Preparation method of double-layer carbon paper

By modifying carbon fibers with an alkali lignin-urea alkaline solution and combining it with a wet papermaking process to prepare double-layer carbon paper, the problem of poor interlayer bonding was solved, and the high air permeability and strength were improved. This improved the performance of the gas diffusion layer and increased the energy conversion efficiency.

CN118943391APending Publication Date: 2024-11-12ZHEJIANG UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411333472.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-24
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The bonding effect between the layers of existing multilayer carbon paper is not ideal, which affects air permeability and tensile strength.

Method used

Carbon fibers were modified using an alkali lignin-urea alkaline solution system, and double-layer carbon paper was prepared using a wet papermaking process. First, wet paper webs were stacked and rotated together, and then impregnated, dried, and hot-pressed to form a double-layer carbon paper with excellent bonding ability.

Benefits of technology

It improves the interlayer bonding effect of carbon paper, enhances tensile strength, while maintaining good air permeability and conductivity, improves the application performance of gas diffusion layer, and improves the efficiency of energy conversion system.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118943391A_ABST
    Figure CN118943391A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of double-layer carbon paper. The preparation method comprises the following steps: step 1, respectively obtaining 2-4mm carbon fibers and 6-8mm carbon fibers; 2, alkali lignin and urea are added into a NaOH solution with the concentration of 0.5 mol / L to 1.5 mol / L, and dispersion liquid is formed; step 3, adding carbon fibers into the dispersion liquid for dispersion, and adding a proper amount of polyvinyl alcohol fibers to prepare a first carbon fiber slurry suspension and a second carbon fiber slurry suspension; 4, manufacturing a rectangular first wet paper web and a rectangular second wet paper web by adopting a wet papermaking process; 5, the first wet paper web and the second wet paper web are overlapped in a cross mode, then the first wet paper web is rotated till the first wet paper web and the second wet paper web coincide in the length direction, drying is conducted, and carbon paper base paper is obtained; and step 6, dipping, drying, hot-pressing and insulating the raw paper of the carbon paper to obtain a finished product of the double-layer carbon paper. The interlayer bonding effect of the double-layer carbon paper can be improved, the air permeability of the carbon paper is not affected, and the tensile strength of the carbon paper is enhanced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of carbon paper, and in particular to a method for preparing double-layer carbon paper. Background Art

[0002] The proton exchange membrane fuel cell is a device that directly converts chemical energy into electrical energy. Its anode cannot be over-dried to affect the transport of hydrogen, and the cathode should maintain appropriate humidity to avoid affecting the efficiency of the proton exchange membrane and the diffusion of oxygen. The gas diffusion layer is an important component located between the PEMFC bipolar plate and the catalyst layer, and is usually modified to improve its water management ability. Carbon paper is the main macroporous gas diffusion backing used in GDL, which plays an important role in strength support, gas transport and water discharge. At present, studies have explored the way to combine multi-layer carbon paper. If this multi-layer carbon paper is generally made by wet papermaking method to make paper from carbon fiber suspensions of different lengths to obtain carbonized fiber base paper of different fiber lengths, and then the base paper is stacked in sequence according to the fiber length, with 2-5 layers. However, if the number of layers of this multi-layer carbon paper is more, the bonding effect between the layers is not ideal, and the air permeability is affected at the same time. When the number of layers is small, the tensile strength and other properties of the carbon paper will be affected. Summary of the invention

[0003] The purpose of the present invention is to provide a method for preparing double-layer carbon paper, which can improve the interlayer bonding effect of the double-layer carbon paper without affecting the air permeability of the carbon paper and enhance the tensile strength of the carbon paper.

[0004] The technical solution of the present invention is a method for preparing a double-layer carbon paper, comprising the following steps:

[0005] Step 1, respectively obtain 2-4 mm carbon fiber and 6-8 mm carbon fiber;

[0006] Step 2, adding alkali lignin and urea to a 0.5-1.5 mol / L NaOH solution to form a dispersion; wherein the concentration of alkali lignin in the dispersion is 1-2 wt%, and the concentration of urea is 3-8 wt%;

[0007] Step 3, adding 2-4 mm carbon fiber and 6-8 mm carbon fiber into the dispersion respectively for dispersion, and adding an appropriate amount of polyvinyl alcohol fiber to obtain a first carbon fiber slurry suspension and a second carbon fiber slurry suspension;

[0008] Step 4: using a wet papermaking process to respectively form a first rectangular wet paper web and a second rectangular wet paper web from the first carbon fiber slurry suspension and the second carbon fiber slurry suspension;

[0009] Step 5, stacking the first wet paper web and the second wet paper web in a cross pattern, then rotating the first wet paper web until it overlaps with the second wet paper web in the length direction, and drying to obtain a carbon paper base;

[0010] Step 6: impregnate, dry, hot-press and heat-insulate the carbon paper base paper to obtain a double-layer carbon paper finished product.

[0011] In the above-mentioned method for preparing double-layer carbon paper, in step 2, the concentration of the NaOH solution is 1 mol / L, the concentration of the alkali lignin in the dispersion is 1.5 wt %, and the concentration of urea is 5 wt %.

[0012] In the aforementioned method for preparing double-layer carbon paper, in step 2, the dispersion is prepared by first adding alkali lignin to a NaOH solution to form a mixed solution, then heating the mixed solution to 60-70° C., and then adding urea to the mixed solution.

[0013] In the above-mentioned method for preparing double-layer carbon paper, in step 3, the dispersion liquid is heated to 80-100° C., and then the carbon fibers are added to the cellulose suspension and stirred, and ultrasonic stirring is performed for 1-3 minutes to complete the dispersion of the carbon fibers.

[0014] In the preparation method of the aforementioned double-layer carbon paper, in step 3, the wet papermaking process is to pour the first carbon fiber slurry suspension and the second carbon fiber slurry suspension into the paper sheet former respectively, add excess NaOH, bubble homogenize for 5 minutes, and then open the water valve to allow the carbon fiber to settle freely on the copper mesh to form the first wet paper web and the second wet paper web respectively.

[0015] In the aforementioned method for preparing double-layer carbon paper, in step 4, the rotation angle of the first wet paper web is 270°.

[0016] In the aforementioned method for preparing double-layer carbon paper, in step 5, the drying temperature is 150° C. and the drying pressure is 1 MPa.

[0017] The aforementioned method for preparing double-layer carbon paper, wherein the impregnation, drying, hot pressing and heat preservation of the carbon paper base paper specifically comprises:

[0018] The carbon paper base was immersed in a 10wt% phenolic resin solution for 30 minutes, and then placed in a room for drying, and then moved into a blast drying oven for drying at 80°C for 40 minutes. Subsequently, the carbon paper base was placed on a flat vulcanizer and hot pressed at 150°C and 10MPa for 40 minutes. Finally, the base paper was placed in an atmosphere furnace, nitrogen was introduced for protection, the temperature was raised to 1500°C at a rate of 30°C / min, and the temperature was kept for 30 minutes to obtain a double-layer carbon paper product.

[0019] In the aforementioned method for preparing double-layer carbon paper, in step 1, the lengths of the carbon fibers are selected to be 4 mm and 6 mm respectively.

[0020] Compared with the prior art, the present invention first configures an alkaline solution of alkali lignin, and then adds urea to form an alkali lignin-urea alkaline solution system. Under this system, the active groups of alkali lignin are used to modify the carbon fibers, thereby increasing the surface hydrophilic groups and the surface roughness structure. At the same time, under the action of heating and ultrasonic stirring, the viscosity of the alkali lignin-urea alkaline solution system increases with the increase in temperature, thereby limiting the mutual connection of the carbon fibers, reducing the interaction force between the carbon fibers, and reducing the internal friction between the carbon fibers, thereby achieving rapid dispersion of the carbon fibers under the influence of multiple factors. Based on this dispersion ability, the present application selects 2-4mm carbon fiber and 6-8mm carbon fiber as the raw materials for double-layer carbon paper. First, a first wet paper web and a second wet paper web are prepared. Then, the first wet paper web and the second wet paper web are superimposed and rotated to overlap, so that the layers of the wet paper web can be intertwined with each other and can achieve good bonding between the layers. Finally, they are impregnated and hot-pressed to obtain a double-layer carbon paper with excellent bonding ability. The double-layer carbon paper is combined and stacked together longitudinally, and has differentiated pore characteristics between different layers. The Bernoulli effect can be better utilized, which can effectively improve the application performance of the gas diffusion layer and improve the efficiency of the energy conversion system. At the same time, the modification of the carbon fiber and the layer bonding method make it have good mechanical properties and conductivity. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 Schematic diagram of the photos of double-layer carbon paper prepared in the embodiment and the comparative example;

[0022] Figure 2 It is a 400 times SEM schematic diagram of the double-layer carbon paper prepared in the embodiment and the comparative example;

[0023] Figure 3 It is a 2500 times SEM schematic diagram of the double-layer carbon paper prepared in the embodiment and the comparative example. DETAILED DESCRIPTION

[0024] The present invention is further described below in conjunction with the accompanying drawings and embodiments, but they are not intended to limit the present invention.

[0025] Embodiment 1: A method for preparing a double-layer carbon paper, comprising the following steps:

[0026] Step 1, obtain 2g of 2mm carbon fiber and 2g of 6mm carbon fiber respectively;

[0027] Step 2, adding alkali lignin to a 0.75 mol / L NaOH solution to form a mixed solution, then heating the mixed solution to 60° C., and then adding urea to the mixed solution to form a dispersion; wherein the concentration of alkali lignin in the dispersion is 1 wt%, and the concentration of urea is 3 wt%;

[0028] Step 3, adding 2 mm carbon fiber and 6 mm carbon fiber into the dispersion respectively for dispersion, heating the dispersion to 80° C., ultrasonically stirring for 2 minutes, and then adding 2 g of polyvinyl alcohol fiber to obtain a first carbon fiber slurry suspension and a second carbon fiber slurry suspension;

[0029] Step 4: using a wet papermaking process, the first carbon fiber slurry suspension and the second carbon fiber slurry suspension are respectively poured into a paper sheet former, after adding an excess of NaOH, the bubbles are homogenized for 5 minutes, and then the drain valve is opened to allow the carbon fibers to settle freely on the copper mesh to form a first wet paper web and a second wet paper web respectively;

[0030] Step 5, the first wet paper web and the second wet paper web are firstly superimposed in a cross manner, and then the first wet paper web is rotated 270 degrees to make the first wet paper web and the second wet paper web overlap in the length direction, and then dried at a temperature of 150° C. and a pressure of 1 MPa to obtain a carbon paper base paper;

[0031] Step 6: soak the carbon paper base in a 10wt% phenolic resin solution for 30 minutes, then place it in a room to dry, and then move it into a forced air drying oven to dry it at 80°C for 40 minutes. Then, place the carbon paper base on a flat vulcanizer and hot press it at 150°C and 10MPa for 40 minutes. Finally, place the base paper in an atmosphere furnace, introduce nitrogen for protection, heat it to 1500°C at a rate of 30°C / min, and keep it warm for 30 minutes to obtain a double-layer carbon paper product.

[0032] Embodiment 2: A method for preparing a double-layer carbon paper, comprising the following steps:

[0033] Step 1, obtain 2g of 2mm carbon fiber and 2g of 8mm carbon fiber respectively;

[0034] Step 2, adding alkali lignin to a 1.25 mol / L NaOH solution to form a mixed solution, then heating the mixed solution to 65° C., and then adding urea to the mixed solution to form a dispersion; wherein the concentration of alkali lignin in the dispersion is 2 wt %, and the concentration of urea is 6 wt %;

[0035] Step 3, adding 2 mm carbon fiber and 8 mm carbon fiber into the dispersion respectively for dispersion, heating the dispersion to 95° C., ultrasonically stirring for 1 minute, and then adding 2 g of polyvinyl alcohol fiber to obtain a first carbon fiber slurry suspension and a second carbon fiber slurry suspension;

[0036] Step 4: using a wet papermaking process, the first carbon fiber slurry suspension and the second carbon fiber slurry suspension are respectively poured into a paper sheet former, after adding an excess of NaOH, the bubbles are homogenized for 5 minutes, and then the drain valve is opened to allow the carbon fibers to settle freely on the copper mesh to form a first wet paper web and a second wet paper web respectively;

[0037] Step 5, the first wet paper web and the second wet paper web are firstly superimposed in a cross manner, and then the first wet paper web is rotated 270 degrees to make the first wet paper web and the second wet paper web overlap in the length direction, and then dried at a temperature of 150° C. and a pressure of 1 MPa to obtain a carbon paper base paper;

[0038] Step 6: soak the carbon paper base in a 10wt% phenolic resin solution for 30 minutes, then place it in a room to dry, and then move it into a forced air drying oven to dry it at 80°C for 40 minutes. Then, place the carbon paper base on a flat vulcanizer and hot press it at 150°C and 10MPa for 40 minutes. Finally, place the base paper in an atmosphere furnace, introduce nitrogen for protection, heat it to 1500°C at a rate of 30°C / min, and keep it warm for 30 minutes to obtain a double-layer carbon paper product.

[0039] Embodiment 3: A method for preparing a double-layer carbon paper, comprising the following steps:

[0040] Step 1, obtain 2g of 4mm carbon fiber and 2g of 8mm carbon fiber respectively;

[0041] Step 2, adding alkali lignin to a 0.5 mol / L NaOH solution to form a mixed solution, then heating the mixed solution to 70° C., and then adding urea to the mixed solution to form a dispersion; wherein the concentration of alkali lignin in the dispersion is 2 wt%, and the concentration of urea is 8 wt%;

[0042] Step 3, adding 4 mm carbon fiber and 8 mm carbon fiber into the dispersion respectively for dispersion, heating the dispersion to 100° C., ultrasonically stirring for 2 minutes, and then adding 2 g of polyvinyl alcohol fiber to obtain a first carbon fiber slurry suspension and a second carbon fiber slurry suspension;

[0043] Step 4: using a wet papermaking process, the first carbon fiber slurry suspension and the second carbon fiber slurry suspension are respectively poured into a paper sheet former, after adding an excess of NaOH, the bubbles are homogenized for 5 minutes, and then the drain valve is opened to allow the carbon fibers to settle freely on the copper mesh to form a first wet paper web and a second wet paper web respectively;

[0044] Step 5, the first wet paper web and the second wet paper web are firstly superimposed in a cross manner, and then the first wet paper web is rotated 270 degrees to make the first wet paper web and the second wet paper web overlap in the length direction, and then dried at a temperature of 150° C. and a pressure of 1 MPa to obtain a carbon paper base paper;

[0045] Step 6: soak the carbon paper base in a 10wt% phenolic resin solution for 30 minutes, then place it in a room to dry, and then move it into a forced air drying oven to dry it at 80°C for 40 minutes. Then, place the carbon paper base on a flat vulcanizer and hot press it at 150°C and 10MPa for 40 minutes. Finally, place the base paper in an atmosphere furnace, introduce nitrogen for protection, heat it to 1500°C at a rate of 30°C / min, and keep it warm for 30 minutes to obtain a double-layer carbon paper product.

[0046] Embodiment 4: A method for preparing a double-layer carbon paper, comprising the following steps:

[0047] Step 1, obtain 2g of 4mm carbon fiber and 2g of 6mm carbon fiber respectively;

[0048] Step 2, adding alkali lignin to a 1 mol / L NaOH solution to form a mixed solution, then heating the mixed solution to 65° C., and then adding urea to the mixed solution to form a dispersion; wherein the concentration of alkali lignin in the dispersion is 1.5 wt %, and the concentration of urea is 5 wt %;

[0049] Step 3, adding 4 mm carbon fiber and 6 mm carbon fiber into the dispersion respectively for dispersion, heating the dispersion to 90° C., ultrasonically stirring for 2 minutes, and then adding 2 g of polyvinyl alcohol fiber to obtain a first carbon fiber slurry suspension and a second carbon fiber slurry suspension;

[0050] Step 4: using a wet papermaking process, the first carbon fiber slurry suspension and the second carbon fiber slurry suspension are respectively poured into a paper sheet former, after adding an excess of NaOH, the bubbles are homogenized for 5 minutes, and then the drain valve is opened to allow the carbon fibers to settle freely on the copper mesh to form a first wet paper web and a second wet paper web respectively;

[0051] Step 5, the first wet paper web and the second wet paper web are firstly superimposed in a cross manner, and then the first wet paper web is rotated 270 degrees to make the first wet paper web and the second wet paper web overlap in the length direction, and then dried at a temperature of 150° C. and a pressure of 1 MPa to obtain a carbon paper base paper;

[0052] Step 6: soak the carbon paper base in a 10wt% phenolic resin solution for 30 minutes, then place it in a room to dry, and then move it into a forced air drying oven to dry it at 80°C for 40 minutes. Then, place the carbon paper base on a flat vulcanizer and hot press it at 150°C and 10MPa for 40 minutes. Finally, place the base paper in an atmosphere furnace, introduce nitrogen for protection, heat it to 1500°C at a rate of 30°C / min, and keep it warm for 30 minutes to obtain a double-layer carbon paper product.

[0053] Comparative Example 1: Preparation method of double-layer carbon paper in the current laboratory:

[0054] First, the carbon fiber was surface pretreated, and 2g of 2mm carbon fiber, 4mm carbon fiber, 8mm carbon fiber and polyvinyl alcohol fiber were weighed. 1L of deionized water was taken, and an appropriate amount of Carbomer was slowly added while stirring. The stirring was continued until the Carbomer was completely dissolved to prepare a 0.5wt% Carbomer solution. Then, the carbon fiber was added to the Carbomer solution and the polyvinyl alcohol fiber was added. Finally, an appropriate amount of NaOH was added to thicken the slurry;

[0055] Through the laboratory wet papermaking process, the dispersed carbon fiber is made into a wet paper web. The specific process is as follows: Pour the carbon fiber slurry suspension into the paper sheet former, add excess NaOH, and bubble homogenize for 2 minutes to evenly disperse the carbon fiber slurry. Open the waterproof valve to allow the carbon fiber to settle freely on the copper mesh to form a wet paper web; stack multiple wet paper webs according to Table 1, and then place them on a flat vulcanizer, dry them at 150°C and 1MPa, peel them off to obtain carbon paper base paper, and after the paper sheet is formed, use filter paper to absorb the surface moisture, and then transfer to a flat vulcanizer, dry them at 150°C and 1MPa, and obtain base paper after drying.

[0056] Finally, the base paper was immersed in a 10wt% phenolic resin solution for 30 minutes, and then placed in a room for drying, and then moved into a blast drying oven for drying at 80°C for 40 minutes. Subsequently, the base paper was placed on a flat vulcanizer and hot pressed at 150°C and 10MPa for 40 minutes. Finally, the base paper was placed in an atmosphere furnace, nitrogen was introduced for protection, the temperature was raised to 1500°C at a rate of 30°C / min, and the temperature was kept for 30 minutes to obtain carbon paper.

[0057] In order to meet the complex mass transfer requirements of the gas diffusion layer in the proton exchange membrane fuel cell, several key properties of carbon paper need to be considered: porosity, thickness, conductivity, air permeability, and tensile strength. Therefore, the present invention characterizes the performance of the carbon paper prepared in the examples and comparative examples.

[0058] 1. Cut the samples of Examples 3-4 and the comparative example to appropriate sizes, adhere them to the sample table, and mark them. Then place the sample table in the spraying equipment for spraying. Take out the sample table, place it under a desktop scanning electron microscope (SEM), and adjust the clarity. Finally, select a suitable position and appropriate magnification to take pictures of the carbon paper. First, at the macro level, the surface of the carbon paper can show different textures and patterns. Figure 1 As shown. At the microscopic level, the material structure of carbon paper is similar to a nanostructure composed of carbon fibers and carbide crystallites of varying sizes. These microstructures present different morphologies and arrangements, and have a high degree of order and various physical properties in the vertical and horizontal directions, as shown below Figure 2 and Figure 3 As shown. Figure 2 and Figure 3 It can be seen that the carbon fiber and the polyvinyl alcohol fiber of Examples 3 and 4 are tightly bonded, and the bonding between the layers and between the layers in the multilayer gradient carbon paper is relatively close. However, it can be seen from the comparative example that the bonding between the carbon fiber and the polyvinyl alcohol fiber is slightly inferior to that of the present application.

[0059] 2. Calculate the porosity of the samples of Examples 3-4 and the comparative example. In this experiment, the following four groups of double-layer carbon papers were designed using the comparative example method:

[0060] Length and amount of the first layer of carbon fiber Second layer of carbon fiber length and amount Combination method 2mm carbon fiber 2g 6mm carbon fiber 2g Wet paper stacking 2mm carbon fiber 2g 8mm carbon fiber 2g Wet paper stacking 4mm carbon fiber 2g 8mm carbon fiber 2g Wet paper stacking 4mm carbon fiber 2g 6mm carbon fiber 2g Wet paper stacking

[0061] Table 1

[0062] The porosity is calculated by using an electronic balance to weigh the mass of the carbon paper base or the carbon paper before and after being impregnated with anhydrous ethanol, and using the drainage method to calculate the porosity of the sample according to the following formula:

[0063]

[0064] Where W 2 is the mass after immersion in anhydrous ethanol, W 1 is the mass before immersion in anhydrous ethanol, ρ 2 is the density of anhydrous ethanol, ρ 1 It is the average density of carbon paper base or carbon paper.

[0065] The results are shown in Table 2 below:

[0066] sample Porosity / % 2mm vs. 6mm 91.27 2mm vs. 8mm 91.18 4mm vs. 8mm 91.46 4mm vs. 6mm 92.65 Example 1 94.54 Example 2 95.75 Example 3 96.12 Example 4 96.86

[0067] Table 2

[0068] It can be seen from Table 2 that the double-layer carbon paper product prepared by the present invention has better porosity.

[0069] Furthermore, the above samples were tested for conductivity, and the resistivity was determined using an RTS-8 four-probe tester. First, estimate the resistivity range of the sample based on its size and select the corresponding range. Place the sample, press the probe, and connect the sample to the current. Calculate the required test resistivity based on the sample size and instrument parameters, and adjust the potentiometer to the host display required test current. Then adjust the mode so that the host displays the test results. Test at least 9 points for each sample, measure and take the average value, which is the resistivity of the sample. The reciprocal of the resistivity is the conductivity. The results are shown in Table 3 below:

[0070]

[0071]

[0072] Table 3

[0073] It can be seen from Table 3 that the double-layer carbon paper product prepared by the present invention has better conductivity.

[0074] Furthermore, the air permeability of the above samples was tested using an FX3000 air permeability tester to measure the air permeability of the carbon paper and the carbon paper base. The double-sided carbon paper was placed on the stage of the air permeability tester, and the test area was selected to be 20 cm 2 , select 200Pa as the test pressure, and measure according to the instrument usage method. After the instrument reading remains stable, record the data. Test the air permeability of at least 5 points of each sample, and take the average value to obtain the air permeability of the sample. The results are shown in Table 4 below:

[0075] sample <![CDATA[Average air permeability / L·m -2 ·s -1 > 2mm vs. 6mm 814 2mm vs. 8mm 1131 4mm vs. 8mm 998 4mm vs. 6mm 1132 Example 1 1321 Example 2 1418 Example 3 1487 Example 4 1515

[0076] Table 4

[0077] It can be seen from Table 2 that the double-layer carbon paper product prepared by the present invention has better air permeability.

[0078] Furthermore, the tensile strength of the above samples was tested, and the tensile strength of the carbon paper base paper and the carbon paper was measured using a horizontal computer tensile tester. The sample was cut into a paper strip with a width of 15 mm, and the two sides were clamped with the fixture of the instrument and tension was gradually applied until the sample broke to obtain its tensile strength. Each group of samples was tested for tensile strength at least nine locations, and the average value was calculated, which was the tensile strength of the sample. The results are shown in Table 5.

[0079] sample <![CDATA[Average Tensile Strength / kN·m -1 > 2mm vs. 6mm 0.242 2mm vs. 8mm 0.306 4mm vs. 8mm 0.394 4mm vs. 6mm 0.384 Example 1 0.452 Example 2 0.467 Example 3 0.484 Example 4 0.492

[0080] Table 5

[0081] It can be seen from Table 5 that the double-layer carbon paper product prepared by the present invention has better tensile strength.

[0082] In summary, the present invention first configures an alkaline solution of alkali lignin, and then adds urea to form an alkali lignin-urea alkaline solution system. Under this system, the active groups of alkali lignin are used to modify the carbon fibers, thereby increasing the surface hydrophilic groups and the surface roughness structure. At the same time, under the action of heating and ultrasonic stirring, the viscosity of the alkali lignin-urea alkaline solution system increases with the increase in temperature, thereby limiting the mutual connection of the carbon fibers, reducing the interaction force between the carbon fibers, and reducing the internal friction between the carbon fibers, thereby achieving rapid dispersion of the carbon fibers under the influence of multiple factors. Based on this dispersion ability, the present application selects 2-4mm carbon fiber and 6-8mm carbon fiber as the raw materials for double-layer carbon paper. First, a first wet paper web and a second wet paper web are prepared. Then, the first wet paper web and the second wet paper web are superimposed and rotated to overlap, so that the layers of the wet paper web can be intertwined and achieve good bonding between the layers. Finally, they are impregnated and hot-pressed to obtain a double-layer carbon paper with excellent bonding ability. The double-layer carbon paper is combined and stacked together longitudinally, and has differentiated pore characteristics between different layers. The Bernoulli effect can be better utilized, which can effectively improve the application performance of the gas diffusion layer and improve the efficiency of the energy conversion system. At the same time, the modification of the carbon fiber and the layer bonding method make it have good mechanical properties and conductivity.

Claims

1. A method for preparing a double-layer carbon paper, characterized in that: The steps include: Step 1, respectively obtain 2-4 mm carbon fiber and 6-8 mm carbon fiber; Step 2, adding alkali lignin and urea to a 0.5-1.5 mol / L NaOH solution to form a dispersion; wherein the concentration of alkali lignin in the dispersion is 1-2 wt%, and the concentration of urea is 3-8 wt%; Step 3, adding 2-4 mm carbon fiber and 6-8 mm carbon fiber into the dispersion respectively for dispersion, and adding an appropriate amount of polyvinyl alcohol fiber to obtain a first carbon fiber slurry suspension and a second carbon fiber slurry suspension; Step 4: using a wet papermaking process to respectively form a first rectangular wet paper web and a second rectangular wet paper web from the first carbon fiber slurry suspension and the second carbon fiber slurry suspension; Step 5, stacking the first wet paper web and the second wet paper web in a cross pattern, then rotating the first wet paper web until it overlaps with the second wet paper web in the length direction, and drying to obtain a carbon paper base; Step 6: impregnate, dry, hot-press and heat-insulate the carbon paper base paper to obtain a double-layer carbon paper finished product.

2. The method for preparing double-layer carbon paper according to claim 1, characterized in that: In step 2, the concentration of the NaOH solution is 1 mol / L, the concentration of the alkali lignin in the dispersion is 1.5 wt %, and the concentration of urea is 5 wt %.

3. The method for preparing double-layer carbon paper according to claim 1, characterized in that: In step 2, the dispersion is prepared by first adding alkali lignin to a NaOH solution to form a mixed solution, then heating the mixed solution to 60-70° C., and then adding urea to the mixed solution.

4. The method for preparing double-layer carbon paper according to claim 1, characterized in that: In step 3, the dispersion liquid is heated to 80-100° C., and then the carbon fibers are added to the cellulose suspension and stirred, and ultrasonic stirring is performed for 1-3 minutes to complete the dispersion of the carbon fibers.

5. The method for preparing double-layer carbon paper according to claim 1, characterized in that: In step 3, the wet papermaking process is to pour the first carbon fiber slurry suspension and the second carbon fiber slurry suspension into the paper sheet former respectively, add excess NaOH, bubble homogenize for 5 minutes, and then open the water valve to allow the carbon fiber to settle freely on the copper mesh to form the first wet paper web and the second wet paper web respectively.

6. The method for preparing double-layer carbon paper according to claim 1, characterized in that: In step 4, the first wet paper web is rotated at an angle of 270°.

7. The method for preparing double-layer carbon paper according to claim 1, characterized in that: In step 5, the drying temperature is 150° C. and the drying pressure is 1 MPa.

8. The method for preparing double-layer carbon paper according to claim 1, characterized in that: The impregnation, drying, hot pressing and heat preservation of the carbon paper base paper specifically include: The carbon paper base was immersed in a 10wt% phenolic resin solution for 30 minutes, and then placed in a room for drying, and then moved into a blast drying oven for drying at 80°C for 40 minutes. Subsequently, the carbon paper base was placed on a flat vulcanizer and hot pressed at 150°C and 10MPa for 40 minutes. Finally, the base paper was placed in an atmosphere furnace, nitrogen was introduced for protection, the temperature was raised to 1500°C at a rate of 30°C / min, and the temperature was kept for 30 minutes to obtain a double-layer carbon paper product.