Fuel cell Pt / beta-Bi2O3 electrocatalyst and application thereof

The supported Pt/β-Bi2O3 nanoelectrocatalyst prepared by chemical precipitation and hydrothermal reaction methods solves the problem of insufficient catalytic activity and stability of the Pt catalyst during ethanol oxidation, and realizes the efficient ethanol oxidation performance of the catalyst, which is significantly better in commercial Pt/C catalysts.

CN118943399APending Publication Date: 2024-11-12CHINA THREE GORGES UNIV
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411129950.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The Pt catalysts in existing direct ethanol fuel cells have problems with insufficient catalytic activity and stability during the ethanol oxidation process, especially the agglomeration of Pt nanoparticles, resulting in a degradation of catalytic performance.

Method used

The supported Pt/β-Bi2O3 nanoelectrocatalyst was prepared by chemical precipitation, high-temperature calcination and hydrothermal reaction. P123 was used as a reducing agent and a protective agent, and the conditions were controlled to react at 180°C for 12 hours to form a Pt nanochain structure and Bi2O3. Combined, the active site exposure and structural stability of the catalyst are improved.

Benefits of technology

The catalytic performance and stability of the Pt catalyst were significantly improved, and the oxidative activity of ethanol was enhanced. The Pt:Bi atom ratio of the catalyst was 9:10-11, the Pt nanoparticles were uniformly distributed, the average particle size was about 4.49nm, and the support Bi2O3 The cross-sectional diameter is about 30 nm, and the specific active current density of the catalyst to ethanol oxidation reaches 2477.5 mA·mgPt-1, which is significantly better than that of commercial Pt/C catalysts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118943399A_ABST
    Figure CN118943399A_ABST
Patent Text Reader

Abstract

The invention provides a Pt / beta-Bi2O3 electrocatalyst for a fuel cell. The preparation method comprises the following steps: weighing P123, dissolving the P123 in a NaOH solution, carrying out ultrasonic stirring until the P123 is completely dissolved, dropwise adding a bismuth nitrate aqueous solution, and reacting to obtain monoclinic phase alpha-Bi2O3; the preparation method comprises the following steps: dropwise adding a bismuth nitrate aqueous solution into a P123 and Na2CO3 solution, and reacting to obtain beta-Bi2O3; the preparation method comprises the following steps: weighing P123 and Bi (NO3) 3.5 H2O, dissolving the P123 and Bi (NO3) 3.5 H2O in ethylene glycol, carrying out uniform ultrasonic dispersion, heating in a water bath to 70 DEG C, pouring a NaOH solution, standing, cooling to room temperature, washing and centrifuging with water and ethanol for three times respectively, and carrying out vacuum drying to obtain the cubic phase gamma-Bi2O3. And then carrying out hydrothermal reaction on P123, x-Bi2O3 (x = alpha, beta, gamma) and K2PtCl6 to obtain the fuel cell Pt / x-Bi2O3 (x = alpha, beta, gamma) electrocatalyst. The prepared catalyst has excellent electro-catalytic oxidation ethanol performance, Pt / beta-Bi2O3 shows the highest EOR performance (2477.5 mA. Mg <-1 > Pt) and good catalytic stability, and the catalyst has great application and development prospects in direct ethanol fuel cells.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of fuel cells and relates to a method for preparing an anode catalyst, in particular to a method for preparing a Pt / β-Bi2O3 electrocatalyst for a direct ethanol fuel cell. Background Art

[0002] Proton exchange membrane fuel cell (PEMFC) is a highly efficient conversion device that converts chemical energy stored in fuel into electrical energy. It does not go through a thermal engine process and is not limited by the Carnot cycle. It has a very high conversion efficiency and is rated as one of the most promising emerging energy conversion devices. As long as the raw materials are replenished, electrical energy can be continuously output to the external circuit. Direct ethanol fuel cell (DEFC) is a type of proton exchange membrane fuel cell. It has the advantages of simple structure, high theoretical specific density, low toxicity of fuel, safe and easy storage and transportation, etc. It can be obtained in large quantities only by organic fermentation containing sugars. It is a non-toxic, environmentally friendly and renewable fuel. Once successfully developed, it has a very broad prospect. Summary of the invention

[0003] In the present invention, by preparing a Pt / β-Bi2O3 nano-electrocatalyst with a supported Pt chain structure, the active sites exposed by the Pt nanoparticles are effectively increased, thereby improving the catalytic performance thereof. Bi2O3 has special properties such as high oxygen ion conductivity and significant band gap, which helps to effectively oxidize CO molecules and improve the anti-poisoning performance of Pt. Moreover, its structure is stable, which effectively supports the Pt nanoparticles and reduces the agglomeration phenomenon.

[0004] In the present invention, β-Bi2O3 is prepared by chemical precipitation and high-temperature calcination, and a supported Pt nanochain Pt / β-Bi2O3 electrocatalyst is prepared by hydrothermal reaction with P123 as a reducing agent and a protective agent at 180°C.

[0005] The purpose of the present invention is to improve the catalytic activity and stability of a Pt-based catalyst by controlling the result control, and to prepare a fuel cell Pt / β-Bi2O3 nano-electrocatalyst with excellent ethanol catalytic performance.

[0006] The technical solution adopted by the present invention to achieve the above-mentioned purpose is as follows: (1) Weigh P123 (PEO 19 -PPO 69 -PEO 19) and Na2CO3 are dissolved in deionized water (H2O) and ultrasonically dispersed until uniform. The solution is transferred to a beaker and bismuth nitrate (Bi(NO3)3) aqueous solution is added dropwise while magnetically stirring. A large amount of milky white precipitate (Bi2O2CO3) appears immediately. After the addition is completed, the supernatant is allowed to stand and separated. The white powder is washed three times by centrifugation in an ethanol aqueous solution and calcined in a muffle furnace at a high temperature. After the reaction is completed, it is ground in an agate mortar. The bright yellow powder obtained is tetragonal β-Bi2O3.

[0007] (2) P123, β-Bi2O3 and K2PtCl6 were dissolved in deionized water, ultrasonically stirred for 30 min, and then transferred into a polychlorofluoroethylene liner and placed in a reaction kettle. The reaction was carried out in a forced air drying oven at 180°C for 12 h. (3) After the reaction is completed, the heating is stopped, the mixture is naturally cooled to room temperature, and the mixture is centrifuged and washed 3 to 4 times with deionized water and anhydrous ethanol at 8000 to 10000 rpm / min, respectively, to obtain a fuel cell Pt / β-Bi2O3 electrocatalyst.

[0008] In the steps of the present invention, P123 is a reducing agent and a protective agent, and H2O is used as a solvent. During the centrifugal washing process, the catalyst is first washed with double distilled water for 3 to 4 times, and then washed with anhydrous ethanol for 3 to 4 times to ensure that the unreacted reactants and P123 are removed from the catalyst surface.

[0009] In the step (1), the mass ratio of P123, potassium chloroplatinite, and bismuth trioxide is 1: 0.01-0.02: 0.01-0.012. In some preferred cases, the mass ratio of P123, potassium chloroplatinite, and bismuth trioxide is 1: 0.02: 0.012.

[0010] In the step (1), the calcination condition is to increase the temperature to 350-450°C at a heating rate of 1-5°C / min and calcine for 2-4 hours. Preferably, the calcination condition is to increase the temperature to 380°C at a heating rate of 2°C / min and calcine for 2 hours.

[0011] In the step (2), the hydrothermal reaction conditions are 150-200° C. for 10-15 hours, preferably 180° C. for 12 hours.

[0012] In the electrocatalyst obtained by adopting the technical solution of the present invention, Pt is dispersed between Bi2O3 in a nanochain structure, the average particle size of Pt nanoparticles is about 4.49±0.03nm, and the cross-sectional diameter of the carrier Bi2O3 is about 30nm; the atomic ratio of Pt:Bi is about 9:10-11, of which Pt accounts for about 30-40% of the total mass of the catalyst.

[0013] The fuel cell Pt / β-Bi2O3 electrocatalyst has Pt nanoparticles evenly distributed among Bi2O3, and a small amount of Pt nanoparticles distributed around Bi2O3 in a chain structure. The cross-sectional diameter of Bi2O3 is about 30 nm. The specific active current density of the catalyst for ethanol oxidation is 2477.5 mA·mg Pt -1 .

[0014] The fuel cell Pt / β-Bi2O3 electrocatalyst reduces the agglomeration of Pt NPs, has a characteristic chain structure, and effectively improves the catalytic performance and stability of the Pt / β-Bi2O3 nano electrocatalyst.

[0015] The Pt / β-Bi2O3 electrocatalyst for fuel cells and the preparation method thereof involved in the present invention have the following significant features: (1) The preparation method is simple. The first step is to synthesize the carrier β-Bi2O3 particles; the second step is to reduce the Pt nanoparticles.

[0016] (2) P123 acts as both a reducing agent and a protective agent, and H2O is used as a solvent. No organic reagents or surfactants are used in the experiment, which is low-cost, green and pollution-free.

[0017] (3) The prepared catalyst has excellent electrocatalytic oxidation performance for ethanol and has great application and development prospects in direct ethanol fuel cells. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 X-ray diffraction analysis patterns of x-Bi2O3 (x=α, β, γ) prepared in Examples 1, 2, 3, and 4.

[0019] Figure 2 Transmission electron microscope image and elements of the fuel cell Pt / β-Bi2O3 electrocatalyst prepared in Example 1.

[0020] Element distribution diagram, where (a)-(c) are catalyst TEM images, the inset in c is the catalyst particle size distribution diagram, (d) and (e) are HRTEM images, and (f)-(j) are HAADF-STEM images; where g, h, i, j are the element maps and overlapping images of Pt, Bi, and O, respectively.

[0021] Figure 3 Cyclic voltammetry curves of the fuel cell electrocatalysts prepared in Examples 1, 2, 3, and 4 and the commercial Pt / C electrocatalytic oxidation of ethanol.

[0022] Figure 4 The chronoamperometric curves of the fuel cell electrocatalysts prepared in Examples 1, 2, 3, and 4 and the commercial Pt / C electrocatalytic oxidation of ethanol are shown.

[0023] Figure 5 This is a comparison chart of the fuel cell electrocatalysts prepared in Examples 1, 2, and 3 and commercial Pt / C electrocatalytic oxidation of ethanol for 200 cycles. DETAILED DESCRIPTION

[0024] The present invention will be further described below in conjunction with the accompanying drawings and specific implementation cases. It should be stated here that these implementation cases are only used to illustrate the present invention rather than to limit the scope of the present invention. After reading the present invention, modifications to various equivalent forms by those skilled in the art all fall within the scope defined by the claims attached to this application.

[0025] Example 1 (1) Weigh 1 g P123 and 6 g NaCO3 into a 500 mL beaker, add 180 mL H2O, and dissolve under ultrasonic stirring. Under magnetic stirring, slowly add 25 mL Bi(NO3)3 solution (1.2 g Bi(NO3)3•5 H2O dissolved in 25 mL 0.1M HNO3) using a constant pressure dropping funnel. Control the flow rate and complete the addition within 30 min. After standing, the bottom of the solution is filled with white flocculent precipitates. Centrifuge and dry to obtain white Bi2O2CO3 powder, which is then placed in a muffle furnace for reaction for 2 h at a reaction temperature of 380 °C and a heating rate of 2 °C / min. After the reaction is completed, grind in an agate mortar to obtain a bright yellow powder, which is tetragonal β-Bi2O3.

[0026] (2) Dissolve 1 g of P123 in 20 mL of H2O in a beaker and stir ultrasonically for 30 min to completely dissolve it. Add K2PtCl6 (20 mg) and β-Bi2O3 (12 mg) in a ratio of Pt:β-Bi2O3 = 1:4 with a Pt mass percentage of 40 wt%. Mix well with ultrasonic waves and transfer to a reactor. React in a forced air drying oven at 180 °C for 12 h.

[0027] (3) Cooling naturally to room temperature and keeping it still, the black turbid liquid obtained after the reaction was centrifuged at 10000 r / min, washed with deionized water for 4 times, and then washed with anhydrous ethanol solution for 4 times. Finally, the obtained product was dispersed and protected by adding anhydrous ethanol to obtain a fuel cell Pt / β-Bi2O3 electrocatalyst.

[0028] (4) The Pt / β-Bi2O3 electrocatalyst prepared in this example was modified on a glassy carbon electrode to prepare a working electrode, and cyclic voltammetry and chronoamperometry tests were performed on the electrode. The test conditions were: the solution was a nitrogen-saturated 1 mol / L KOH+1 mol / L EtOH solution, and the CV scanning range was -0.9-0.3 V (vs. SCE). The potential value was converted to the standard hydrogen electrode potential, which can be converted by the following formula: E (RHE) = E (SCE) +0.0591*pH+0.242. The scan rate is 50 mV / s, the it potential is -0.2V, and the test results are shown in Figure 3 and Figure 4 middle.

[0029] Figure 1 X-ray analysis spectrum (XRD) of the carrier Bi2O3 prepared in Examples 1, 2, and 3. As can be seen from Figure 1, the diffraction peaks (red curve) of the prepared Bi2O3 correspond to the peaks of the PDF standard comparison card (PDF#78-1793) of β-Bi2O3, indicating that the main crystal form of the synthesized Bi2O3 is tetragonal β-Bi2O3; the black curve part, in which the two main peaks are located near 27.4° and 28.0°, respectively, corresponds to the peaks of α-Bi2O3 (PDF#65-2366), indicating that the main crystal form of the material is mainly monoclinic α-Bi2O3. At the same time, we also found impurity peaks near 23.9° and 30.3°. Analysis shows that it belongs to the peak of Bi2(CO3)O2 (PDF#98-5331), which is often purified by further calcination in the industry; the blue curve corresponds to γ-Bi2O3 (PDF#80593) corresponds to the PDF card.

[0030] In the electrocatalyst obtained by adopting the technical solution of the present invention, Pt is dispersed between Bi2O3 in a nanochain structure, the average particle size of Pt nanoparticles is about 4.49±0.03nm, and the cross-sectional diameter of the carrier Bi2O3 is about 30nm; the atomic ratio of Pt:Bi is about 9:10, of which Pt accounts for about 40% of the total mass of the catalyst.

[0031] Depend on Figure 3 It can be seen that the Pt / β-Bi2O3 electrocatalyst prepared in Example 1 exhibits good ethanol oxidation activity. Example 1 Electrocatalytic oxidation activity of ethanol (2477.5 mA·mg Pt -1 ) is better than Example 2 (1946.3 mA·mg Pt -1 ) and 3(1852.5 mA·mg Pt -1), which is significantly better than Example 4 and commercial Pt / C nanocatalyst, about 23.93 times that of Example 4 and 3.95 times that of commercial Pt / C.

[0032] Example 2 (1) Preparation of monoclinic α-Bi2O3: The traditional chemical precipitation method was used. The specific synthesis steps are as follows: Weigh 2 g of P123 and dissolve it in 80 mL of 1.5 m / L NaOH solution. Stir ultrasonically for 30 min until P123 is completely dissolved. Heat the water bath to 70 °C, and use a constant pressure separatory funnel to drop 25 mL of 0.1 m / L Bi(NO3)3 solution within 30 min. After the addition is complete, let it stand and cool to room temperature. Wash it with water and ethanol three times each and centrifuge it to completely remove P123 and NaOH. Then dry it in a vacuum oven (50 °C) for 10 h. After grinding it in an agate mortar, the light yellow powder obtained is the monoclinic α-Bi2O3.

[0033] (2) Dissolve 1 g of P123 in 20 mL of H2O in a beaker and stir ultrasonically for 30 min to completely dissolve it. Add K2PtCl6 (20 mg) and α-Bi2O3 (12 mg) according to the mass percentage of Pt being 40 wt%, i.e., the mass ratio of Pt: α-Bi2O3 = 1:4. Mix them ultrasonically until evenly mixed. Transfer the mixture to a reactor and react at 180 °C in a forced air drying oven for 12 h. (3) Cooling naturally to room temperature and keeping it still, the black turbid liquid obtained after the reaction was centrifuged at 10000 r / min, washed with deionized water for 4 times, and then washed with anhydrous ethanol solution for 4 times. Finally, the obtained product was dispersed and protected by adding anhydrous ethanol to obtain a fuel cell Pt / α-Bi2O3 electrocatalyst.

[0034] (4) The Pt / β-Bi2O3 electrocatalyst prepared in this example was modified on a glassy carbon electrode to prepare a working electrode, and cyclic voltammetry and chronoamperometry tests were performed on the electrode. The test conditions were: the solution was a nitrogen-saturated 1 mol / L KOH+1 mol / L EtOH solution, and the CV scanning range was -0.9-0.3 V (vs. SCE). The potential value was converted to the standard hydrogen electrode potential, which can be converted by the following formula: E (RHE) = E (SCE) +0.0591*pH+0.242. The scan rate is 50 mV / s, the it potential is -0.2V, and the test results are shown in Figure 3 and Figure 4 middle.

[0035] Example 3 (1) Cubic γ-Bi2O3: The product was synthesized by traditional wet chemical method. The specific synthesis steps are as follows: 2.4 g Bi(NO3)3·5H2O and 1 g P123 were weighed and dissolved in 25 mL ethylene glycol (EG), and ultrasonically stirred for 30 min to completely dissolve the product, which was recorded as solution A. After the water bath was heated to 70°C, 80 mL 1.5 m / L NaOH solution was measured and recorded as solution B. Solution B was then quickly poured into solution A, and the product was allowed to stand and cool to room temperature. The product was washed with water and ethanol and centrifuged three times each until neutral, and P123 was completely removed. After drying in a vacuum oven (50°C) for 10 h, the product was ground in an agate mortar. The resulting powder was cubic γ-Bi2O3.

[0036] (2) Dissolve 1 g of P123 in 20 mL of H2O in a beaker and stir ultrasonically for 30 min to completely dissolve it. Add K2PtCl6 (20 mg) and γ-Bi2O3 (12 mg) in a ratio of Pt:γ-Bi2O3 = 1:4 with a Pt mass percentage of 40 wt%. Mix well with ultrasonic waves and transfer to a reactor. React in a forced air drying oven at 180 °C for 12 h. (3) Cooling naturally to room temperature and keeping it still, the black turbid liquid obtained after the reaction was centrifuged at 10000 r / min, washed with deionized water for 4 times, and then washed with anhydrous ethanol solution for 4 times. Finally, the obtained product was dispersed and protected by adding anhydrous ethanol to obtain a fuel cell Pt / γ-Bi2O3 electrocatalyst.

[0037] (4) The Pt / β-Bi2O3 electrocatalyst prepared in this example was modified on a glassy carbon electrode to prepare a working electrode, and cyclic voltammetry and chronoamperometry tests were performed on the electrode. The test conditions were: the solution was a nitrogen-saturated 1 mol / L KOH+1 mol / L EtOH solution, and the CV scanning range was -0.9-0.3 V (vs. SCE). The potential value was converted to the standard hydrogen electrode potential, which can be converted by the following formula: E (RHE) = E (SCE) +0.0591*pH+0.242. The scan rate is 50 mV / s, the it potential is -0.2V, and the test results are shown in Figure 3 and Figure 4 middle.

[0038] Example 4 (1) Dissolve 1 g of P123 in 20 mL of H2O in a beaker and stir ultrasonically for 30 min to completely dissolve it. Then add K2PtCl6 (20 mg) and mix ultrasonically until it is evenly dissolved. Transfer the mixture to a reactor and react it in a forced air drying oven at 180 °C for 12 h.

[0039] (2) Cool naturally to room temperature and keep it still. Centrifuge the black turbid liquid obtained after the reaction at 10000 r / min, wash it with deionized water for 4 times, and then wash it with anhydrous ethanol solution for 4 times. Finally, add anhydrous ethanol to disperse the obtained product to obtain a fuel cell Pt NPs electrocatalyst.

[0040] (3) The Pt NPs electrocatalyst prepared in this example was modified on a glassy carbon electrode to prepare a working electrode, and cyclic voltammetry and chronoamperometry tests were performed on the electrode. The test conditions were: the solution was a nitrogen-saturated 1 mol / L KOH + 1 mol / L EtOH solution, the CV scan range was -0.9-0.3 V (vs. SCE), the scan rate was 50 mV / s, and the it potential was -0.2 V. The test results are shown in Figure 3 , 4 middle.

[0041] Figure 4 The chronoamperometric curves of Examples 1, 2, 3, 4 and commercial Pt / C show that the Pt / β-Bi2O3 electrocatalyst prepared in Example 1 exhibits the highest stability. Figure 5 This is also confirmed by the accelerated aging test. It is worth noting that the Pt / β-Bi2O3 catalyst prepared in Example 1 retained an activity of 2232.5 mA·mg after 200 cycles of testing. Pt -1 , Only 1.9% activity loss was observed, while commercial Pt / C was 363.2 mA·mg Pt -1 , The loss of activity was as high as 49.2%.

Claims

1. A Pt / β-Bi2O3 electrocatalyst for a fuel cell, characterized in that: The atomic ratio of Pt:Bi in the electrocatalyst is about 9:10-11, of which Pt accounts for about 30-40% of the total mass of the catalyst.

2. The fuel cell Pt / β-Bi2O3 electrocatalyst according to claim 1, characterized in that: The electrocatalyst Pt is dispersed between Bi2O3 in a nanochain structure, and the average particle size of Pt nanoparticles is about 4.49±0.03nm; the atomic ratio of Pt:Bi in the electrocatalyst is about 9:10, of which Pt accounts for about 40% of the total mass of the catalyst.

3. The method for preparing a fuel cell Pt / β-Bi2O3 electrocatalyst according to claim 1 or 2, characterized in that: The preparation method is as follows: (1) P123 and Na2CO3 are weighed and dissolved in water, and then a bismuth nitrate aqueous solution is added dropwise. After standing, the bottom of the solution is filled with white flocculent precipitates; white Bi2O2CO3 powder is obtained after centrifugal drying, and the white Bi2O2CO3 powder is calcined to obtain tetragonal β-Bi2O3; (2) P123, β-Bi2O3 and K2PtCl6 are dissolved in water and subjected to a hydrothermal reaction to obtain a fuel cell Pt / β-Bi2O3 electrocatalyst.

4. The method for preparing a fuel cell Pt / β-Bi2O3 electrocatalyst according to claim 3, characterized in that: The mass ratio of P123, potassium chloroplatinite and bismuth trioxide is 1:0.01-0.02:0.01-0.

012.

5. The method for preparing a fuel cell Pt / β-Bi2O3 electrocatalyst according to claim 3, characterized in that: The mass ratio of P123, potassium chloroplatinite and bismuth trioxide is 1:0.02:0.

012.

6. The method for preparing a fuel cell Pt / β-Bi2O3 electrocatalyst according to claim 3, characterized in that: The calcination conditions are to increase the temperature to 350-450°C at a heating rate of 1-5°C / min and calcine for 2-4h.

7. The method for preparing a fuel cell Pt / β-Bi2O3 electrocatalyst according to claim 6, characterized in that: The calcination conditions are to increase the temperature to 380°C at a heating rate of 2°C / min and calcine for 2h.

8. The method for preparing a fuel cell Pt / β-Bi2O3 electrocatalyst according to claim 3, characterized in that: The hydrothermal reaction conditions are 150-200° C. for 10-15 hours.

9. The method for preparing a fuel cell Pt / β-Bi2O3 electrocatalyst according to claim 8, characterized in that: The hydrothermal reaction conditions are to react at 180° C. for 12 hours.

10. An electrocatalyst for electrocatalyzing ethanol, characterized in that: A fuel cell Pt / β-Bi2O3 electrocatalyst comprising any one of claims 3-9.

Citation Information

Cited By

  • Platinum-bismuth alloy catalyst, preparation method thereof and direct methanol fuel cell

    CN121862772A

  • Platinum-bismuth alloy catalyst, method for preparing the same, and direct methanol fuel cell

    CN121862772B