Ultra-thin proton exchange membrane of fuel cell for unmanned aerial vehicle and preparation method of ultra-thin proton exchange membrane
By using modified nano cerium oxide and perfluorosulfonic acid resin in the ultra-thin proton exchange membrane of fuel cell, combined with the slit coating method, the problems of low mechanical strength and difficult process are solved, and the conductivity and mechanical of the membrane are improved Performance, extends battery life and reduces costs.
Patent Information
- Application Number
- CN202411079380.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-07
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing ultra-thin proton exchange membranes of fuel cells have low mechanical strength due to the decrease in thickness, which is prone to membrane perforation, and the ultra-thinization process is difficult, resulting in increased production costs and increased defective yield.
After hydrophilization treatment of polytetrafluoroethylene porous membrane, combined with perfluorosulfonic acid resin and modified nano cerium oxide dispersion, a composite reinforced ultra-thin proton exchange membrane was prepared by slit coating to increase mechanical strength and conductance. Rate.
It significantly improves the mechanical strength and conductivity of the proton exchange membrane, extends the battery life, reduces production costs, and maintains stable proton conduction performance under different humidity conditions.
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of proton exchange membranes for fuel cells, and more specifically, to an ultra-thin proton exchange membrane for a fuel cell for an unmanned aerial vehicle and a preparation method thereof. Background Art
[0002] A drone is an unmanned aircraft. Existing drones mainly use battery energy such as lithium batteries and nickel-metal hydride batteries. This type of battery energy has the disadvantages of small battery capacity, poor safety and stability, and harmful air emissions. New energy drones using fuel cells have higher energy density, longer flight time, and are environmentally friendly.
[0003] Proton exchange membrane fuel cell (PEMFC) is a clean and efficient energy conversion device that can directly convert chemical energy into electrical energy through chemical reactions. The key component that determines PEMFC is its internal membrane electrode assembly (MEA), which is a sandwich structure composed of a catalyst layer (CL), a proton exchange membrane (PEM) and a gas diffusion layer (GDL). Among them, PEM mainly plays the role of transferring protons, shielding electrons and isolating reaction gases in PEMFC. The performance of PEM directly determines the performance of PEMFC.
[0004] Optimizing PEM can improve the performance of PEMFC, and the thickness of PEM is one of the main factors affecting the performance of PEMFC. Ultra-thinning the thickness of PEM can help reduce the proton transport barrier, reduce ohmic resistance, improve proton exchange efficiency, and increase the diffusion rate of water on the anode and cathode sides, thereby improving the water management ability of PEMFC; in addition, ultra-thinning can also reduce the consumption of raw materials, thereby reducing production costs. However, the ultra-thin PEM in the prior art often has low mechanical strength due to its reduced thickness, and is prone to membrane perforation during actual assembly and use, greatly reducing battery life. In addition, the ultra-thin process of existing PEM is difficult, resulting in an increase in the rate of defective products, which in turn leads to an increase in production costs. Based on the above statements, the present application provides an ultra-thin proton exchange membrane for a fuel cell for an unmanned aerial vehicle and a preparation method thereof. Summary of the invention
[0005] In order to solve the problems in the prior art that ultra-thin PEM often has low mechanical strength due to its reduced thickness, and membrane perforation is very likely to occur during actual assembly and use, which greatly reduces the battery life, and the ultra-thin process of existing PEM is difficult, resulting in an increase in the rate of defective products and further an increase in production costs, the present application provides an ultra-thin proton exchange membrane for a fuel cell for an unmanned aerial vehicle and a preparation method thereof.
[0006] In the first aspect, the present application provides a method for preparing an ultra-thin proton exchange membrane for a fuel cell for an unmanned aerial vehicle, using the following technical solution:
[0007] A method for preparing an ultra-thin proton exchange membrane for a fuel cell for an unmanned aerial vehicle comprises the following preparation steps:
[0008] S1, pre-treating the polytetrafluoroethylene porous membrane and drying it for standby use, preparing a K2Cr2O7 / H2SO4 mixed solution, immersing the dried polytetrafluoroethylene porous membrane in the mixed solution for hydrophilization treatment, and then discharging the hydrophilized polytetrafluoroethylene porous membrane under vacuum to obtain a treated polytetrafluoroethylene porous membrane;
[0009] S2, using a mixed solution of ethanol and water as a solvent, dissolving perfluorosulfonic acid resin in the solvent to obtain a resin solution, adding the modified nano-cerium oxide dispersion to the resin solution and mixing evenly, then adding polyethylene oxide and polyvinyl alcohol and stirring until the mixture is evenly mixed, removing bubbles, and obtaining a casting slurry;
[0010] S3. Using the treated polytetrafluoroethylene porous membrane as a substrate and the above-mentioned membrane casting slurry, a desired ultra-thin proton exchange membrane is prepared by slit coating.
[0011] Preferably, the specific step of discharging in step S1 is to place the polytetrafluoroethylene porous membrane in a vacuum coating machine and evacuate the vacuum to 10 -2 ~10 -4 Pa.
[0012] Preferably, the solvent in step S2 is obtained by mixing ethanol and water in a mass ratio of 0.8 to 1.2:1.
[0013] Preferably, in step S2, the mass ratio of the perfluorosulfonic acid resin to the solvent is 0.2-0.4:1.
[0014] Preferably, the amount of the modified nano-cerium oxide dispersion added in step S2 is 40% to 60% of the mass of the perfluorosulfonic acid resin solution.
[0015] Preferably, the modified nano-cerium oxide dispersion is prepared from the following raw materials in weight percentage: 1% to 5% polyethylene glycol, 1% to 5% sodium citrate, 2% to 10% nano-cerium oxide powder, and the balance is deionized water.
[0016] Preferably, in step S2, the mass ratio of polyethylene oxide to polyvinyl alcohol is 0.8-1.2:1, and the total amount of polyethylene oxide and polyvinyl alcohol added is 3%-8% of the mass of the perfluorosulfonic acid resin solution.
[0017] In the second aspect, the present application also provides an ultra-thin proton exchange membrane for a fuel cell for an unmanned aerial vehicle, which adopts the following technical solution:
[0018] An ultra-thin proton exchange membrane for a fuel cell for an unmanned aerial vehicle is prepared by the above-mentioned preparation method.
[0019] In summary, this application has the following beneficial effects:
[0020] 1. The present application promotes the improvement of the surface properties of nano-cerium oxide by adding polyethylene glycol and sodium citrate during the preparation of nano-cerium oxide dispersion, which is beneficial to improving the dispersibility and compatibility of nano-cerium oxide in the resin solution, and further helps to improve the conductivity of the proton exchange membrane, enhance the mechanical strength, and improve its stability.
[0021] 2. In the present application, polyethylene oxide and polyvinyl alcohol are added to the perfluorosulfonic acid resin solution. The polyethylene oxide can interact with the sulfonic acid groups in the perfluorosulfonic acid resin to form more proton transmission channels, further promote the conduction of protons, and help improve the conductivity of the proton exchange membrane; the hydrophilicity of polyethylene oxide helps to regulate the water absorption and water retention of the proton exchange membrane, so that it can maintain stable proton conduction performance under different humidity conditions while improving its mechanical strength and toughness. Adding polyethylene oxide and polyvinyl alcohol together to the perfluorosulfonic acid resin can significantly enhance the comprehensive performance of the proton exchange membrane, making it more durable and stable.
[0022] 3. The present application uses the treated polytetrafluoroethylene porous membrane as a substrate, combines the casting slurry with the substrate through a slit coating method to finally obtain a composite enhanced ultra-thin proton exchange membrane, which further improves its mechanical strength while ensuring ultra-thin thickness. DETAILED DESCRIPTION
[0023] The present application is further described in detail below with reference to the embodiments.
[0024] Embodiment 1-3 provides an ultra-thin proton exchange membrane for a fuel cell for an unmanned aerial vehicle and a method for preparing the same.
[0025] Example 1
[0026] A method for preparing an ultra-thin proton exchange membrane for a fuel cell for an unmanned aerial vehicle comprises the following preparation steps:
[0027] S1. Soak the polytetrafluoroethylene porous membrane completely in an acetone solution for half an hour, rinse the membrane surface with distilled water to remove residual acetone, rinse it five times, and then place it in a vacuum oven at 100°C to dry for 10 hours;
[0028] Prepare K2Cr2O7 / H2SO4 mixed solution: add 37g K2Cr2O7 solid and 300ml water into a 500ml beaker, heat until the solid is completely dissolved to obtain a saturated solution, and after cooling, slowly add 300ml of 98% concentrated sulfuric acid while stirring;
[0029] The dried polytetrafluoroethylene porous membrane was immersed in the mixed solution for hydrophilization treatment at a temperature of 40°C for 15 hours, and then placed in a vacuum coating machine and evacuated to 10 -2 Pa, and obtain the treated polytetrafluoroethylene porous membrane.
[0030] S2. Prepare a mixed solution of ethanol and water in a mass ratio of 0.8:1 as a solvent, add perfluorosulfonic acid resin to the solvent at a mass ratio of 0.2:1 to obtain a perfluorosulfonic acid resin solution; add the modified nano cerium oxide dispersion to the resin solution and mix evenly, then add polyethylene oxide and polyvinyl alcohol and stir evenly, remove bubbles, and obtain a casting slurry; wherein the modified nano cerium oxide dispersion is prepared from the following raw materials in weight percentage: 1% polyethylene glycol, 1% sodium citrate, 2% nano cerium oxide powder, and the remainder is deionized water; the amount of the modified nano cerium oxide dispersion added is 40% of the mass of the perfluorosulfonic acid resin solution; the mass ratio of polyethylene oxide to polyvinyl alcohol is 0.8:1, and the total amount of polyethylene oxide and polyvinyl alcohol added is 3% of the mass of the perfluorosulfonic acid resin solution.
[0031] S3. Turn on the scraper, set the coating speed to 25 cm / min, the scraper height to 11 μm, place the treated polytetrafluoroethylene porous membrane on the scraper, add the casting slurry dropwise, start the equipment for coating, and after coating, place it in an oven at 160°C for 10 minutes to remove the solvent, thereby obtaining a proton exchange membrane.
[0032] Example 2
[0033] A method for preparing an ultra-thin proton exchange membrane for a fuel cell for an unmanned aerial vehicle comprises the following preparation steps:
[0034] S1. Soak the polytetrafluoroethylene porous membrane completely in an acetone solution for half an hour, rinse the membrane surface with distilled water to remove residual acetone, rinse it repeatedly five times, and then place it in a 100°C vacuum oven to dry for 10 hours; prepare a K2Cr2O7 / H2SO4 mixed solution: add 37 grams of K2Cr2O7 solid and 300ML water to a 500ML beaker, heat it until the solid is completely dissolved to obtain a saturated solution, and after it cools, slowly add 300ML of 98% concentrated sulfuric acid while stirring; soak the dried polytetrafluoroethylene porous membrane in the mixed solution for hydrophilization treatment at a temperature of 40°C for 15 hours, then place it in a vacuum coating machine and evacuate to 10 -3 Pa, and obtain the treated polytetrafluoroethylene porous membrane.
[0035] S2. Prepare a mixed solution of ethanol and water in a mass ratio of 0.8:1 as a solvent, add perfluorosulfonic acid resin to the solvent at a mass ratio of 0.3:1 to obtain a perfluorosulfonic acid resin solution; add the modified nano cerium oxide dispersion to the resin solution and mix evenly, then add polyethylene oxide and polyvinyl alcohol and stir evenly, remove bubbles, and obtain a casting slurry; wherein the modified nano cerium oxide dispersion is prepared from the following raw materials in weight percentage: 3% polyethylene glycol, 3% sodium citrate, 6% nano cerium oxide powder, and the remainder is deionized water; the amount of the modified nano cerium oxide dispersion added is 50% of the mass of the perfluorosulfonic acid resin solution; the mass ratio of polyethylene oxide to polyvinyl alcohol is 1:1, and the total amount of polyethylene oxide and polyvinyl alcohol added is 6% of the mass of the perfluorosulfonic acid resin solution.
[0036] S3. Turn on the scraper, set the coating speed to 25 cm / min, the scraper height to 11 μm, place the treated polytetrafluoroethylene porous membrane on the scraper, add the casting slurry dropwise, start the equipment for coating, and after coating, place it in an oven at 160°C for 10 minutes to remove the solvent, thereby obtaining a proton exchange membrane.
[0037] Example 3
[0038] A method for preparing an ultra-thin proton exchange membrane for a fuel cell for an unmanned aerial vehicle comprises the following preparation steps:
[0039] S1. Soak the polytetrafluoroethylene porous membrane completely in an acetone solution for half an hour, rinse the membrane surface with distilled water to remove residual acetone, rinse it repeatedly five times, and then place it in a 100°C vacuum oven to dry for 10 hours; prepare a K2Cr2O7 / H2SO4 mixed solution: add 37 grams of K2Cr2O7 solid and 300ML water to a 500ML beaker, heat it until the solid is completely dissolved to obtain a saturated solution, and after it cools, slowly add 300ML of 98% concentrated sulfuric acid while stirring; soak the dried polytetrafluoroethylene porous membrane in the mixed solution for hydrophilization treatment at a temperature of 40°C for 15 hours, then place it in a vacuum coating machine and evacuate to 10 -4 Pa, and obtain the treated polytetrafluoroethylene porous membrane.
[0040] S2. Prepare a mixed solution of ethanol and water in a mass ratio of 0.8:1 as a solvent, add perfluorosulfonic acid resin to the solvent at a mass ratio of 0.4:1 to obtain a perfluorosulfonic acid resin solution; add the modified nano cerium oxide dispersion to the resin solution and mix evenly, then add polyethylene oxide and polyvinyl alcohol and stir evenly, remove bubbles, and obtain a casting slurry; wherein the modified nano cerium oxide dispersion is prepared from the following raw materials in weight percentage: 5% polyethylene glycol, 5% sodium citrate, 10% nano cerium oxide powder, and the remainder is deionized water; the amount of the modified nano cerium oxide dispersion added is 60% of the mass of the perfluorosulfonic acid resin solution; the mass ratio of polyethylene oxide to polyvinyl alcohol is 1.2:1, and the total amount of polyethylene oxide and polyvinyl alcohol added is 8% of the mass of the perfluorosulfonic acid resin solution.
[0041] S3. Turn on the scraper, set the coating speed to 25 cm / min, the scraper height to 11 μm, place the treated polytetrafluoroethylene porous membrane on the scraper, add the casting slurry dropwise, start the equipment for coating, and after coating, place it in an oven at 160°C for 10 minutes to remove the solvent, thereby obtaining a proton exchange membrane.
[0042] In order to verify the comprehensive performance of the ultra-thin proton exchange membrane for the fuel cell of the drone prepared in Examples 1-3 of the present application, the applicant set up comparative examples 1-5, which are as follows:
[0043] Comparative Example 1
[0044] A method for preparing an ultra-thin proton exchange membrane for a fuel cell for an unmanned aerial vehicle comprises the following preparation steps:
[0045] Comparative Example 1 is the same as Example 1, except that the mass of polyethylene glycol is replaced by sodium citrate.
[0046] Comparative Example 2
[0047] A method for preparing an ultra-thin proton exchange membrane for a fuel cell for an unmanned aerial vehicle comprises the following preparation steps:
[0048] Comparative Example 2 is the same as Example 1, except that the mass of sodium citrate is replaced by polyethylene glycol.
[0049] Comparative Example 3
[0050] A method for preparing an ultra-thin proton exchange membrane for a fuel cell for an unmanned aerial vehicle comprises the following preparation steps:
[0051] Comparative Example 3 is the same as Example 1, except that the mass of polyethylene oxide is replaced by polyvinyl alcohol.
[0052] Comparative Example 4
[0053] A method for preparing an ultra-thin proton exchange membrane for a fuel cell for an unmanned aerial vehicle comprises the following preparation steps:
[0054] Comparative Example 4 is the same as Example 1, except that the mass of polyvinyl alcohol is replaced by polyethylene oxide.
[0055] Comparative Example 5
[0056] A method for preparing an ultra-thin proton exchange membrane for a fuel cell for an unmanned aerial vehicle comprises the following preparation steps:
[0057] S1. Prepare a mixed solution of ethanol and water in a mass ratio of 0.8:1 as a solvent, add perfluorosulfonic acid resin to the solvent at a mass ratio of 0.2:1 to obtain a perfluorosulfonic acid resin solution; add the modified nano cerium oxide dispersion to the resin solution and mix evenly, then add polyethylene oxide and polyvinyl alcohol and stir evenly, remove bubbles, and obtain a casting slurry; wherein the modified nano cerium oxide dispersion is prepared from the following raw materials in weight percentage: polyethylene glycol 1%, sodium citrate 1%, nano cerium oxide powder 2%, and the balance is deionized water; the amount of the modified nano cerium oxide dispersion added is 40% of the mass of the perfluorosulfonic acid resin solution; the mass ratio of polyethylene oxide to polyvinyl alcohol is 0.8:1, and the total amount of polyethylene oxide and polyvinyl alcohol added is 3% of the mass of the perfluorosulfonic acid resin solution.
[0058] S2. Turn on the scraper, set the coating speed to 25 cm / min, the scraper height to 11 μm, place the treated polytetrafluoroethylene porous membrane on the scraper, add the casting slurry dropwise, start the equipment for coating, and after coating, place it in an oven at 160°C for 10 minutes to remove the solvent to obtain a proton exchange membrane.
[0059] Performance Testing:
[0060] The conductivity, water absorption, tensile strength and breaking strength properties of the proton exchange membranes prepared in Examples 1-3 of the present application and Comparative Examples 1-5 were tested respectively.
[0061] 1. Conductivity
[0062] The proton exchange membranes prepared in this embodiment and the comparative example were used as samples, and the conductivity of the proton exchange membranes in the vertical direction and the horizontal direction were tested by electrochemical impedance spectroscopy. Electrochemical impedance spectroscopy can eliminate the complex concentration polarization and ion accumulation problems at the electrode-electrolyte interface, and avoid the influence of charge transfer resistance at the electrode-electrolyte interface.
[0063] 2. Water absorption
[0064] The water absorption rate of the film was measured by the dry and wet weighing method. The specific steps are as follows: cut a film of about 4 cm × 4 cm, place the film in a vacuum drying oven at 100 ° C for 24 hours, and quickly weigh the dry film to obtain the mass W dryThe dry film was soaked in deionized water and placed in a water bath constant temperature oscillator for 24 hours to allow the film to fully absorb water. After taking it out, the surface water was quickly absorbed with filter paper and weighed again to obtain the mass W of the wet film. wet The water absorption rate of the membrane is calculated using the following formula:
[0065] 3. Tensile strength, breaking strength
[0066] The test was carried out on an electronic universal testing machine in accordance with national standards GB1039-79 and GB1040-79WD-10D, with a tensile rate of 10 mm min -1 .
[0067] The test results are shown in Table 1 below:
[0068] Table 1
[0069] Conductivity (S / cm) Water absorption (%) Tensile strength(Mpa) Breaking strength(Mpa) Example 1 0.254 61.2 28.4 32.3 Example 2 0.267 58.3 29.8 35.6 Example 3 0.258 56.9 30.2 36.4 Comparative Example 1 0.182 24.3 8.3 10.3 Comparative Example 2 0.174 25.3 9.3 11.2 Comparative Example 3 0.163 28.9 11.7 14.5 Comparative Example 4 0.188 27.5 9.7 14.3 Comparative Example 5 0.142 18.3 6.2 8.9
[0070] It can be seen from the data shown in Table 1 above that the conductivity and water absorption of the proton exchange membrane prepared in the embodiment of the present application are significantly better than those of the comparative example, and the performance of the proton exchange membrane in the embodiment is significantly better than that of the comparative example.
[0071] It can be seen from the data shown in Table 2 above that the tensile strength and breaking strength of the proton exchange membrane prepared in the examples of the present application are significantly better than those in the comparative examples, and the mechanical strength of the proton exchange membrane in the examples is significantly better than that in the comparative examples.
[0072] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A method for preparing an ultra-thin proton exchange membrane for a fuel cell for an unmanned aerial vehicle, characterized in that: The method comprises the following preparation steps: S1, pre-treating the polytetrafluoroethylene porous membrane and drying it for standby use, preparing a K2Cr2O7 / H2SO4 mixed solution, immersing the dried polytetrafluoroethylene porous membrane in the mixed solution for hydrophilization treatment, and then discharging the hydrophilized polytetrafluoroethylene porous membrane under vacuum to obtain a treated polytetrafluoroethylene porous membrane; S2, using a mixed solution of ethanol and water as a solvent, dissolving perfluorosulfonic acid resin in the solvent to obtain a resin solution, adding the modified nano-cerium oxide dispersion to the resin solution and mixing evenly, then adding polyethylene oxide and polyvinyl alcohol and stirring until the mixture is evenly mixed, removing bubbles, and obtaining a casting slurry; S3. Using the treated polytetrafluoroethylene porous membrane as a substrate and the above-mentioned membrane casting slurry, a desired ultra-thin proton exchange membrane is prepared by slit coating.
2. The method for preparing an ultra-thin proton exchange membrane for a fuel cell for an unmanned aerial vehicle according to claim 1, characterized in that: The specific step of discharging in step S1 is to place the polytetrafluoroethylene porous membrane in a vacuum coating machine and evacuate the vacuum to 10 -2 ~10 -4 Pa.
3. The method for preparing an ultra-thin proton exchange membrane for a fuel cell for an unmanned aerial vehicle according to claim 1, characterized in that: The solvent in step S2 is obtained by mixing ethanol and water in a mass ratio of 0.8 to 1.2:
1.
4. The method for preparing an ultra-thin proton exchange membrane for a fuel cell for an unmanned aerial vehicle according to claim 1, characterized in that: In the step S2, the mass ratio of the perfluorosulfonic acid resin to the solvent is 0.2-0.4:
1.
5. The method for preparing an ultra-thin proton exchange membrane for a fuel cell for an unmanned aerial vehicle according to claim 1, characterized in that: The amount of the modified nano-cerium oxide dispersion added in step S2 is 40% to 60% of the mass of the perfluorosulfonic acid resin solution.
6. The method for preparing an ultra-thin proton exchange membrane for a fuel cell for an unmanned aerial vehicle according to claim 5, characterized in that: The modified nano cerium oxide dispersion is prepared from the following raw materials in weight percentage: 1% to 5% polyethylene glycol, 1% to 5% sodium citrate, 2% to 10% nano cerium oxide powder, and the balance is deionized water.
7. The method for preparing an ultra-thin proton exchange membrane for a fuel cell for an unmanned aerial vehicle according to claim 1, characterized in that: In the step S2, the mass ratio of polyethylene oxide to polyvinyl alcohol is 0.8-1.2:1, and the total amount of polyethylene oxide and polyvinyl alcohol added is 3%-8% of the mass of the perfluorosulfonic acid resin solution.
8. An ultra-thin proton exchange membrane for a fuel cell for an unmanned aerial vehicle, characterized in that: Prepared by the preparation method according to any one of claims 1 to 8.
Citation Information
Cited By
Preparation method of multifunctional composite proton exchange membrane
CN119542481A