Alkali ion secondary battery electrolyte and preparation method and application thereof
By using polyhydroxyphenols, fluorovinyl carbonate, and organic silicate in alkali-ion secondary battery electrolyte, the problem of inflation of sodium ion batteries is solved, and higher circulation and safety performance are achieved.
Patent Information
- Application Number
- CN202410981152.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-11-12
AI Technical Summary
There are serious gas problems in existing alkali ion secondary batteries, especially sodium ion batteries, which lead to a decrease in the capacity and charging capacity of the battery cell and a safety hazard. The traditional modification method has limited effect.
An alkali ion secondary battery electrolyte is used, which contains active alkali metal salts, organic solvents and anti-bloating additives. The anti-bloating additives include polyhydroxyphenols, fluorovinyl carbonate and organic silicate. Through the synergistic effect of these additives, Stabilize the solid electrolyte membrane, inhibit bloating, and optimize the viscosity of the electrolyte.
It significantly improves circulation performance, first-effect, charge capacity and safety performance, avoids battery inflation, and improves the overall performance of the battery.
Smart Images

Figure BDA0004956103670000021 
Figure BDA0004956103670000022 
Figure BDA0004956103670000031
Abstract
Description
Technical Field
[0001] The present invention relates to the field of new energy technology, and in particular to an alkali ion secondary battery electrolyte and a preparation method and application thereof. Background Art
[0002] Common alkaline ion secondary batteries include lithium ion batteries, sodium ion batteries and potassium ion batteries. These batteries either have excellent electrochemical properties or have obvious price advantages, and have broad application prospects in the fields of energy storage, power batteries or small household appliances. Among them, sodium ion batteries have great application potential in electric vehicles, battery vehicles and energy storage due to their low cost, high safety and long cycle life. However, in actual alkaline ion secondary battery systems, especially sodium ion batteries, there is still a serious problem of battery flatulence. Flatulence not only reduces the capacity, charge capacity, cycle and other performance of the battery cell, but also brings great safety risks.
[0003] Flatulence is caused by many factors, including the dissolution of the SEI film and the decomposition of the electrolyte EC. In traditional technology, in order to suppress the generation of flatulence, the positive and negative electrode materials or the electrolyte are usually modified. However, at present, the above modification methods have achieved limited results. Summary of the invention
[0004] The present invention aims to solve at least one of the technical problems existing in the prior art. To this end, the present invention provides an electrolyte for an alkali ion secondary battery, which can effectively avoid the problem of bloating of the alkali ion secondary battery.
[0005] The invention also provides a method for preparing the electrolyte of the alkali ion secondary battery.
[0006] The present invention also provides an alkali ion secondary battery comprising the alkali ion secondary battery electrolyte.
[0007] According to an embodiment of the first aspect of the present invention, an alkali ion secondary battery electrolyte is provided, wherein raw materials for preparing the alkali ion secondary battery electrolyte include an active alkali metal salt, an organic solvent and an anti-flatulence additive;
[0008] The anti-flatulence additives include polyhydroxyphenol additives, fluoroethylene carbonate and organosilicon nitrile;
[0009] The anti-flatulence additive accounts for ≤8.5% of the mass percentage of the electrolyte of the alkali ion secondary battery.
[0010] The alkaline ion secondary battery electrolyte according to the embodiment of the present invention has at least the following beneficial effects:
[0011] The polyhydroxyphenol structural units help stabilize the decomposition product PF5 of MPF6, thereby promoting the formation of MF (where M is an alkali metal ion, specifically lithium ions, sodium ions and potassium ions, etc.), which plays a role in stabilizing the SEI film. The generated SEI film is denser and more stable than conventional film-forming additives.
[0012] By adding fluoroethylene carbonate, HF generated in the electrolyte of the alkali ion secondary battery can be eliminated, which plays a role in controlling the HF content; the wettability of the battery pole piece can be increased; further, compared with other components in the electrolyte of the alkali ion secondary battery, it can be preferentially reduced, so it has a good film-forming effect, and can be preferentially decomposed in the electrolyte of the alkali ion secondary battery and form a passivation film on the negative electrode surface. Furthermore, compared with other types of fluorocarbonates, the viscosity of the fluoroethylene carbonate used in the present invention is more suitable and the cost is lower.
[0013] Due to its structure, organosilicon nitrile can protect the surface layer of the positive electrode and protect ester organic solvents such as EC from decomposition, thereby reducing the gas production of the battery. When used with polyhydroxyphenol additives, it can make up for the shortcomings of polyhydroxyphenol additives and has a synergistic effect in improving flatulence.
[0014] By limiting the dosage of the anti-flatulence additive, the overall viscosity of the electrolyte of the alkali ion secondary battery can be optimized, thereby giving full play to the synergistic effect of the three anti-flatulence additives.
[0015] In summary, in the alkaline ion secondary battery electrolyte provided by the present invention, the anti-flatulence additives have a synergistic effect, which can significantly stabilize the solid electrolyte membrane on the surface of the positive and negative electrodes, play a role in inhibiting flatulence, and ultimately achieve the effect of improving the cycle performance, first effect, charging capacity and safety performance.
[0016] According to some embodiments of the present invention, in the structural formula of the polyhydroxyphenol additive, the number of hydroxyl groups is ≥ 5, for example, 20 or 25.
[0017] According to some embodiments of the present invention, the structural formula of the polyhydroxyphenol additive is as shown in Formula I:
[0018]
[0019] Wherein, R is selected from at least one of methyl, vinyl and the structure shown in formula II:
[0020]
[0021] According to some embodiments of the present invention, the polyhydroxyphenol additive includes tannic acid.
[0022] According to some embodiments of the present invention, the molecular weight of the polyhydroxyphenol additive is 200-2500, for example, 1500-2000, and more specifically, 1700-1710.
[0023] If the molecular weight of the polyhydroxyphenol additive is lower than 200, it cannot meet the limitation of ≥5 hydroxyl groups of the polyhydroxyphenol additive, and it is difficult to play a synergistic role with FEC and silicone nitrile; that is, the limitation of the lower limit of the molecular weight is actually still a limitation on the number of hydroxyl groups, and it is essentially the number of hydroxyl groups that affects the synergistic effect. However, if the molecular weight of the polyhydroxyphenol additive is higher than 2500, the solubility of the polyhydroxyphenol additive in the alkaline ion secondary battery electrolyte will deteriorate, and the synergistic effect with FEC and silicone nitrile will decrease. In summary, selecting the above range can significantly promote the synergistic effect.
[0024] According to some embodiments of the present invention, the mass percentage of the polyhydroxyphenol additive in the alkaline ion secondary battery electrolyte is 0.6-2.8%, for example, about 0.7%, 0.8%, 0.9%, 1.0%, 1.5%, 1.8%, 2.0% or about 2.5%.
[0025] According to some embodiments of the present invention, the mass percentage of the fluoroethylene carbonate in the electrolyte of the alkali ion secondary battery is 0.1-6.7%, for example, 0.5%, 1.0%, 2.0%, 3.0%, 3.5%, 4%, 5%, 6%, 6.1%, 6.2%, 6.3%, 6.4%, 6.5% or about 6.6%.
[0026] According to some embodiments of the present invention, the structural formula of the organosilicon nitrile is shown in Formula III:
[0027]
[0028] Wherein, R4 is selected from one of an aromatic group or an aliphatic ring;
[0029] R1, R2, and R3 are independently selected from at least one of methyl, vinyl, and halogen;
[0030] n is selected from any integer between 1 and 5.
[0031] According to some embodiments of the present invention, the mass percentage of the organosilicon nitrile in the electrolyte of the alkali ion secondary battery is 1.2-5.6%, for example, about 1.3%, 1.4%, 1.5%, 1.6%, 1.8%, 2.0%, 3.0%, 3.5%, 4.0%, 5.0% or about 5.5%.
[0032] According to some embodiments of the present invention, the mass ratio of the organosilicon nitrile to the polyhydroxyphenol additive is 1.5 to 2.5:1. For example, it can be about 2:1. The amount of the polyhydroxyphenol additive used will affect the generation of MF to a certain extent. MF is only a component of the SEI film. Too much or too little will affect the performance of the SEI film. Within the above range, a more appropriate amount of MF can be formed, thereby improving the ion mobility of the resulting SEI film.
[0033] According to some embodiments of the present invention, the anti-flatulence additive accounts for ≤8.5% of the mass percentage of the electrolyte of the alkali ion secondary battery, thereby avoiding the negative impact of the anti-flatulence additive on electrochemical performance while exerting the synergistic effect of the anti-flatulence additive.
[0034] According to some embodiments of the present invention, the concentration of the active alkali metal salt in the alkali ion secondary battery electrolyte is 0.1 to 3.0 mol / L, for example, 0.7 to 1.4 mol / L.
[0035] According to some embodiments of the present invention, the mass percentage of the active alkali metal salt in the alkali ion secondary battery electrolyte is 0.1% to 20.0%, for example, about 5%, 10%, 12%, 13%, 14% or about 15%.
[0036] According to some embodiments of the present invention, the active alkali metal salt includes at least one of a lithium salt, a sodium salt and a potassium salt.
[0037] According to some embodiments of the present invention, the lithium salt includes lithium hexafluorophosphate.
[0038] According to some embodiments of the present invention, the sodium salt includes at least one of sodium hexafluorophosphate, lithium tetrafluoroborate, sodium hexafluoroarsenate, sodium perchlorate, sodium bis(oxalatoborate), sodium difluorooxalatoborate, sodium difluorophosphate, sodium bis(fluorosulfonyl)imide and sodium bis(trifluoromethylsulfonyl)imide.
[0039] According to some embodiments of the present invention, the organic solvent includes at least two of dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, propylene carbonate, ethylene carbonate, methyl propyl carbonate, ethyl propionate, ethyl acetate, ethyl formate, propyl butyrate, tetrahydrofuran, dioxane, diethanol diethyl ether and γ-butyrolactone.
[0040] According to some embodiments of the present invention, the organic solvent is a mixture of ethylene carbonate (EC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC) and ethyl acetate. Wherein, in terms of mass ratio:
[0041] EC:DEC=1:1-2; for example, it may be about 1:1.5.
[0042] EC:EMC=1:1.5-2.5; for example, it may be about 1:2.
[0043] EC:ethyl acetate=1:0.3-0.6; for example, it can be about 1:0.5.
[0044] According to some embodiments of the present invention, the mass percentage of the organic solvent in the alkali ion secondary battery electrolyte is 75.0% to 88.0%.
[0045] According to some embodiments of the present invention, the raw materials for preparing the electrolyte of the alkali ion secondary battery further include a film-forming additive.
[0046] According to some embodiments of the present invention, the film-forming additive includes at least one of a positive electrode film-forming additive and a negative electrode film-forming additive.
[0047] According to some embodiments of the present invention, the negative electrode film-forming additive includes TMSP (tris(trimethylsilyl)phosphite).
[0048] According to some embodiments of the present invention, the mass percentage of the negative electrode film-forming additive in the electrolyte of the alkali ion secondary battery is 1-2%, for example, specifically about 1.5%.
[0049] According to some embodiments of the present invention, the positive electrode film-forming additive includes at least one of PS (1,3-propane sultone) and DTD (diethylene sulfate).
[0050] The positive electrode film-forming additive includes the PS and DTD. The mass ratio of the PS to the DTD is 1:0.8 to 1.2. For example, it can be about 1:1.
[0051] According to some embodiments of the present invention, the mass percentage of the positive electrode film-forming additive in the electrolyte of the alkali ion secondary battery is 1.5-3%, for example, specifically about 2%.
[0052] According to an embodiment of the second aspect of the present invention, a method for preparing the alkali ion secondary battery electrolyte is provided, the method comprising mixing raw materials for preparing the alkali ion secondary battery electrolyte.
[0053] Since the preparation method adopts all the technical solutions of the alkaline ion secondary battery electrolyte of the above embodiment, it at least has all the beneficial effects brought by the technical solutions of the above embodiment.
[0054] According to some embodiments of the present invention, the water content in the environment in which the preparation method is implemented is ≤10 ppm, for example, it can be carried out in a glove box filled with argon.
[0055] According to an embodiment of the third aspect of the present invention, an alkali ion secondary battery is provided, wherein raw materials for preparing the alkali ion secondary battery include the alkali ion secondary battery electrolyte.
[0056] Since the alkali ion secondary battery adopts all the technical solutions of the alkali ion secondary battery electrolyte of the above embodiment, it at least has all the beneficial effects brought by the technical solutions of the above embodiment.
[0057] According to some embodiments of the present invention, the alkali ion secondary battery includes at least one of a lithium ion battery, a sodium ion battery and a potassium ion battery.
[0058] According to some embodiments of the present invention, the alkali ion secondary battery is selected from a sodium ion battery. When the alkali ion secondary battery electrolyte is applied to a sodium ion battery, the polyhydroxyphenol additive can promote the decomposition of NaPF6 to generate NaF; the polyhydroxyphenol additive can react with NaPF6 to generate sodium phenol salt, and then react with the organic solvent to form a stable and dense inorganic / organic composite SEI film, but the battery pole system is difficult to infiltrate; the fluoroethylene carbonate can increase the wettability of the system, but it is easy to produce HF and CO2 gas at high temperature; organic silicon nitrile can inhibit the decomposition of some esters at high temperature and reduce CO2 gas. When the alkali ion secondary battery electrolyte is applied to a sodium ion battery, due to the synergistic effect between the anti-flatulence additives, the problems of the polyhydroxyphenol additive being difficult to wet, inhibiting the decomposition of the fluoroethylene carbonate, etc., and reducing the gas production of the battery system can be significantly avoided. That is, the combination of the alkali ion secondary battery electrolyte and the sodium ion battery system has a higher improvement in the performance of the sodium ion battery.
[0059] According to some embodiments of the present invention, the alkali ion secondary battery includes a battery cell soaked in the alkali ion secondary battery electrolyte; the battery cell includes a positive electrode sheet, a negative electrode sheet, and a separator disposed between the positive electrode sheet and the negative electrode sheet.
[0060] According to some embodiments of the present invention, the positive electrode sheet includes a positive electrode current collector and a positive electrode coating covering a surface of the positive electrode current collector.
[0061] According to some embodiments of the present invention, the positive electrode coating includes a positive electrode binder, a positive electrode conductor and a positive electrode active material.
[0062] According to some embodiments of the present invention, when the alkali ion secondary battery is selected from the sodium ion battery, the positive electrode active material includes at least one of sodium copper iron manganese oxide and sodium nickel iron manganese oxide.
[0063] According to some embodiments of the present invention, the positive electrode conductive agent includes at least one of Ketjen black, multi-walled carbon nanotubes and ordered mesoporous carbon. Specifically, the positive electrode conductive agent is selected from Ketjen black.
[0064] According to some embodiments of the present invention, the positive electrode binder includes PVDF.
[0065] According to some embodiments of the present invention, in the positive electrode coating, the weight ratio of the positive electrode active material, the positive electrode conductive agent and the positive electrode binder is 90-97:0.8-1.5:0.6-2.6.
[0066] The mass ratio of the positive electrode active material to the positive electrode conductive agent is 87 to 88.5:1, for example, specifically about 88:1.
[0067] The mass ratio of the positive electrode active material to the positive electrode binder is 48 to 49:1, for example, specifically about 48.5:1.
[0068] According to some embodiments of the present invention, the method for setting the positive electrode sheet is as follows: the raw materials for preparing the positive electrode coating are made into positive electrode slurry, which is then coated on the positive electrode collector, followed by drying, rolling, striping or die-cutting and tab welding.
[0069] According to some embodiments of the present invention, the negative electrode sheet includes a negative electrode current collector and a negative electrode coating covering a surface of the negative electrode current collector.
[0070] According to some embodiments of the present invention, the raw materials for preparing the negative electrode coating include a thickener, a negative electrode active material, a negative electrode conductive agent and a negative electrode binder.
[0071] The thickener includes sodium carboxymethylcellulose (CMC).
[0072] The negative electrode active material includes hard carbon.
[0073] The binder includes SBR.
[0074] According to some embodiments of the present invention, the negative electrode sheet is provided by mixing the raw materials for preparing the negative electrode coating into a negative electrode slurry, coating the negative electrode slurry on the surface of the negative electrode collector, and then drying, rolling, striping or die-cutting and welding the tabs.
[0075] According to some embodiments of the present invention, the preparation method of the negative electrode slurry includes first preparing the thickener and water into a glue solution, then mixing part of the glue solution, the negative electrode active material, the negative electrode conductive agent and the negative electrode binder; and finally mixing the obtained mixture with the remaining glue solution and adjusting the viscosity.
[0076] The mass percentage of the partial glue solution to the total glue solution is 50-70%, for example, specifically about 60%.
[0077] In the raw materials for preparing the glue solution, the mass ratio of the thickener to water is 0.7-1.5:1.
[0078] The weight ratio of the negative electrode active material, the negative electrode conductive agent, the negative electrode binder and the thickener is 89-94.4: 0.5-1.6: 0.5-2: 0.5-2. Specifically:
[0079] The mass ratio of the negative electrode active material to the negative electrode conductive agent is 117 to 118:1, for example, specifically about 117.5:1;
[0080] The mass ratio of the negative electrode active material to the negative electrode binder is 45 to 50:1, for example, specifically about 47:1;
[0081] The mass ratio of the negative electrode active material to the thickener is 55 to 60:1, for example, specifically about 58:1 or about 59:1.
[0082] According to some embodiments of the present invention, the alkali ion secondary battery assembly method includes preparing the positive electrode sheet, the negative electrode sheet and the separator into a battery cell by winding or stacking, and then placing the battery cell into a battery shell, injecting the alkali ion secondary battery electrolyte, and letting it stand.
[0083] If there is no special explanation, the actual meaning of “about” in the present invention is that the error is allowed to be within the range of ±2%, for example, about 100 is actually 100±2%×100.
[0084] Unless otherwise specified, “between” in the present invention includes the number itself, for example, “between 2 and 3” includes the endpoint values 2 and 3.
[0085] Other features and advantages of the present invention will be set forth in the description which follows, and in part will be apparent from the description, or may be learned by practice of the present invention. DETAILED DESCRIPTION
[0086] The following will be combined with the embodiments to clearly and completely describe the concept of the present invention and the technical effects produced, so as to fully understand the purpose, characteristics and effects of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, other embodiments obtained by those skilled in the art without creative work are all within the scope of protection of the present invention.
[0087] In the description of the present invention, the description with reference to the terms "one embodiment", "some embodiments", "illustrative embodiments", "examples", "specific examples", or "some examples" means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner.
[0088] Unless otherwise specified, the raw materials and reagents used in the following examples are commercially available or can be prepared by known methods.
[0089] Example 1
[0090] In this example, a sodium ion battery electrolyte was prepared, and the specific steps were as follows:
[0091] In an argon atmosphere glove box with a water content of <10 ppm, an organic solvent, an active sodium salt, an anti-flatulence additive and other additives are mixed.
[0092] The organic solvent is ethylene carbonate (EC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), and ethyl acetate mixed in a mass ratio of 2:3:4:1; the mass percentage of the organic solvent in the sodium ion battery electrolyte is 100% and the difference between the sum of the mass percentages of other components;
[0093] The active sodium salt is NaPF6, which accounts for 13% of the mass percentage of the sodium ion battery electrolyte;
[0094] The amount of the anti-flatulence additive is as shown in Table 1. The polyhydroxyphenol is tannic acid (CAS No.: 1401-55-4) selected from Hubei Changyao Biotechnology Co., Ltd.; the structural formula of the organosilicon nitrile is as follows:
[0095] Wherein n=2, R1 and R2 are methyl groups, R3 is vinyl group, and R4 is phenyl group.
[0096] Other additives are as follows:
[0097] The negative electrode film-forming additive TMSP tris(trimethylsilyl)phosphite, CAS number 1795-31-9, is added at a ratio of 1.5%; the positive electrode film-forming additive PS1,3-propane sultone, CAS number 1120-71-4, is added at a ratio of 1%; DTD vinyl sulfate, CAS number 1072-53-3, is added at a ratio of 1%.
[0098] Examples 2 to 5 respectively prepare a sodium ion battery electrolyte, which is different from Example 1 in that the amount of the anti-flatulence additive is slightly different, and the specific differences are shown in Table 1.
[0099] Example 6
[0100] This example prepares a lithium ion battery electrolyte, which is different from Example 3 in that:
[0101] The active salt was replaced by an equal amount of lithium hexafluorophosphate from sodium hexafluorophosphate.
[0102] Example 7
[0103] This example prepares a sodium ion battery electrolyte, which is different from Example 3 in that:
[0104] The polyhydroxyphenol additive has different numbers of hydroxyl groups, the number of hydroxyl groups in Example 1 is ≥ 5, and the number of hydroxyl groups in Comparative Example 6 is 3. The specific polyhydroxyphenol additive used is luteolin (CAS: 491-70-3).
[0105] Comparative Examples 1 to 5 respectively prepared a sodium ion battery electrolyte, which differed from Example 1 in that:
[0106] The types and amounts of anti-flatulence additives vary slightly, as shown in Table 1.
[0107] Comparative Examples 6 to 8 respectively prepared a lithium ion battery electrolyte, which differed from Example 6 in that:
[0108] The types and amounts of anti-flatulence additives vary slightly, as shown in Table 1.
[0109] Table 1 Amount of anti-flatulence additives in sodium ion battery electrolytes of Examples and Comparative Examples
[0110]
[0111]
[0112] Application Examples
[0113] This example provides a sodium ion secondary battery, specifically:
[0114] The electrolytes are respectively from the sodium ion battery electrolytes obtained in the examples or comparative examples (Examples 1 to 5, Example 7, Comparative Examples 1 to 5). The sodium ion secondary batteries of this example are numbered according to the source of the electrolyte.
[0115] Positive electrode sheet: The positive electrode active material sodium nickel iron manganese oxide (purchased from Hunan Changyuan Lithium Technology Co., Ltd., model NY303, nominal gram capacity 125 mAh / g), conductive agent Ketjen black, and binder PVDF are mixed in a weight ratio of 96.9%:1.1%:2.0%, and solvent N-methylpyrrolidone is added. The mixture is stirred and mixed to obtain a positive electrode slurry, which is then coated on both surfaces of the positive electrode current collector aluminum foil, and then dried and cold pressed to obtain a positive electrode sheet.
[0116] Negative electrode sheet: First, the thickener and water are prepared into a glue solution, and then part of the glue solution, negative electrode active material, negative electrode conductive agent and negative electrode binder are mixed; finally, the obtained mixture is mixed with the remaining glue solution, and the viscosity is adjusted. Among them, the mass percentage of the partial glue solution to all the glue solutions is 60%; the mass concentration of the glue solution is 40%. The weight ratio of the negative electrode active material hard carbon, the negative electrode conductive agent conductive carbon black, the negative electrode binder SBR, and CMC is 94:0.8:2.0:1.6. Then the obtained negative electrode slurry is coated on both surfaces of the negative electrode current collector copper foil, and the negative electrode sheet is obtained after drying and cold pressing.
[0117] Diaphragm: A polyethylene porous membrane coated with alumina ceramic on both sides produced by Shanghai Enjie New Material Technology Co., Ltd.
[0118] Assemble, roll the positive electrode sheet, negative electrode sheet and separator into a sodium ion battery cell with a capacity of 2600mAh, place it in an aluminum-plastic film, inject electrolyte, package it, and let it stand.
[0119] Application Example 2
[0120] The electrolytes are respectively from lithium ion battery electrolytes obtained in the examples or comparative examples (Example 6 and Comparative Examples 6 to 8). The lithium ion secondary batteries of this example are numbered according to the source of the electrolyte.
[0121] Positive electrode sheet: The positive electrode active material lithium cobalt oxide (purchased from Hunan Changyuan Lithium Technology Co., Ltd., model LC230, nominal gram-specific capacity 188 mAh / g), conductive agent Ketjen black, and binder PVDF are mixed in a weight ratio of 96.9%:1.1%:2.0%, and solvent N-methylpyrrolidone is added. The mixture is stirred and mixed thoroughly to obtain a positive electrode slurry, which is then coated on both surfaces of the positive electrode current collector aluminum foil, and then dried and cold pressed to obtain a positive electrode sheet.
[0122] Negative electrode: Same as Application Example 1.
[0123] Diaphragm: A polyethylene porous membrane coated with alumina ceramic on both sides produced by Shanghai Enjie New Material Technology Co., Ltd.
[0124] Assemble, roll the positive electrode sheet, negative electrode sheet and separator into a lithium-ion battery cell with a capacity of 3910 mAh, place it in an aluminum-plastic film, inject electrolyte, package it, and let it stand.
[0125] Test Example 1
[0126] This example tests the electrochemical performance of the sodium ion battery obtained in Application Example 1, wherein:
[0127] The test method is: charge to 4.0V at 1.0C constant current and constant voltage, and then discharge to 2.0V at 1.0C constant current (set 1C current to 2.6A).
[0128] First charge and discharge efficiency (%) = first discharge capacity / first charge capacity*100%;
[0129] Capacity retention rate (%) = 1000th week capacity / initial capacity (25±3°C) * 100%. The test temperature is 25°C.
[0130] Thickness change rate (%) = high temperature storage at 85°C for 3 hours / initial thickness*100%.
[0131] Test Example 2
[0132] This example tests the electrochemical performance of the lithium-ion battery obtained in Application Example 2, wherein:
[0133] The test method is: charge to 4.5V at 1.0C constant current and constant voltage, and then discharge to 3.0V at 1.0C constant current (set 1C current to 3.91A).
[0134] First charge and discharge efficiency (%) = first discharge capacity / first charge capacity*100%;
[0135] Capacity retention rate (%) = 1000th week capacity / initial capacity (25±3°C) * 100%. The test temperature is 25°C.
[0136] Thickness change rate (%) = high temperature storage at 85°C for 3 hours / initial thickness*100%.
[0137] The test results are shown in Table 2.
[0138] Table 2 Electrochemical performance of sodium ion and lithium ion batteries obtained in the application examples
[0139]
[0140]
[0141] In Examples 1 to 3, as the content of organosilicon nitrile and polyhydroxyphenol additives increases, synergistic effects are produced, gas production is reduced, and the difference in the first effect is not significant. Within a certain content, organosilicon nitrile, polyhydroxyphenol additives and FEC have synergistic effects.
[0142] In Examples 4 and 5, as FEC decreases, the first efficiency decreases. FEC can be consumed first to form the negative electrode SEI film. If the content is too low, side reactions during formation will reduce the first efficiency.
[0143] Comparing Example 6 with Example 3, the electrochemical performance of the three additives in the sodium ion battery system is better than that in the lithium ion battery system. This shows that there is a significant synergistic effect between the alkali ion secondary battery electrolyte provided by the present invention and the sodium ion battery system.
[0144] By comparing Example 7 with Example 1, it can be seen that if the hydroxyl content of the polyhydroxyphenol additive is less than 5, the electrochemical properties such as capacity retention rate can still be improved to a certain extent, and the gas production problem can be improved to a small extent, but the improvement effect on the gas production problem is slightly poor.
[0145] From Comparative Examples 1 to 4, it can be seen that in the anti-flatulence additives provided by the present invention, any two additives cannot improve gas production, and the sum of the effects on electrochemical performance is significantly inferior to the combined effect of the three additives in Example 1; thus, it can be seen that in the anti-flatulence additives provided by the present invention, the three substances have a significant synergistic effect, so the electrochemical performance can be greatly improved. Comparative Examples and Comparative Example 5 show that if the amount of the anti-flatulence additive is not within the range required by the present invention, it will significantly affect the viscosity of the obtained alkali ion secondary battery electrolyte and the synergistic effect between the components, thereby affecting the improvement of its electrochemical performance and safety performance.
[0146] The results of Comparative Examples 6 to 8 show that the two additives still cannot improve gas production in the lithium-ion battery system, and the sum of their effects on the electrochemical performance is significantly inferior to the combined effect of the three additives in Example 6; thus, it can be seen that the components of the alkaline ion secondary battery electrolyte provided by the present invention can also play a significant synergistic role in the lithium-ion battery system.
[0147] According to the above comparison, the alkali ion secondary battery electrolyte provided by the present invention can achieve the effect of inhibiting flatulence through the synergistic effect between the anti-flatulence additives, thereby improving the electrochemical properties such as cycle performance and first effect. Since the above-mentioned alkali ion secondary battery electrolyte has the above advantages, the alkali ion secondary battery prepared therefrom also has good electrochemical performance and safety performance, and is expected to be widely used in the fields of energy storage, power batteries and small household appliances.
[0148] The above is a detailed description of the embodiments of the present invention, but the present invention is not limited to the above embodiments. Various changes can be made within the knowledge of ordinary technicians in the relevant technical field without departing from the purpose of the present invention. In addition, the embodiments of the present invention and the features in the embodiments can be combined with each other without conflict.
Claims
1. An alkali ion secondary battery electrolyte, characterized in that: The raw materials for preparing the electrolyte of the alkali ion secondary battery include active alkali metal salt, organic solvent and anti-flatulence additive; The anti-flatulence additives include polyhydroxyphenol additives, fluoroethylene carbonate and organosilicon nitrile; The anti-flatulence additive accounts for ≤8.5% of the mass percentage of the electrolyte of the alkali ion secondary battery.
2. The alkaline ion secondary battery electrolyte according to claim 1, characterized in that: In the structural formula of the polyhydroxyphenol additive, the number of hydroxyl groups is ≥5; and / or, the structural formula of the polyhydroxyphenol additive is as shown in Formula I: Wherein, R is selected from at least one of methyl, vinyl and the structure shown in formula II:
3. The alkaline ion secondary battery electrolyte according to claim 1 or 2, characterized in that: The molecular weight of the polyhydroxyphenol additive is 200-2500; and / or the mass percentage of the polyhydroxyphenol additive in the alkaline ion secondary battery electrolyte is 0.6-2.8%.
4. The alkaline ion secondary battery electrolyte according to claim 1, characterized in that: The mass percentage of the fluoroethylene carbonate in the electrolyte of the alkali ion secondary battery is 0.1-6.7%.
5. The alkaline ion secondary battery electrolyte according to claim 1, characterized in that: The structural formula of the organosilicon nitrile As shown in formula III: Wherein, R4 is selected from one of an aromatic group or an aliphatic ring; R1, R2, and R3 are independently selected from at least one of methyl, vinyl, and halogen; n is selected from any integer between 1 and 5.
6. The alkaline ion secondary battery electrolyte according to claim 1, characterized in that: The mass percentage of the organic silicon nitrile in the electrolyte of the alkali ion secondary battery is 1.2-5.6%.
7. The alkaline ion secondary battery electrolyte according to claim 1, characterized in that: The active alkali metal salt includes at least one of a lithium salt, a sodium salt and a potassium salt; and / or the sodium salt includes at least one of sodium hexafluorophosphate, lithium tetrafluoroborate, sodium hexafluoroarsenate, sodium perchlorate, sodium bis(oxalatoborate), sodium difluorooxalatoborate, sodium difluorophosphate, sodium bis(fluorosulfonyl)imide and sodium bis(trifluoromethylsulfonyl)imide.
8. A method for preparing an alkali ion secondary battery electrolyte according to any one of claims 1 to 7, characterized in that: The preparation method comprises mixing the raw materials for preparing the alkali ion secondary battery electrolyte.
9. An alkali ion secondary battery, characterized in that: The raw materials for preparing the alkali ion secondary battery include the alkali ion secondary battery electrolyte according to any one of claims 1 to 7.
10. The alkali ion secondary battery according to claim 9, characterized in that: The alkali ion secondary battery includes at least one of a lithium ion battery, a sodium ion battery and a potassium ion battery.