc-air battery. DETAILED DESCRIPTION
[0038] It should be noted that the following detailed descriptions are illustrative and intended to provide further explanation of the present invention. Unless otherwise specified, all technical and scientific terms used in the present invention have the same meanings as those commonly understood by those skilled in the art to which the present invention belongs.
[0039] The present invention will be further described in detail below in conjunction with specific embodiments. It should be noted that the specific embodiments are intended to explain the present invention rather than to limit it.
[0040] Example 1 : This embodiment provides a method for preparing a broccoli-shaped MnWO4 electrocatalyst.
[0041] S1. Dissolve 3mmol KMnO4 and 0.04mmol silicotungstic acid in 40ml water and stir to form a transparent solution A;
[0042] S2, dissolve 2mmol H3BTC in 20ml ethanol and stir to form a transparent solution B;
[0043] S3, mixing solution A and solution B under stirring conditions, stirring for 1 hour, and then transferring the mixture into an autoclave to react at 150°C for 18 hours; after the reaction is completed, collecting the precipitate, washing it with deionized water and ethanol, and then drying it in a vacuum drying oven;
[0044] S4. The product is placed in a vacuum tube furnace and calcined at 800°C to obtain broccoli-shaped MnWO4 with high catalytic activity.
[0045] Figure 1 (A) is a scanning electron microscope image of the sample prepared in Example 1. It can be seen from the figure that the broccoli-like material was successfully synthesized in this example, with a regular and beautiful morphology and a porous and rough surface; Figure 1 (B) is the XRD pattern of the prepared sample. When the pattern is compared with the standard XRD card of MnWO4, it is found that the characteristic peaks appear at the corresponding positions and the peaks are clear, proving that the prepared material is MnWO4.
[0046] Example 2
[0047] The difference from Example 1 is that the concentration of KMnO4 in step S1 is changed to 1 mmol, 2 mmol, and 4 mmol respectively, and the other steps remain unchanged.
[0048] Figure 2 This is a scanning electron microscope image of the sample prepared in Example 2. It can be seen from the figure that the material morphology can be changed by changing the concentration of manganese salt: when the concentration of KMnO4 is 1mmol, the broccoli morphology cannot be formed; when the concentration of KMnO4 is 2mmol, the broccoli morphology begins to appear; when the concentration of KMnO4 continues to increase to 4mmol, the broccoli morphology disappears again, and it can be seen that the terminal tube becomes fibrous, and the original cluster structure can be vaguely seen.
[0049] Example 3
[0050] The difference from Example 1 is that the manganese salt described in step S1 is Mn(Ac)2, MnSO4, MnCl2, etc., and the other steps remain unchanged.
[0051] Figure 3 This is a scanning electron microscope image of the sample prepared in Example 3. It can be seen from the figure that when the manganese salt is manganese acetate, a rod-like structure is formed; when the manganese salt is manganese sulfate and manganese chloride, a broccoli morphology appears.
[0052] Example 4
[0053] The difference from Example 1 is that the polyoxometalate described in step S1 is phosphotungstic acid, and the other steps remain unchanged.
[0054] Figure 4 This is a scanning electron microscope image of the sample prepared in Example 4. As can be seen from the figure, when the polyoxometalate is phosphotungstic acid, the morphology of the product changes to a certain extent, but the morphology of broccoli can still be maintained.
[0055] Example 5
[0056] The difference from Example 1 is that the solvent thermal reaction time in step S3 is changed to 6 h, 12 h, 18 h, and 30 h respectively, and the other steps remain unchanged.
[0057] Figure 5The scanning electron microscope image of the sample prepared in Example 5. It can be seen from the figure that the material morphology can be affected by changing the reaction time and the growth process of the material can be found: in A, when the reaction time is 6 hours, broccoli stems appear, but the end does not form a capillary structure, and it is still in a cluster; in B, when the reaction time is 12 hours, it is already relatively clear, and a capillary structure is formed at the end; in C, when the reaction time is 18 hours, the broccoli-like structure is relatively complete, and a pore structure appears on the surface; in D, when the reaction time is 30 hours, the capillary structure at the end of the broccoli-like structure is clear, but due to the long reaction time, the end capillary is partially broken.
[0058] Example 6
[0059] The difference from Example 1 is that the solvent thermal reaction temperature in step S3 is changed to 125° C. and 180° C. respectively, and the other steps remain unchanged.
[0060] Figure 6 This is a scanning electron microscope image of the sample prepared in Example 6. It can be seen from the figure that temperature has a great influence on the material morphology: when the synthesis temperature is 125°C, the material is a rod-like structure and does not form a broccoli morphology; when the synthesis temperature is increased to 180°C, the broccoli-like morphology begins to be destroyed, and the amount of solvent in the synthesis process needs to be considered.
[0061] Example 7
[0062] The material prepared in Example 1 was used for electrochemical catalysis of ORR and OER reactions.
[0063] The tests were carried out in a three-electrode system of a CHI760E electrochemical workstation (Shanghai Zhenhua Instrument Co., Ltd.), with a rotating disk electrode (RDE) or rotating ring disk electrode (RRDE), a silver / silver chloride electrode (3 M KCl), and a platinum coil as the working electrode, reference electrode, and counter electrode in alkaline electrolyte, respectively.
[0064] The working electrode was prepared by first dispersing 2.0 mg of the catalyst in 985 μL of ethanol, then adding 15 μL of Nafion solution (5.0 wt%) and ultrasonicating for 0.5 h to form a relatively uniform suspension. Then 28.0 μL of the catalyst ink was added to the glassy carbon disk electrode, so that the effective loading mass on the glassy carbon electrode was ∼0.3 mg cm -2 The Pt / C and IrO2 test electrodes were prepared in the same way. The ORR and OER performances were tested by linear scanning polarization curves in 0.1M KOH and 1M KOH solutions.
[0065] from Figure 7It can be seen that the catalytic performance of the material obtained in Example 2 in catalyzing ORR and OER performance curves is relatively high, but there is a gap in performance between different samples. Among them, the material prepared in Example 1 (blue curve) has the highest performance in catalyzing ORR and OER reactions.
[0066] Example 8
[0067] Liquid zinc-air batteries were assembled to test battery performance. The catalyst ink was prepared in the same manner as in Example 7. The catalyst ink was evenly drop-coated on the gas diffusion layer (GDL) carbon paper. The catalyst loading was 1 mg cm -2 The battery was tested as the negative electrode, and the positive electrode was a polished Zn sheet. The reaction area of the two electrodes was 1cm 2 The electrolyte is a mixed solution of 6M KOH and 0.2M Zn(OAc)2. During the test, the electrolyte is slowly pumped into the battery by a peristaltic pump and circulated continuously. The blue electric test system is used to test the battery at 5mA cm -2 The charge and discharge test was carried out at a current of 20 minutes per cycle to test the charge and discharge performance of the material.
[0068] Figure 8 The material prepared in Example 1 still maintains its performance after more than 1500 cycles of charge and discharge in a reversible zinc-air battery, proving that the catalyst has superb stability.
[0069] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a broccoli-shaped MnWO4 electrocatalyst, comprising the following steps: S1, dissolving a manganese salt and a polyoxometalate in deionized water to form a solution A; S2, the linker is dissolved in an organic solvent to form a solution B; S3, mixing solution A and solution B, performing a solvothermal reaction, and preparing a MnWO4 precursor; S4. calcining MnWO4 to obtain broccoli-shaped MnWO4.
2. The preparation method according to claim 1, characterized in that The molar ratio of the manganese salt, the polyoxometalate, and the linker is 2-3.5:0.02-0.05:1.5-2.5; Preferably, the molar ratio of the manganese salt, the polyoxometalate and the linker is 3:0.04:
2.
3. The preparation method according to claim 1, characterized in that: In step S1, the manganese salt is selected from one or more of MnSO4, MnCl2, KMnO4, and Mn(Ac)2.
4. The preparation method according to claim 1, characterized in that: In step S1, the polyoxometalate is selected from silicotungstic acid or phosphotungstic acid and other simple tungstate-based polyoxometalates.
5. The preparation method according to claim 1, characterized in that: In step S2, the linking agent is trimesic acid; the organic solvent is selected from one or more of methanol, ethanol, and ethylene glycol; preferably, the organic solvent is ethanol.
6. The preparation method according to claim 1, characterized in that: In step S3, the reaction temperature is 125-180°C and the reaction time is 6h-30h; The product after the solvothermal reaction is washed with deionized water and ethanol, and then dried in a vacuum drying oven.
7. The preparation method according to claim 1, characterized in that: In step S4, the calcination temperature is between 600 and 800°C.
8. The preparation method according to claim 1, characterized in that: In step S4, the calcination is performed in an inert atmosphere, and the inert atmosphere is one or a combination of hydrogen, nitrogen, and argon.
9. A broccoli-shaped MnWO4 electrocatalyst, characterized in that The method is obtained by the preparation method according to any one of claims 1 to 8.
10. Use of the broccoli-shaped MnWO4 electrocatalyst as claimed in claim 1 in preparing a reversible zinc-air battery.