Electrostatic spinning diaphragm as well as preparation and application thereof

By dissolving PVDF and PVA in DMF and electrospinning and post-treatment, cross-linked structures and pores are formed, the contradiction between the porosity and tensile strength of the electrospinning separator is solved, and the electrochemical performance of the battery is significantly improved.

CN118943645AInactive Publication Date: 2024-11-12HUBEI ENG UNIV

Patent Information

Application Number
CN202411228489.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-03
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Electrospinned separators are difficult to maintain sufficient tensile strength while increasing porosity, limiting their application in high-performance batteries.

Method used

Polyvinylidene fluoride (PVDF) and polyvinyl alcohol (PVA) are dissolved in DMF to form a mixed solution. The composite nanofiber separator is made through electrospinning technology, and heat treatment and ultrasonic washing steps are carried out to form cross-linked structures and holes, and balance it. Porosity and tensile strength.

Benefits of technology

It effectively improves the tensile strength and porosity of the electrospinned separator, improves the electrochemical performance of the battery, and solves the problem that both porosity and tensile strength cannot be taken into account.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005025383760000071
    Figure BDA0005025383760000071
Patent Text Reader

Abstract

The invention discloses an electrostatic spinning diaphragm and preparation and application thereof, and the preparation method comprises the following steps: S1, dispersing polyvinylidene fluoride and polyvinyl alcohol in a solvent to obtain a mixed solution, and carrying out electrostatic spinning on the mixed solution to obtain a composite nanofiber diaphragm; s2, carrying out heating treatment on the composite nanofiber diaphragm to obtain a heat-treated fiber diaphragm; s3, standing the heat-treated fiber diaphragm in deionized water at 95 DEG C for ultrasonic cleaning to obtain an electrostatic spinning diaphragm; polyvinylidene fluoride (PVDF) and polyvinyl alcohol (PVA) are dissolved in DMF to form a mixed solution, an electrostatic spinning technology is used for manufacturing a composite nanofiber diaphragm, then heat treatment and water washing processes are carried out, the tensile strength of the diaphragm is improved through the heat treatment process, the porosity of the diaphragm is improved through the ultrasonic water washing process, and the composite nanofiber diaphragm is obtained. The problem that porosity and tensile strength cannot be considered at the same time in the prior art is effectively solved, and the electrochemical performance of the battery is further improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of battery technology, and in particular to an electrostatic spinning diaphragm and preparation and application thereof. Background Art

[0002] As one of the key components of batteries, the performance of battery separators directly affects the safety and life of batteries. Traditional separators are mainly made of materials such as polyethylene (PE) and polypropylene (PP) through dry or wet methods. However, these traditional separators have some limitations, such as low porosity, which is especially insufficient in the application of high energy density and high power batteries.

[0003] Electrospinning technology has attracted widespread attention in the field of battery separators in recent years because of its ability to prepare nanofiber membranes. Electrospinning uses high voltage to spray polymer solutions or melts into ultrafine fibers to form nanofiber membranes with a three-dimensional network structure. Compared with traditional separators, electrospinning separators have significant advantages. First, electrospinning separators have higher porosity and more uniform pore size distribution, which helps to improve the ionic conductivity and overall performance of the battery. Secondly, electrospinning separators exhibit better thermal stability, can maintain structural integrity in high temperature environments, and reduce the risk of battery short circuits. In addition, the electrospinning process can flexibly control the fiber diameter and membrane thickness, thereby optimizing the performance of the separator to meet the needs of different applications. However, since electrospun separators are irregularly stacked nanofibers, they generally have low tensile strength.

[0004] Therefore, there is a need to provide a solution for electrospinning membranes that can simultaneously improve porosity and tensile strength. Summary of the invention

[0005] In view of this, the present application provides an electrospinning membrane and its preparation and application, which are used to solve the problem of how to simultaneously improve the porosity and tensile strength of the electrospinning membrane.

[0006] In order to achieve the above technical objectives, this application adopts the following technical solutions:

[0007] In a first aspect, a method for preparing an electrospinning membrane comprises the following steps:

[0008] S1. dispersing polyvinylidene fluoride and polyvinyl alcohol in a solvent to obtain a mixed solution, and electrospinning the mixed solution to obtain a composite nanofiber membrane;

[0009] S2. The composite nanofiber membrane is heat treated and polyvinylidene fluoride is melted to obtain a heat-treated fiber membrane;

[0010] S3. Under heating conditions, the heat-treated fiber membrane is placed in deionized water for ultrasonic washing to obtain an electrospinning membrane.

[0011] Preferably, in step S1, the solvent includes at least DMF.

[0012] Preferably, in step S1, the process conditions for electrospinning are: solution concentration 12-14%, spray voltage 18-20 KV, receiving distance 100-120 mm, solution propulsion speed 0.025-0.03 ml / min, and needle diameter 0.86-0.95 mm.

[0013] Preferably, in step S1, the mass ratio of polyvinylidene fluoride to polyvinyl alcohol is 2:1-1.5.

[0014] Preferably, in step S2, the heating temperature of the heat treatment is 170-210° C., and the heat treatment time is 10-20 min.

[0015] Preferably, in step S3, the heating temperature is 95-100°C.

[0016] Preferably, the standing time in step S3 is 30-40 min.

[0017] In a second aspect, the present application provides an electrospinning membrane.

[0018] In a third aspect, the present application provides an application of an electrospinning membrane in a battery membrane.

[0019] In a fourth aspect, the present application provides a battery comprising an electrospun membrane.

[0020] The beneficial effects of the present application are as follows: The present application dissolves polyvinylidene fluoride (PVDF) and polyvinyl alcohol (PVA) in DMF to form a mixed solution, and uses electrospinning technology to manufacture a composite nanofiber diaphragm, and then performs post-treatment according to the melting point and water solubility of each component. While ensuring that the diaphragm has a high porosity, its tensile strength is greatly improved, effectively solving the problem of the porosity and tensile strength that cannot be taken into account in the prior art, and further improving the electrochemical performance of the battery. DETAILED DESCRIPTION

[0021] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0022] In related technologies, electrospinning membranes generally face a key problem, that is, it is often difficult to maintain sufficient tensile strength while achieving high porosity. Traditional electrospinning membranes usually have a contradiction between porosity and tensile strength due to the irregular stacking of nanofibers: membranes with high porosity usually have low tensile strength, while membranes with high tensile strength have a porosity that is difficult to meet the requirements. This characteristic limits its application in high-performance batteries.

[0023] At present, although some methods have been tried to improve this contradiction by adjusting the fiber diameter and increasing fiber cross-linking, the effect is often limited and it is difficult to find the best balance between the two. In addition, the existing post-processing process is complex and costly, making it difficult to achieve large-scale production and application.

[0024] Based on this, this application was created.

[0025] In a first aspect, the present application provides a method for preparing an electrospinning membrane, comprising the following steps:

[0026] S1. dispersing polyvinylidene fluoride and polyvinyl alcohol in a solvent to obtain a mixed solution, and electrospinning the mixed solution to obtain a composite nanofiber membrane;

[0027] S2. The composite nanofiber membrane is heat treated and polyvinylidene fluoride is melted to obtain a heat-treated fiber membrane;

[0028] S3. Under heating conditions, the heat-treated fiber membrane is placed in 95°C deionized water for ultrasonic washing to obtain an electrospinning membrane.

[0029] The present application dissolves PVDF / PVA in DMF to form a mixed solution, and uses electrospinning technology to manufacture a composite nanofiber diaphragm, and then performs post-treatment according to the melting point and water solubility of each component, thereby greatly improving the tensile strength of the diaphragm while ensuring that the diaphragm has a high porosity. This method effectively solves the problem of the inability to balance porosity and tensile strength in the prior art.

[0030] After obtaining the composite nanofiber diaphragm, heat treatment and water washing steps are involved. The principle of the heat treatment step is that the melting point of PVDF (170°C) is much lower than that of PVA (235°C), and the composite nanofiber diaphragm is treated in a 175°C incubator for 15 minutes. At this time, PVDF melts and forms a cross-linked structure at the intersection of the fibers, thereby improving the tensile strength of the diaphragm; the principle of the water washing step is that, based on the characteristics that PVDF is insoluble in water and PVA is soluble at 95°C, the heat-treated composite nanofiber diaphragm is placed in deionized water at 95°C for 30 minutes, so that PVA is dissolved and partially removed from the fiber structure, thereby forming a large number of holes on the fiber surface and inside, and improving the porosity of the diaphragm. Through the above process, the cross-linked structure formed by PVDF at the intersection of the fibers significantly enhances the mechanical strength of the diaphragm, making it more stable under tensile stress; and the holes formed after the dissolution of PVA significantly increase the porosity of the diaphragm, so that it can accommodate more electrolytes and improve the ionic conductivity and overall performance of the battery. The constituent material of the diaphragm obtained in the present application is PVDF and has a cross-linked structure at the connection, and there are cavities on the fibers.

[0031] In some embodiments, in step S1, the solvent includes at least DMF.

[0032] In this embodiment, DMF can make PVDF and PVA dispersed evenly.

[0033] In some embodiments, in step S1, the process conditions of electrospinning are: solution concentration 12-14%, spray voltage 18-20KV, receiving distance 100-120mm, solution propulsion speed 0.025-0.03ml / min, and needle diameter 0.86-0.95mm.

[0034] In some embodiments, in step S1, the mass ratio of polyvinylidene fluoride to polyvinyl alcohol is 2:1-1.5.

[0035] In this embodiment, the usage ratio of PVDF and PVA is limited to further balance the porosity and tensile strength of the diaphragm. If the PVDF content is too much, the tensile strength of the diaphragm will be significantly improved, but the porosity will be reduced, resulting in a decrease in the electrolyte absorption capacity and ion conductivity, affecting the overall performance of the battery. In addition, too much PVDF may make the diaphragm too rigid, reducing its adaptability during the battery assembly process.

[0036] On the contrary, too little PVDF content will lead to insufficient tensile strength of the diaphragm, increasing the risk of breakage. Although the porosity increases, which is beneficial for electrolyte absorption and ion conduction, it may make the diaphragm structure unstable. Therefore, the PVDF content needs to be controlled within a reasonable range to ensure that the diaphragm has both high tensile strength and high porosity to achieve optimal battery performance.

[0037] If there is too much PVA, it will be dissolved and removed during the water washing step, resulting in excessive pores in the composite nanofiber separator. Although this will significantly increase the porosity of the separator, too many pores may weaken the structural integrity and mechanical strength of the separator, reducing its stability in battery applications.

[0038] If there is too little PVA, the amount of PVA dissolved and removed in the water washing step is reduced, resulting in fewer pores. Although this can maintain the mechanical strength of the separator, the porosity is insufficient and cannot provide enough space to accommodate the electrolyte, which may reduce the ionic conductivity and overall performance of the battery.

[0039] In some embodiments, in step S2, the heating temperature of the heat treatment is 170-210° C., and the heat treatment time is 10-20 min.

[0040] In this embodiment, the heating temperature of the heat treatment is higher than the melting point of PVDF but lower than the melting point of PVA, which is beneficial to the melting of PVDF and the formation of a cross-linked structure at the intersection of fibers to enhance the tensile strength of the separator.

[0041] In some embodiments, in step S3, the heating temperature is 95-100°C.

[0042] In this embodiment, the porosity of the separator is increased by dissolving PVA, taking advantage of the fact that PAN and PVDF are insoluble in water, while PVA is soluble in water at 95°C.

[0043] In some embodiments, the standing time in step S3 is 30-40 min.

[0044] In a second aspect, the present application provides an electrospinning membrane.

[0045] In a third aspect, the present application provides an application of an electrospinning membrane in a battery membrane.

[0046] In a fourth aspect, the present application provides a battery comprising an electrospun membrane.

[0047] The present solution is further described below through specific embodiments.

[0048] Example 1

[0049] A method for preparing an electrospinning membrane comprises the following steps:

[0050] S1. Disperse polyvinylidene fluoride and polyvinyl alcohol in DMF in a mass ratio of 2:1 to obtain a mixed solution, and electrospin the mixed solution with a solution concentration of 12%, a spray voltage of 18KV, a receiving distance of 100mm, a solution propulsion speed of 0.025ml / min, and a needle diameter of 0.86mm to obtain a composite nanofiber membrane;

[0051] S2. The composite nanofiber membrane was placed in a 175°C incubator for 15 min to melt the PVDF and obtain a heat-treated fiber membrane;

[0052] S3. The heat-treated fiber membrane was placed in deionized water at 95° C. for washing for 30 min to dissolve and remove the PVA, thereby obtaining an electrospinning membrane.

[0053] Example 2

[0054] A method for preparing an electrospinning membrane comprises the following steps:

[0055] S1. Disperse polyvinylidene fluoride and polyvinyl alcohol in DMF at a mass ratio of 4:3 to obtain a mixed solution, and electrospin the mixed solution with a solution concentration of 12%, a spray voltage of 18KV, a receiving distance of 100mm, a solution propagation speed of 0.025ml / min, and a needle diameter of 0.86mm to obtain a composite nanofiber membrane;

[0056] S2. The composite nanofiber membrane was placed in a 200°C incubator for 15 min to melt the PVDF and obtain a heat-treated fiber membrane;

[0057] S3. The heat-treated fiber membrane was placed in deionized water at 95° C. for washing for 30 min to dissolve and remove the PVA, thereby obtaining an electrospinning membrane.

[0058] Example 3

[0059] A method for preparing an electrospinning membrane comprises the following steps:

[0060] S1. Disperse polyvinylidene fluoride and polyvinyl alcohol in DMF at a mass ratio of 4:1 to obtain a mixed solution, and electrospin the mixed solution with a solution concentration of 12%, a spray voltage of 18KV, a receiving distance of 100mm, a solution propagation speed of 0.025ml / min, and a needle diameter of 0.86mm to obtain a composite nanofiber membrane;

[0061] S2. The composite nanofiber membrane was placed in a 175°C incubator for 15 min to melt the PVDF and obtain a heat-treated fiber membrane;

[0062] S3. The heat-treated fiber membrane is placed in deionized water at 100° C. for washing for 30 minutes to dissolve and remove the PVA, thereby obtaining an electrospinning membrane.

[0063] Comparative Example 1

[0064] A method for preparing an electrospinning membrane, the other contents of which are the same as those of Example 1, except that step S2 is not included.

[0065] Comparative Example 2

[0066] A method for preparing an electrospinning membrane, the other contents of which are the same as those of Example 1, except that step S3 is not included.

[0067] Comparative Example 3

[0068] A method for preparing an electrospinning membrane, the other contents of which are the same as those of Example 1, except that steps S2 and S3 are not included.

[0069] Test and Evaluation

[0070] The porosity and tensile strength of the electrospun membranes obtained in each embodiment and comparative example were tested, and the testing method was as follows:

[0071] Porosity test method: The porosity of the membrane was measured by the n-butanol method. The dried membrane was cut into a circular shape with a diameter of 2.0 cm. The circular membrane with a dry weight Md was immersed in n-butanol for 2 h, and then the n-butanol on the surface was removed with filter paper to obtain the wet weight Mw. The porosity (P%) of the membrane was calculated using the following formula: Where ρ is the density of n-butanol and V is the volume of the dry membrane.

[0072]

[0073] Tensile strength test method: Use a thickness gauge to measure the thickness of the diaphragm and record it as A. Put the diaphragm on the cutting machine and cut it into strips with a width of 10mm. Then, draw a mark at a spacing of 10cm on the diaphragm cut into strips, and then clamp the diaphragm on the universal tester, enter the relevant parameters, and start measuring. When the diaphragm is broken, the tensile strength will be displayed, and the tensile strength can be read. The results are shown in Table 1.

[0074] Table 1 Test results

[0075] Porosity (%) Tensile strength(MPa) Example 1 67.3 18.1 Example 2 58.6 19.2 Example 3 64.5 17.6 Comparative Example 1 71.6 6.3 Comparative Example 2 56.2 19.4 Comparative Example 3 64.1 7.2

[0076] Comparing Example 1, Example 2, and Example 3, it is obvious that as the mass of PVDF increases, the tensile strength increases, but the porosity decreases. However, as the mass of PVA increases, the porosity increases, but the tensile strength decreases. Comparing Example 1, Comparative Example 1, Comparative Example 2, and Comparative Example 3, it can be found that the cross-linked structure formed at the intersection of fibers after the heat-melted PVDF significantly enhances the mechanical strength of the diaphragm, making it more stable under tensile stress; and the holes formed after the PVA is dissolved significantly increase the porosity of the diaphragm. Example 1 maintains a relatively high porosity while ensuring that the diaphragm has a sufficiently high tensile strength.

[0077] The above are only preferred specific implementations of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily conceived by any technician familiar with the technical field within the technical scope disclosed by the present invention should be covered within the protection scope of the present invention.

Claims

1. A method for preparing an electrospinning membrane, It is characterized in that The following steps are involved: S1. dispersing polyvinylidene fluoride and polyvinyl alcohol in a solvent to obtain a mixed solution, and electrospinning the mixed solution to obtain a composite nanofiber membrane; S2. The composite nanofiber membrane is heat treated and polyvinylidene fluoride is melted to obtain a heat-treated fiber membrane; S3. Under heating conditions, the heat-treated fiber membrane is placed in deionized water for ultrasonic washing to obtain the electrospinning membrane.

2. The method for preparing the electrospinning membrane according to claim 1, It is characterized in that In step S1, the solvent includes at least DMF.

3. The method for preparing the electrospinning membrane according to claim 1, It is characterized in that In step S1, the process conditions of electrospinning are: solution concentration 12-14%, spray voltage 18-20KV, receiving distance 100-120mm, solution propulsion speed 0.025-0.03ml / min, and needle diameter 0.86-0.95mm.

4. The method for preparing the electrospinning membrane according to claim 1, It is characterized in that In step S1, the mass ratio of polyvinylidene fluoride to polyvinyl alcohol is 2:1-1.

5.

5. The method for preparing the electrospinning membrane according to claim 1, It is characterized in that In step S2, the heating temperature of the heat treatment is 170-210°C, and the heat treatment time is 10-20 minutes.

6. The method for preparing the electrospinning membrane according to claim 1, It is characterized in that In step S3, the heating temperature is 95-100°C.

7. The method for preparing the electrospinning membrane according to claim 1, It is characterized in that The standing time in step S3 is 30-40 min.

8. An electrospinning membrane obtained by the preparation method according to any one of claims 1 to 7.

9. Use of the electrospun membrane according to claim 8 in battery membranes.

10. A battery comprising the electrospun membrane according to claim 8.

Citation Information

Patent Citations

  • Preparation method of P(VDF-HFP) (Poly(Vinyl Fluoride-Hexafluoropropylene)) inorganic compound porous nano fiber lithium ion battery separator

    CN103258978A

  • Preparation method of reinforced electrostatic spinning nano-fiber lithium-ion battery separator

    CN103469488A

  • Method for enhancing electrostatic spinning nanofiber membrane

    CN103541149A

  • A preparation method of a lithium ion battery separator

    CN109244331A

  • Preparation method for porous membrane of composite nanofiber

    CN110284264A

Cited By

  • Microporous dielectric diaphragm as well as preparation method and application thereof

    CN121394188A

  • Microporous dielectric separator and method of making and using same

    CN121394188B