Modified diaphragm lithium-sulfur button cell and preparation method thereof
By making vacant positions in CoSe2 and doping P, P-CS-NaBH4 catalyst was prepared for the modification of the separator of lithium sulfur batteries, the problems of lithium polysulfide shuttle effect and uneven metal lithium deposition in lithium sulfur batteries were solved, and the Cycling performance and safety of the battery.
Patent Information
- Application Number
- CN202411081678.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-08
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-08-08
AI Technical Summary
It is difficult to effectively suppress the shuttle effect of lithium polysulfide and the uneven deposition of metal lithium, which affects the cycling performance and safety of the battery.
By creating vacancies in CoSe2 and inducing P doping, P-CS-NaBH4 catalyst was prepared for separator modification of lithium sulfur batteries, promoting rapid nucleation and decomposition of lithium sulfide, and improving polysulfide adsorption and catalytic conversion. process.
It effectively inhibits the shuttle effect, improves the nucleation and decomposition capacity of Li2S, enhances the redox kinetics of polysulfides, and improves the cycling performance and safety of the battery.
Smart Images

Figure CN118943643A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of battery materials, and in particular to a modified diaphragm lithium-sulfur button battery and a preparation method thereof. Background Art
[0002] Lithium-sulfur batteries have the advantages of high theoretical specific capacity, high specific energy, abundant natural reserves of raw materials, environmental friendliness, and low preparation cost. They are the research hotspot of the next generation of energy storage systems. However, some defects hinder the large-scale commercial application of lithium-sulfur batteries. In lithium-sulfur batteries, the separator not only acts as an electrolyte storage device, but also promotes the transfer of Li + The modified functional membrane also has a large number of active sites for adsorbing polysulfide ions, which promotes the formation of lithium polysulfide and inhibits the shuttling to the lithium negative electrode. In addition, the functional modified separator can also induce the uniform deposition of metallic lithium, inhibit the growth of lithium dendrites, and improve the cycle performance and safety of the battery.
[0003] Various catalysts, such as oxides, carbides, nitrides, sulfides, etc., have inherent properties that make it difficult for them to meet the requirements of high catalytic performance due to the slow redox kinetics of sulfur. Transition metal selenides have both sulfur-philic and lithium-philic sites. The sulfur-philic sites can effectively adsorb polysulfides to reduce the shuttle effect, while the lithium-philic sites can reduce the nucleation barrier of lithium sulfide and induce the uniform deposition of lithium ions on the negative electrode side. Therefore, transition metal selenides have become a hot topic in current research.
[0004] Based on this, this application is approved by CoSe 2 Vacancies were created in the solution and P was induced to dope to obtain the corresponding composite material, P-CS-NaBH 4 Catalysts and used for diaphragm modification of lithium-sulfur batteries. It catalyzes the rapid nucleation and decomposition of lithium sulfide, increases the nucleation and decomposition capacity, effectively improves the adsorption and catalytic conversion process of polysulfides, and thus inhibits the shuttle effect. Summary of the invention
[0005] The purpose of the present invention is to provide a modified diaphragm lithium-sulfur button battery and a preparation method thereof, and to prepare P-CS-NaBH 4 Catalysts and used for separator modification of lithium-sulfur batteries.
[0006] The embodiment of the present application discloses a modified diaphragm lithium-sulfur button cell and a preparation method thereof, comprising a negative electrode (lithium sheet), a positive electrode and an electrolyte, and a modified diaphragm.
[0007] Preferably, the positive electrode is prepared by: mixing S and carbon nanotubes (CNT) in a mass ratio of 8:2, and heating at 155°C for 16 h to obtain an S / CNT composite material; adding S / CNT, Super P and PVDF in a mass ratio of 7:2:1 in an NMP solvent to obtain a slurry; applying the slurry on aluminum foil, placing it in an oven at 50°C for 12 h, and cutting it into discs with a diameter of 12 mm.
[0008] Preferably, the electrolyte comprises 0.5 M LiTFSI and LiNO 3 A solution of 1,3-dioxolane and ethylene glycol dimethyl ether (1:1 by volume).
[0009] Preferably, the modified diaphragm preparation method comprises the following steps: S1 Preparation of ZIF-67, etching of ZIF-67 with tannic acid to obtain a hollow structure and in-situ selenization to obtain a hollow cubic structure of CoSe 2 ; S2 The prepared CoSe was mixed in a mass volume ratio of 1mg:1ml 2 At different concentrations of NaBH 4 The mixture was immersed in the solution for 30 min, washed with deionized water for several times, and dried at 60 °C for 8-16 h to obtain material A; S3 NaH with a mass ratio of 1:1 2 PO 2 The materials A and S2 were placed in the upstream and downstream of the tube furnace respectively, and P-CS-NaH 2 PO 2 Composite materials; S4 P-CS-NaH 2 PO 2 The composite material powder, Super P and PVDF are added into NMP solvent in proportion to obtain a mixed slurry; S5 coated the slurry on the PP diaphragm, and the material loading was about 0.5 mg / cm 2 , then dried and cut into discs with a diameter of 19 mm to obtain the modified diaphragm.
[0010] Furthermore, the preparation method of ZIF-67 in step S1 is: weigh Co(NO 3 ) 2 6H 2O and hexadecyltrimethylammonium bromide were added to deionized water and stirred to obtain solution A; 2-methylimidazole was added to deionized water in proportion and stirred to obtain solution B; solution A was poured into solution B and stirred at high speed for 40 min to obtain a purple suspension; ethanol was used for centrifugal washing six times to obtain a purple substance, which was dried under vacuum at 60°C to obtain ZIF-67.
[0011] Furthermore, in step S1, CoSe 2 Preparation: Hollow ZIF-67 and selenium powder were placed in a crucible at a mass ratio of 1:3 and heated in H 2 / Ar protective atmosphere, and then heated at 450℃ for 2 h (heating rate of 2℃ / min) to obtain CoSe 2 .
[0012] Furthermore, the heating system in step S3 is: heating at 300-400° C. for 1.5-3 h under Ar protective atmosphere.
[0013] Furthermore, in step S4, P-CS-NaH 2 PO 2 The mass ratio of composite material powder, Super P and PVDF is 5:4:1.
[0014] Furthermore, the drying temperature in step S4 is 45-60° C., and the drying time is 10-16 h.
[0015] The invention has the advantages that ZIF-67 is etched with tannic acid to obtain a hollow structure and then subjected to in-situ selenization treatment to obtain a hollow cubic structure of CoSe. 2 , followed by NaBH 4 Vacancies were created and P doping was induced to obtain the P-CS-0.5 catalyst. P-CS-0.5 can catalyze the rapid nucleation and decomposition of lithium sulfide, increase the nucleation and decomposition capacity, effectively improve the adsorption and catalytic conversion process of polysulfides, and thus inhibit the shuttle effect. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0017] Figure 1 The figure shows the SEM spectrum of the diaphragm material prepared in Example 2, where (a) is the PP film and (b) is the prepared P-CS-0.5 modified diaphragm; Figure 2 (a) Li of different materials obtained in Examples 1-3: CS, CS-0.1, CS-0.5, CS-1 and P-CS-0.5 2 S deposition curve and (b) Li 2 S-decomposition curve; Figure 3 Shown are the CV curves of different batteries of different materials obtained in Examples 1-3 at a scan rate of 0.1 mV s-1; Figure 4 Shown are (a) in situ Raman spectrum and (b) Raman contour map of the P-CS-0.5 modified membrane obtained in Example 2 at 0.5°C. DETAILED DESCRIPTION
[0018] The following will describe the technical solutions in the embodiments of the present invention in detail in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0019] Example 1 Preparation of S1 ZIF-67: 300 mg Co(NO 3 ) 2 6H 2 O and 15 mg hexadecyltrimethylammonium bromide were added to 20 mL of deionized water and stirred to obtain solution A; 908 mg of 2-methylimidazole was added to 140 mL of deionized water and stirred to obtain solution B; solution A was poured into solution B and stirred at high speed for 40 min to obtain a purple suspension; ethanol was used for centrifugal washing six times to obtain a purple substance, which was dried at 60°C under vacuum for 12 h to obtain ZIF-67.
[0020] S2 Preparation of hollow ZIF-67: The prepared ZIF-67 was dispersed in 20 mL of ethanol, and then poured into 160 mL of a mixed solution of ethanol and deionized water containing 1 mg / mL tannic acid, stirred at room temperature for 15 min, and the product was collected by centrifugation and washed several times with ethanol to obtain a hollow structured ZIF-67.
[0021] S3 CoSe 2 Preparation: Hollow ZIF-67 and selenium powder (mass ratio of 1:3) were placed in a crucible and heated in H 2 CoSe was obtained by heating at 450℃ for 2 h (heating rate of 2℃ / min) under Ar atmosphere. 2 ; 50 mg of prepared CoSe2 In 50 mL of NaBH 4 The resulting product was immersed in a 0.1 mol / L solution for 30 min, washed with deionized water for several times, and dried at 60 °C overnight to obtain the target material (CS-0.1).
[0022] Preparation of S4 P-CS-0.1 composite material: NaH 2 PO 2 and CS-0.1 were placed in the upstream and downstream of the tube furnace respectively, and after heating at 350 °C in Ar atmosphere for 2 h, P-CS-0.1 was obtained.
[0023] Preparation of S5 modified membrane: P-CS-0.1 powder, Super P and PVDF were added to NMP solvent in a mass ratio of 5:4:1 to obtain a mixed slurry; the slurry was coated on the PP membrane, and the material loading was about 0.5 mg cm -2 , then dried at 50 °C for 12 h and cut into discs with a diameter of 19 mm.
[0024] Preparation of S6 positive electrode material: S and carbon nanotubes (CNTs) were mixed in a mass ratio of 8:2 and heated at 155°C for 16 h to obtain an S / CNT composite material; S / CNT, Super P and PVDF were added to NMP solvent in a mass ratio of 7:2:1 to obtain a slurry; the slurry was coated on aluminum foil, placed in an oven at 50°C for 12 h, and then cut into discs with a diameter of 12 mm.
[0025] Preparation of S7 lithium-sulfur button cell: The S / CNT prepared above was used as the positive electrode, the P-CS-0.5 modified separator was used as the battery separator, the lithium sheet was used as the negative electrode, and the electrolyte contained 0.5 M LiTFSI and LiNO 3 The 1,3-dioxolane and ethylene glycol dimethyl ether (volume ratio of 1:1) solution was used as the electrolyte to complete the assembly of the CR2032 button cell. Example 2
[0026] Preparation of S1 ZIF-67: 300 mg Co(NO 3 ) 2 6H 2 O and 15 mg hexadecyltrimethylammonium bromide were added to 20 mL of deionized water and stirred to obtain solution A; 908 mg of 2-methylimidazole was added to 140 mL of deionized water and stirred to obtain solution B; solution A was poured into solution B and stirred at high speed for 40 min to obtain a purple suspension; ethanol was used for centrifugal washing six times to obtain a purple substance, which was dried at 60°C under vacuum for 12 h to obtain ZIF-67.
[0027] S2 Preparation of hollow ZIF-67: The prepared ZIF-67 was dispersed in 20 mL of ethanol, and then poured into 160 mL of a mixed solution of ethanol and deionized water containing 1 mg / mL tannic acid, stirred at room temperature for 15 min, and the product was collected by centrifugation and washed several times with ethanol to obtain a hollow structured ZIF-67.
[0028] S3 CoSe 2 Preparation: Hollow ZIF-67 and selenium powder (mass ratio of 1:3) were placed in a crucible and heated in H 2 CoSe was obtained by heating at 450℃ for 2 h (heating rate of 2℃ / min) under Ar atmosphere. 2 ; 50 mg of prepared CoSe 2 In 50 mL of NaBH 4 The sample was immersed in a 0.5 mol / L solution for 30 min, washed with deionized water for several times and dried at 60 °C overnight to obtain the target material (CS-0.5).
[0029] Preparation of S4 P-CS-0.5 composite material: NaH 2 PO 2 and CS-0.5 were placed in the upstream and downstream of the tube furnace, respectively, and after heating at 350 °C in Ar atmosphere for 2 h, P-CS-0.5 was obtained.
[0030] Preparation of S5 modified membrane: P-CS-0.5 powder, Super P and PVDF were added to NMP solvent in a mass ratio of 5:4:1 to obtain a mixed slurry; the slurry was coated on the PP membrane, and the material loading was about 0.5 mg cm -2 , then dried at 50 °C for 12 h and cut into discs with a diameter of 19 mm.
[0031] Preparation of S6 positive electrode material: S and carbon nanotubes (CNTs) were mixed in a mass ratio of 8:2 and heated at 155°C for 16 h to obtain an S / CNT composite material; S / CNT, Super P and PVDF were added to NMP solvent in a mass ratio of 7:2:1 to obtain a slurry; the slurry was coated on aluminum foil, placed in an oven at 50°C for 12 h, and then cut into discs with a diameter of 12 mm.
[0032] Preparation of S7 lithium-sulfur button cell: The S / CNT prepared above was used as the positive electrode, the P-CS-0.5 modified separator was used as the battery separator, the lithium sheet was used as the negative electrode, and the electrolyte contained 0.5 M LiTFSI and LiNO 3 The 1,3-dioxolane and ethylene glycol dimethyl ether (volume ratio of 1:1) solution was used as the electrolyte to complete the assembly of the CR2032 button cell. Example 3
[0033] Preparation of S1 ZIF-67: 300 mg Co(NO 3 ) 2 6H 2 O and 15 mg hexadecyltrimethylammonium bromide were added to 20 mL of deionized water and stirred to obtain solution A; 908 mg of 2-methylimidazole was added to 140 mL of deionized water and stirred to obtain solution B; solution A was poured into solution B and stirred at high speed for 40 min to obtain a purple suspension; ethanol was used for centrifugal washing six times to obtain a purple substance, which was dried at 60°C under vacuum for 12 h to obtain ZIF-67.
[0034] S2 Preparation of hollow ZIF-67: The prepared ZIF-67 was dispersed in 20 mL of ethanol, and then poured into 160 mL of a mixed solution of ethanol and deionized water containing 1 mg / mL tannic acid, stirred at room temperature for 15 min, and the product was collected by centrifugation and washed several times with ethanol to obtain a hollow structured ZIF-67.
[0035] S3 CoSe 2 Preparation: Hollow ZIF-67 and selenium powder (mass ratio of 1:3) were placed in a crucible and heated in H 2 CoSe was obtained by heating at 450℃ for 2 h (heating rate of 2℃ / min) under Ar atmosphere. 2 ; 50 mg of prepared CoSe 2 In 50 mL of NaBH 4 The resulting product was immersed in a 1 mol / L solution for 30 min, washed with deionized water for several times, and dried at 60 °C overnight to obtain the target material (CS-1).
[0036] Preparation of S4 P-CS-1 composite material: NaH 2 PO 2 and CS-1 were placed in the upstream and downstream of the tube furnace respectively, and after heating at 350 °C in Ar atmosphere for 2 h, P-CS-1 was obtained.
[0037] Preparation of S5 modified membrane: P-CS-1 powder, Super P and PVDF were added to NMP solvent in a mass ratio of 5:4:1 to obtain a mixed slurry; the slurry was coated on the PP membrane, and the material loading was about 0.5 mg cm -2 , then dried at 50 °C for 12 h and cut into discs with a diameter of 19 mm.
[0038] Preparation of S6 positive electrode material: S and carbon nanotubes (CNTs) were mixed in a mass ratio of 8:2 and heated at 155°C for 16 h to obtain an S / CNT composite material; S / CNT, Super P and PVDF were added to NMP solvent in a mass ratio of 7:2:1 to obtain a slurry; the slurry was coated on aluminum foil, placed in an oven at 50°C for 12 h, and then cut into discs with a diameter of 12 mm.
[0039] Preparation of S7 lithium-sulfur button cell: The S / CNT prepared above was used as the positive electrode, the P-CS-0.5 modified separator was used as the battery separator, the lithium sheet was used as the negative electrode, and the electrolyte contained 0.5 M LiTFSI and LiNO 3 The 1,3-dioxolane and ethylene glycol dimethyl ether (volume ratio of 1:1) solution was used as the electrolyte to complete the assembly of the CR2032 button cell.
[0040] The membrane material prepared in Example 2 was characterized using SEM. Figure 1 As shown in (a) and (b), there are many pores distributed on the original PP diaphragm, and their size is much larger than that of polysulfides, so it is difficult to effectively block polysulfides and inhibit the shuttle effect. After the P-CS-0.5 material is evenly coated on the PP diaphragm, the original pores are completely covered, which can physically block the passage of polysulfides.
[0041] The material was dropped onto carbon paper as the positive electrode and Li 2 S 8 The solution was used as the electrolyte to assemble the battery. 2 S nucleation and decomposition experiments, such as Figure 2 As shown, the battery based on P-CS-0.5 modified separator can promote Li 2 S rapidly nucleates and provides 119 mAh g -1 Li 2 S deposition capacity and 434.1 mAh g -1 The decomposition capacity is higher than that of other materials, indicating that the P-CS-0.5 modified separator can effectively promote the 2 Nucleation and decomposition of S.
[0042] By 0.1 mV s -1 The CV curve under the scanning rate is used to evaluate the reaction kinetics of the battery, such as Figure 3 As shown, the P-CS-0.5 modified membrane exhibits the largest peak current and peak area, and its oxidation peak is located at the lowest potential, indicating that the redox kinetics of polysulfides are significantly enhanced.
[0043] In situ Raman spectroscopy was used to monitor the transformation behavior of polysulfides during discharge and charge. Figure 4As shown, 202, 402 and 451 cm -1 The peak at the Raman shift is attributed to the polysulfides that appear during the charge and discharge process. The weak Raman signal indicates that the polysulfides are rapidly catalytically converted, proving that the P-CS-0.5 modified membrane effectively suppresses the shuttle effect.
[0044] This implementation mode is only an exemplary description of this patent and does not limit its protection scope. Personnel in this field may also make partial changes to it. As long as it does not exceed the spirit of this patent, it shall be regarded as an equivalent replacement of this patent and shall be within the protection scope of this patent.
Claims
1. A modified diaphragm lithium-sulfur button battery and a preparation method thereof, characterized in that: It includes a negative electrode (lithium sheet), a positive electrode and an electrolyte, and a modified diaphragm.
2. The button battery according to claim 1, characterized in that: The positive electrode preparation method is as follows: S and carbon nanotubes (CNT) are mixed in a mass ratio of 8:2, and heated at 155°C for 16 h to obtain an S / CNT composite material; S / CNT, Super P and PVDF are added in a mass ratio of 7:2:1 in an NMP solvent to obtain a slurry; the slurry is coated on an aluminum foil, placed in an oven at 50°C for 12 h, and cut into discs with a diameter of 12 mm.
3. The button battery according to claim 1, characterized in that: The electrolyte is a solution of 1,3-dioxolane and ethylene glycol dimethyl ether (volume ratio is 1:1) containing 0.5 M LiTFSI and LiNO3.
4. The button cell according to claim 1, characterized in that: The modified diaphragm preparation method comprises the following steps: S1. Preparation of ZIF-67. Etching ZIF-67 with tannic acid to obtain a hollow structure and in-situ selenization to obtain CoSe2 with a hollow cubic structure. S2 The prepared CoSe2 was immersed in NaBH4 solutions of different concentrations for 30 min at a mass volume ratio of 1 mg:1 ml, washed with deionized water several times and dried at 60 °C for 8-16 h to obtain material A; S3: placing NaH2PO2 and material A of S2 at a mass ratio of 1:1 at the upstream and downstream of a tube furnace, respectively, and heating to obtain a P-CS-NaH2PO2 composite material; S4 adding P-CS- NaH2PO2 composite material powder, Super P and PVDF into NMP solvent in proportion to obtain a mixed slurry; S5 coated the slurry on the PP diaphragm, and the material loading was about 0.5 mg / cm 2 , then dried and cut into discs with a diameter of 19 mm to obtain the modified diaphragm.
5. The method for preparing a modified diaphragm according to claim 4, characterized in that: The preparation method of ZIF-67 in step S1 is as follows: Co(NO3)2·6H2O and hexadecyltrimethylammonium bromide are weighed in a mass ratio of 20:1, added to deionized water, and stirred to obtain solution A; 2-methylimidazole is added to deionized water in proportion, and stirred to obtain solution B; solution A is poured into solution B, and stirred at high speed for 40 minutes to obtain a purple suspension; The product was washed by centrifugation six times with ethanol to obtain a purple substance, which was then dried under vacuum at 60°C to obtain ZIF-67.
6. The method for preparing a modified diaphragm according to claim 4, characterized in that: Preparation of CoSe2 in step S1: hollow ZIF-67 and selenium powder are placed in a crucible in a mass ratio of 1:3, and heated at 450°C for 2 h (heating rate of 2°C / min) under a H2 / Ar protective atmosphere to obtain CoSe2.
7. The method for preparing a modified diaphragm according to claim 4, characterized in that: The heating system in step S3 is: heating at 300-400° C. for 1.5-3 h under Ar protective atmosphere.
8. The method for preparing a modified diaphragm according to claim 4, characterized in that: In the step S4, the mass ratio of the P-CS-NaH2PO2 composite material powder, Super P and PVDF is 5:4:
1.
9. The method for preparing a modified diaphragm according to claim 4, characterized in that: The drying temperature in step S4 is 45-60° C., and the drying time is 10-16 h.
Citation Information
Patent Citations
Double-effect composite membrane used for lithium sulphur battery and preparation method thereof
CN108461694A
Cobalt diselenide electrocatalyst and preparation method and application thereof
CN115341236A
Separators for use in alkaline cells having high capacity
WO2006088959A2