Stretchable solid-state battery based on fractal structure and preparation method thereof
By adopting a fractal structure of stretchable solid-state batteries in lithium-ion batteries, combined with parallel multi-spray head 3D printing technology, the stability and safety of lithium-ion batteries under tensile deformation are solved, and the battery is realized in wearable devices and reduce manufacturing complexity and safety risks.
Patent Information
- Application Number
- CN202411334248.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-24
- Publication Date
- 2024-11-12
AI Technical Summary
Existing lithium-ion batteries cannot operate stably under tensile deformation, and organic liquid electrolytes have safety risks, making it difficult to meet the needs of wearable electronic products.
Using a stretchable solid-state battery based on fractal structure, the printing ink of lithium iron phosphate positive electrode, lithium titanate negative electrode and solid electrolyte are prepared, combined with parallel multi-tip 3D printing technology, a battery with Hilbert curve structure is printed, using solid-state Electrolyte eliminates the safety risks of liquid electrolytes and achieves stable interface contact between electrodes and electrolytes.
The integrity and rapid recovery of the battery structure after tensile deformation at different angles is achieved, which reduces the internal resistance of the battery, improves safety, is suitable for wearable electronic products power supplies, and simplifies the manufacturing process.
Smart Images

Figure CN118943504A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of new energy batteries, and specifically to a stretchable solid-state battery based on a fractal structure and a preparation method thereof. Background Art
[0002] Wearable electronics are the development trend of next-generation electronic products and the Internet of Things, and have attracted great interest from industry and academia in the past decade. Some typical wearable electronic products, such as wearable fabrics, artificial skin, soft robots, etc., need to ensure safe and stable operation under tensile deformation so that they can be worn on the body surface or installed in the body. An essential component of these electronic products is the battery that provides energy. Ideally, in order to meet the above-mentioned stretchable requirements, the battery should have flexibility and stretchability similar to that of the device. However, lithium-ion batteries, as the mature power source for most portable electronic products, usually have a rigid laminated structure in their internal structure, which is not only bulky but also cannot be stretched.
[0003] In order to meet the requirements of the tensile deformation characteristics of wearable electronic products, it is very important to produce lithium-ion batteries with stretchable functions. At present, there are two strategies for the design of stretchable lithium-ion batteries. One is to find stretchable materials, such as polymers, and compound them with conductive agents and battery active materials as electrodes. However, the stretching rate of electrodes and batteries obtained by this strategy is usually extremely limited, and the introduced stretchable polymers are inactive components, which greatly reduces the overall energy density of the battery. Another strategy is to design stretchable electrode structures from the perspective of electrode structure, such as origami structures, arch structures, serpentine structures, etc. This strategy is easy to obtain a large tensile deformation rate, and the electrode structure can be completely restored after the tensile force is removed. However, the process of manufacturing these stretchable batteries with unconventional structures is usually complicated, and it is difficult to achieve large-scale, low-cost manufacturing. Therefore, it is necessary to find a lower-cost, high-efficiency, and convenient method for preparing stretchable electrodes.
[0004] In addition, the electrolytes of stretchable batteries are still mainly organic liquid electrolytes, which pose great safety risks and are prone to fire and explosion risks under high temperatures and battery damage.
[0005] In summary, the development of a stretchable solid-state battery and its preparation method is extremely necessary for the development of wearable electronic products.
[0006] The information in this background technology section is only intended to enhance the understanding of the overall background of the application and should not be construed as an admission or any form of suggestion that the information constitutes the prior art already known to a person of ordinary skill in the art. Summary of the invention
[0008] Based on the technical problems mentioned in the above background, the present application provides a stretchable solid-state battery based on a fractal structure and a preparation method thereof.
[0009] In some embodiments of the present application, a method for preparing a stretchable solid-state battery based on a fractal structure is provided, comprising the following steps: S1. Preparation of lithium iron phosphate positive electrode, lithium titanate negative electrode and solid electrolyte printing ink, specifically comprising the following steps: S11. Preparation of positive electrode printing ink: The positive electrode printing ink is composed of an active material, lithium iron phosphate, a conductive agent and a binder. After the above powder is dispersed in an organic solvent, a positive electrode printing ink having a suitable viscosity and fluidity is obtained; S12. Preparation of negative electrode printing ink: The negative electrode printing ink is composed of an active material, lithium titanate, a conductive agent and a binder. After the above powder is dispersed in an organic solvent, a negative electrode printing ink having suitable viscosity and fluidity is obtained; S13. Preparation of solid electrolyte ink: polyvinylidene fluoride - hexafluoropropylene (PVDF-HFP) and lithium salt are sequentially added to an organic solvent, and magnetically stirred for a certain period of time under heating conditions to obtain a uniform solid electrolyte ink; S2. Printing of fractal structure stretchable solid-state battery based on parallel multi-nozzle, specifically including the following steps: S21. The positive electrode printing ink, negative electrode printing ink and solid electrolyte ink in S1 are respectively loaded into the positive electrode, negative electrode and solid electrolyte printing barrels, fixed to the 3D printer, and connected to the air pressure tube, and the printing ink is uniformly extruded under the push of air pressure, and the ink is printed on the printing substrate; S22. According to the fractal structure printing path set by the computer, the lithium iron phosphate positive electrode, the solid electrolyte and the lithium titanate negative electrode are arranged in parallel and printed according to the preset fractal structure; S23. placing the printed fractal structure in an oven to remove the solvent; S3. Stretchable battery encapsulation: After mixing polydimethylsiloxane and curing agent in a culture dish, pour them directly onto the dried battery surface; then, cure them under heating conditions to achieve stretchable battery encapsulation.
[0010] In some embodiments of the present application, the fractal structure refers to a continuous curve with a specific structure on a plane, and the stretchable structure, that is, the internal structure of the battery presents a fractal structure, which can produce stable deformation under the action of a stretching force. After the stretching force is removed, the battery can return to its initial state.
[0011] In some embodiments of the present application, the organic solvent in S11 and S12 is N-methylpyrrolidone; the organic solvent in S13 is polydimethylformamide (DMF).
[0012] In some embodiments of the present application, in S22, the preset fractal structure is a plane geometric shape composed of Hilbert curves.
[0013] In some embodiments of the present application, in step S11, the conductive agent is a combination of one or more of Super P, Ketjen black, carbon nanotubes, and graphene.
[0014] In some embodiments of the present application, in step S11, the binder is polyvinylidene fluoride.
[0015] In some embodiments of the present application, in step S11, the mass fraction of the lithium iron phosphate is 60-90 wt%, the mass fraction of the conductive agent is 5-35 wt%, and the mass fraction of the binder is 5-10 wt%.
[0016] In some embodiments of the present application, in step S12, the conductive agent is a combination of one or more of Super P, Ketjen black, carbon nanotubes, and graphene.
[0017] In some embodiments of the present application, in step S12, the binder is polyvinylidene fluoride.
[0018] In some embodiments of the present application, in step S12, the mass fraction of the lithium titanate is 60-90 wt%, the mass fraction of the conductive agent is 5-35 wt%, and the mass fraction of the binder is 5-10 wt%.
[0019] In some embodiments of the present application, in step S13, the mass ratio of PVDF-HFP to lithium salt is 1:1 to 10:1.
[0020] In some embodiments of the present application, in step S13, the heating temperature is 40-60°C and the heating time is 4-12h.
[0021] In some embodiments of the present application, in step S13, the lithium salt is one or more combinations of lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethylsulfonyl)imide, lithium tetrafluoroborate, lithium perchlorate, and lithium hexafluorophosphate.
[0022] In some embodiments of the present application, in step S21, a polydimethylsiloxane film is selected as the printing substrate, and the polydimethylsiloxane film is prepared by a heat curing method. Specifically, uncured polydimethylsiloxane and a curing agent are mixed in a mass ratio of 10:1, stirred evenly in a culture dish, and then placed in a vacuum oven to complete heat curing; the curing temperature is 60-120°C, and the curing time is 30-150 min.
[0023] In some embodiments of the present application, in step S23, the heating temperature is 60-100°C, and the heating time is 6-24h.
[0024] In some embodiments of the present application, in S22, the printing needle diameter is 200-400 μm, the number of printing layers is 1 layer, the printing height is 400 μm, the printing line width is 200-400 μm, the printing speed is 3-5 mm / s, and the air compressor provides an air pressure of 200-300 kPa; In some embodiments of the present application, the mass ratio of polydimethylsiloxane to curing agent in S23 is 10:1, the curing temperature is 60-120° C., and the curing time is 30-150 min.
[0025] In some embodiments of the present application, the preparation of the polydimethylsiloxane in S23 refers to the preparation in S21.
[0026] In other embodiments of the present application, a stretchable solid-state battery prepared by the above-mentioned preparation method is provided.
[0027] The advantages and beneficial effects of this application are as follows: 1. The battery proposed in this application has a fractal structure of a plane geometric shape composed of Hilbert curves, which can keep the battery structure intact under tensile deformation at different angles. Moreover, when the tensile force is removed, the battery structure quickly returns to its initial state. The tensile deformation process has little effect on the battery performance, and is very suitable for the power supply of wearable electronic products.
[0028] 2. To improve battery safety, the battery electrolyte uses a solid electrolyte. The lithium iron phosphate positive electrode, solid electrolyte and lithium titanate negative electrode are arranged in parallel, all forming a fractal structure according to the Hilbert curve; it can eliminate the safety risks brought by liquid organic electrolytes and is more suitable for close-fitting or built-in placement on the human body.
[0029] 3. The stretchable battery preparation method proposed in this application is a parallel multi-nozzle 3D printing technology, which can print the positive electrode, negative electrode and solid electrolyte at the same time in one step. In addition, the stable interface contact between the electrode and the electrolyte reduces the solid-solid interface impedance and greatly reduces the internal resistance of the battery.
[0030] 4. The printing method of this application has great application potential in the fields of wearable electronic products, electronic skin, etc. The proposed manufacturing method has a simple process and high efficiency. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] The drawings described herein are used to provide a further understanding of the embodiments of the present application, constitute a part of the present application, and do not constitute a limitation on the embodiments of the present application. In the drawings: Figure 1 A schematic diagram of a method for preparing a stretchable solid-state battery based on a fractal structure in some embodiments of the present application; Figure 2Schematic diagram of a stretchable battery with a fractal structure in some embodiments of the present application. DETAILED DESCRIPTION
[0032] In order to make the purpose, technical solutions and advantages of the present application more clearly understood, the present application is described in detail in some embodiments of the present application in combination with the embodiments and drawings. The schematic implementation methods of the present application and their description are only used to explain the present application and are not intended to limit the present application.
[0033] In the present application, the terms "comprises", "comprising" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, article or device including a series of elements includes not only those elements, but also includes other elements not explicitly listed, or also includes elements inherent to such process, article or device. In the absence of further restrictions, an element defined by the sentence "comprising a ..." does not exclude the presence of other identical elements in the process, article or device including the element.
[0034] In the embodiments of the present application, words such as "exemplary" or "for example" are used to indicate examples, illustrations or descriptions. Any embodiment or design scheme described as "exemplary" or "for example" in the embodiments of the present application should not be interpreted as being more preferred or more advantageous than other embodiments or designs. Specifically, the use of words such as "exemplary" or "for example" is intended to present related concepts in a specific way.
[0035] Based on the embodiments in this application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments is not specified, they are all conventional products that can be purchased commercially.
[0036] In some embodiments of the present application, a method for preparing a stretchable solid-state battery based on a fractal structure is provided, comprising the following steps: S1. Preparation of lithium iron phosphate positive electrode, lithium titanate negative electrode and solid electrolyte printing ink, specifically comprising the following steps: S11. Preparation of positive electrode printing ink: The positive electrode printing ink is composed of an active material, lithium iron phosphate, a conductive agent and a binder. After the above powder is dispersed in an organic solvent, a positive electrode printing ink having a suitable viscosity and fluidity is obtained; S12. Preparation of negative electrode printing ink: The negative electrode printing ink is composed of an active material, lithium titanate, a conductive agent and a binder. After the above powder is dispersed in an organic solvent, a negative electrode printing ink having suitable viscosity and fluidity is obtained; S13. Preparation of solid electrolyte ink: polyvinylidene fluoride - hexafluoropropylene (PVDF-HFP) and lithium salt are sequentially added to an organic solvent, and magnetically stirred for a certain period of time under heating conditions to obtain a uniform solid electrolyte ink; S2. Printing of fractal structure stretchable solid-state battery based on parallel multi-nozzle, specifically including the following steps: S21. The positive electrode printing ink, negative electrode printing ink and solid electrolyte ink in S1 are respectively loaded into the positive electrode, negative electrode and solid electrolyte printing barrels, fixed to the 3D printer, and connected to the air pressure tube, and the printing ink is uniformly extruded under the push of air pressure, and the ink is printed on the printing substrate; S22. According to the fractal structure printing path set by the computer, the lithium iron phosphate positive electrode, the solid electrolyte and the lithium titanate negative electrode are arranged in parallel and printed according to the preset fractal structure; S23. placing the printed fractal structure in an oven to remove the solvent; S3. Stretchable battery encapsulation: After mixing polydimethylsiloxane and curing agent in a culture dish, pour them directly onto the dried battery surface; then, cure them under heating conditions to achieve stretchable battery encapsulation.
[0037] In some embodiments of the present application, the fractal structure refers to a continuous curve with a specific structure on a plane, and the stretchable structure, that is, the internal structure of the battery presents a fractal structure, which can produce stable deformation under the action of a stretching force. After the stretching force is removed, the battery can return to its initial state.
[0038] In some embodiments of the present application, the organic solvent in S11 and S12 is N-methylpyrrolidone; the organic solvent in S13 is polydimethylformamide (DMF).
[0039] In some embodiments of the present application, in S22, the preset fractal structure is a plane geometric shape composed of Hilbert curves.
[0040] In some embodiments of the present application, in step S11, the conductive agent is a combination of one or more of Super P, Ketjen black, carbon nanotubes, and graphene.
[0041] In some embodiments of the present application, in step S11, the binder is polyvinylidene fluoride.
[0042] In some embodiments of the present application, in step S11, the mass fraction of the lithium iron phosphate is 60-90 wt%, the mass fraction of the conductive agent is 5-35 wt%, and the mass fraction of the binder is 5-10 wt%.
[0043] In some embodiments of the present application, in step S12, the conductive agent is a combination of one or more of Super P, Ketjen black, carbon nanotubes, and graphene.
[0044] In some embodiments of the present application, in step S12, the binder is polyvinylidene fluoride.
[0045] In some embodiments of the present application, in step S12, the mass fraction of the lithium titanate is 60-90 wt%, the mass fraction of the conductive agent is 5-35 wt%, and the mass fraction of the binder is 5-10 wt%.
[0046] In some embodiments of the present application, in step S13, the mass ratio of PVDF-HFP to lithium salt is 1:1 to 10:1.
[0047] In some embodiments of the present application, in step S13, the heating temperature is 40-60°C and the heating time is 4-12h.
[0048] In some embodiments of the present application, in step S13, the lithium salt is one or more combinations of lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethylsulfonyl)imide, lithium tetrafluoroborate, lithium perchlorate, and lithium hexafluorophosphate.
[0049] In some embodiments of the present application, in step S21, a polydimethylsiloxane film is selected as the printing substrate, and the polydimethylsiloxane film is prepared by a heat curing method. Specifically, uncured polydimethylsiloxane and a curing agent are mixed in a mass ratio of 10:1, stirred evenly in a culture dish, and then placed in a vacuum oven to complete heat curing; the curing temperature is 60-120°C, and the curing time is 30-150 min.
[0050] In some embodiments of the present application, in step S23, the heating temperature is 60-100°C, and the heating time is 6-24h.
[0051] In some embodiments of the present application, in S22, the printing needle diameter is 200-400 μm, the number of printing layers is 1 layer, the printing height is 400 μm, the printing line width is 200-400 μm, the printing speed is 3-5 mm / s, and the air compressor provides an air pressure of 200-300 kPa; In some embodiments of the present application, the mass ratio of polydimethylsiloxane to curing agent in S23 is 10:1, the curing temperature is 60-120° C., and the curing time is 30-150 min.
[0052] In some embodiments of the present application, the preparation of the polydimethylsiloxane in S23 refers to the preparation in S21.
[0053] In other embodiments of the present application, a stretchable solid-state battery prepared by the above-mentioned preparation method is provided.
[0054] In some embodiments of the present application, a method for preparing a stretchable solid-state battery based on a fractal structure is characterized by comprising the following steps: S1. Preparation of lithium iron phosphate positive electrode, lithium titanate negative electrode and solid electrolyte printing ink: S11. Preparation of positive electrode printing ink. The active material lithium iron phosphate, the conductive agent Super P and the binder polyvinylidene fluoride are evenly ground in a mass ratio of 8:1:1, and the above powders are dispersed in N-methylpyrrolidone to obtain a positive electrode printing ink with suitable viscosity and fluidity.
[0055] S12. Preparation of negative electrode printing ink. The active material lithium titanate, the conductive agent Super P and the binder polyvinylidene fluoride are evenly ground in a mass ratio of 8:1:1, and the above powders are dispersed in N-methylpyrrolidone to obtain a negative electrode printing ink with suitable viscosity and fluidity.
[0056] S13. Preparation of solid electrolyte ink. PVDF-HFP and lithium bis(fluorosulfonyl)imide were added to polydimethylformamide (DMF) in a mass ratio of 5:1, and magnetically stirred at 50°C for 12 h to obtain a uniform high-voltage cathode-compatible solid electrolyte ink.
[0057] S2. Parallel multi-nozzle printing of stretchable solid-state batteries with fractal structures.
[0058] S21. Preparation of polydimethylsiloxane film on printing substrate. Uncured polydimethylsiloxane and curing agent were mixed in a culture dish and cured after degassing. The mass ratio of polydimethylsiloxane to curing agent was 10:1, the curing temperature was 120 °C, and the curing time was 30 min.
[0059] S22. Load the positive electrode, negative electrode and solid electrolyte ink described in S1 into the positive electrode, negative electrode and solid electrolyte printing cartridges respectively, fix them to the 3D printer, and connect the air pressure tube.
[0060] S23. Print on the polydimethylsiloxane film according to the good printing path set by the computer, that is, the fractal structure. The printing needle diameter is 200 μm, the number of printing layers is 1, the printing height is 400 μm, the printing line width is 200 μm, the printing speed is 4 mm / s, and the air compressor provides an air pressure of 200 kPa.
[0061] S23. Place the printed electrode in an oven and dry it at 80°C for 24 hours to remove the solvent.
[0062] S3. Stretchable battery encapsulation. Referring to the preparation method of polydimethylsiloxane film in S21, uncured polydimethylsiloxane and curing agent are mixed in a culture dish and poured directly onto the surface of the dried battery. Finally, it is cured under heating conditions to achieve the encapsulation of the stretchable battery. The mass ratio of polydimethylsiloxane to curing agent is 10:1, the curing temperature is 50°C, and the curing time is 120 min.
[0063] The specific implementation methods described above further illustrate the purpose, technical solutions and beneficial effects of the present application in detail. It should be understood that the above description is only the specific implementation method of the present application and is not intended to limit the scope of protection of the present application. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present application should be included in the scope of protection of the present application.
Claims
1. A method for preparing a stretchable solid-state battery based on a fractal structure, characterized in that: The following steps are involved: S1. Preparation of lithium iron phosphate positive electrode, lithium titanate negative electrode and solid electrolyte printing ink, specifically comprising the following steps: S11. Preparation of positive electrode printing ink: The positive electrode printing ink is composed of an active material, lithium iron phosphate, a conductive agent and a binder. After the above powder is dispersed in an organic solvent, a positive electrode printing ink having a suitable viscosity and fluidity is obtained; S12. Preparation of negative electrode printing ink: The negative electrode printing ink is composed of an active material, lithium titanate, a conductive agent and a binder. After the above powder is dispersed in an organic solvent, a negative electrode printing ink having suitable viscosity and fluidity is obtained; S13. Preparation of solid electrolyte ink: polyvinylidene fluoride - hexafluoropropylene (PVDF-HFP) and lithium salt are sequentially added to an organic solvent, and magnetically stirred for a certain period of time under heating conditions to obtain a uniform solid electrolyte ink; S2. Printing of fractal structure stretchable solid-state battery based on parallel multi-nozzle, specifically including the following steps: S21. The positive electrode printing ink, negative electrode printing ink and solid electrolyte ink in S1 are respectively loaded into the positive electrode, negative electrode and solid electrolyte printing barrels, fixed to the 3D printer, and connected to the air pressure tube, and the printing ink is uniformly extruded under the push of air pressure, and the ink is printed on the printing substrate; S22. According to the fractal structure printing path set by the computer, the lithium iron phosphate positive electrode, the solid electrolyte and the lithium titanate negative electrode are arranged in parallel and printed according to the preset fractal structure; S23. placing the printed fractal structure in an oven to remove the solvent; S3. Stretchable battery packaging: After mixing polydimethylsiloxane and curing agent, pour them directly onto the dried battery surface, heat and cure them to achieve stretchable battery packaging.
2. The method for preparing a stretchable solid-state battery based on a fractal structure according to claim 1, characterized in that: The fractal structure refers to a continuous curve with a specific structure on a plane. The stretchable structure, i.e., the internal structure of the battery, presents a fractal structure, which can produce stable deformation under the action of a stretching force. After the stretching force is removed, the battery can return to its initial state. Preferably, in S22, the preset fractal structure is a plane geometric shape composed of Hilbert curves.
3. The method for preparing a stretchable solid-state battery based on a fractal structure according to claim 1, characterized in that: The organic solvent in S11 and S12 is N-methylpyrrolidone; the organic solvent in S13 is polydimethylformamide (DMF); In step S11, the conductive agent is a combination of one or more of Super P, Ketjen Black, carbon nanotubes, and graphene; In step S11, the binder is polyvinylidene fluoride; in step S11, the mass fraction of lithium iron phosphate is 60-90wt%, the mass fraction of the conductive agent is 5-35wt%, and the mass fraction of the binder is 5-10wt%.
4. The method for preparing a stretchable solid-state battery based on a fractal structure according to claim 1, characterized in that: In step S12, the conductive agent is a combination of one or more of Super P, Ketjen Black, carbon nanotubes, and graphene; In step S12, the binder is polyvinylidene fluoride; In step S12, the mass fraction of the lithium titanate is 60-90wt%, the mass fraction of the conductive agent is 5-35wt%, and the mass fraction of the binder is 5-10wt%.
5. The method for preparing a stretchable solid-state battery based on a fractal structure according to claim 1, characterized in that: In step S13, the mass ratio of PVDF-HFP to lithium salt is 1:1 to 10:1; in step S13, the heating temperature is 40-60°C, and the heating time is 4-12h; in step S13, the lithium salt is one or more combinations of lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethylsulfonyl)imide, lithium tetrafluoroborate, lithium perchlorate, and lithium hexafluorophosphate.
6. The method for preparing a stretchable solid-state battery based on a fractal structure according to claim 1, characterized in that: In step S21, the printing substrate is a polydimethylsiloxane film, and the polydimethylsiloxane film is prepared by a heating curing method. Specifically, uncured polydimethylsiloxane and a curing agent are mixed in a mass ratio of 10:1, stirred evenly in a culture dish, and then placed in a vacuum oven to complete heating curing; the curing temperature is 60-120° C., and the curing time is 30-150 min; 7. The method for preparing a stretchable solid-state battery based on a fractal structure according to claim 1, characterized in that: In step S23, the heating temperature is 60-100°C and the heating time is 6-24h.
8. The method for preparing a stretchable solid-state battery based on a fractal structure according to claim 1, characterized in that: In the S22, the printing needle diameter is 200-400 μm, the number of printing layers is 1, the printing height is 400 μm, the printing line width is 200-400 μm, the printing speed is 3-5 mm / s, and the air compressor provides an air pressure of 200-300 kPa.
9. The method for preparing a stretchable solid-state battery based on a fractal structure according to claim 1, characterized in that: The mass ratio of polydimethylsiloxane to curing agent in S23 is 10:1, the curing temperature is 60-120° C., and the curing time is 30-150 min.
10. A stretchable solid-state battery, characterized in that: It is prepared using the preparation method described in any one of claims 1 to 9.