Ultra-thin FPC (Flexible Printed Circuit) board and preparation process thereof

By coarsing, cleaning and modification of PI adjuster and multi-layer black hole liquid treatment on the FPC board, the thickness of the pore wall carbon layer is increased, and the problem of clamp hole breakage during the electroplating of traditional ultra-thin FPC board is solved, and the problem of clamp hole breakage during the electroplating of traditional ultra-thin FPC board is improved. Conductivity and yield.

CN118946037APending Publication Date: 2024-11-12SHENZHEN BEIJIA ELECTRONICS MATERIAL
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411201701.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Traditional ultra-thin FPC boards are prone to hole breaking near the grip during electroplating, resulting in poor conductivity.

Method used

By performing PI adjuster roughening treatment, cleaning and modification treatment, first and second black hole fluid treatments on the flexible substrate, the carbon layer thickness on the surface of the hole wall is increased to ensure that the hole wall near the grip points are thickened to form a thickening Carbon layer to avoid breakdown of current.

Benefits of technology

It effectively avoids hole breaking near the clamp point and improves the conductivity and yield of ultra-thin FPC boards.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118946037A_ABST
    Figure CN118946037A_ABST
Patent Text Reader

Abstract

The invention provides an ultra-thin FPC (Flexible Printed Circuit) board and a preparation process thereof. The preparation process of the ultra-thin FPC board comprises the following steps: obtaining a flexible substrate, wherein a plurality of through holes are formed in the flexible substrate; carrying out roughening treatment on the flexible substrate by adopting a PI (Polyimide) regulator; carrying out cleaning modification treatment on the flexible substrate subjected to the roughening treatment; performing first black hole treatment on the flexible substrate subjected to cleaning modification treatment by adopting first black hole liquid; carrying out hole finishing treatment on the flexible substrate after the first black hole treatment; performing second hole blackening treatment on the flexible substrate subjected to hole finishing treatment by adopting second hole blackening liquid; and carrying out electroplating treatment on the flexible substrate after the second black hole treatment to obtain the ultra-thin FPC board.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of circuit boards, and in particular to an ultra-thin FPC board and a preparation process thereof. Background Art

[0002] FPC board, the full name is Flexible Printed Circuit, also known as flexible circuit board or flexible circuit board. This kind of circuit board is made of polyimide or polyester film as the base material, with high reliability, excellent flexibility and excellent electrical performance.

[0003] With the continuous development of the electronics industry, FPC boards face broad development prospects due to their unique performance and wide range of applications. The global FPC market continues to grow, especially in the fields of consumer electronics, automotive electronics, medical equipment, industrial control, and aerospace. At the same time, with the rise of new energy vehicles and the popularization of new technologies such as 5G, the market demand for FPC boards will further increase.

[0004] However, in order to save space in small electronic devices, the thickness of the FPC board is made ultra-thin (36μm thick). The preparation process of the traditional ultra-thin FPC board is generally to directly process the substrate after the hole is opened with a black hole line, that is, immerse it in a black hole tank for activation and carbon hanging, but the hole wall of the FPC board is relatively smooth, and the carbon hanging effect is limited, that is, the thickness of the carbon layer is relatively thin, resulting in the problem of hole breakage near the clamping point of the FPC board during VCP line production. Specifically, the FPC board is clamped by a fixture and immersed in a copper plating tank during electroplating, and then the fixture is energized to plate the holes of the FPC board with a copper layer, but the current near the clamping point is the starting point, that is, the entry point of the current, and the current is instantaneously passed, that is, the amount of current passing through the holes near the clamping point is large, and because the thickness of the carbon hanging is thin, the current will directly break through the carbon layer, resulting in a hole breakage phenomenon near the clamping point, that is, the holes near the clamping point are partially not hung with copper, thereby affecting the conductive performance of the FPC board. Summary of the invention

[0005] The purpose of the present invention is to overcome the deficiencies in the prior art and provide an ultra-thin FPC board and a preparation process thereof that can avoid hole breakage near the pinch point.

[0006] The purpose of this disclosure is achieved through the following technical solutions:

[0007] A preparation process of an ultra-thin FPC board comprises the following steps:

[0008] Obtaining a flexible substrate, wherein a plurality of through holes are formed on the flexible substrate;

[0009] The flexible substrate is roughened by using a PI adjusting agent;

[0010] Performing a cleaning and modification treatment on the flexible substrate after the roughening treatment;

[0011] Using a first black hole liquid to perform a first black hole treatment on the flexible substrate after the cleaning and modification treatment;

[0012] Performing a whole hole treatment on the flexible substrate after the first black hole treatment;

[0013] Performing a second black hole treatment on the flexible substrate after the whole hole treatment using a second black hole liquid;

[0014] Performing electroplating treatment on the flexible substrate after the second black hole treatment to obtain an ultra-thin FPC board;

[0015] The PI adjuster includes a first PI adjuster and a second PI adjuster, the concentration of the first PI adjuster is 5% to 10%, the concentration of the second PI adjuster is 10% to 20%, and the roughening treatment time is 30s to 90s;

[0016] The mass proportion of carbon black in the first black pore liquid is 2.5%, and the mass proportion of carbon black in the second black pore liquid is 7.5%.

[0017] In one embodiment, after the step of roughening the flexible substrate with a PI adjuster and before the step of cleaning and modifying the roughened flexible substrate, the preparation process further comprises the following steps:

[0018] A first micro-etching process is performed on the flexible substrate.

[0019] In one embodiment, after the second black hole treatment is performed on the flexible substrate after the whole hole treatment using the second black hole liquid, and before the step of electroplating the flexible substrate after the second black hole treatment, the preparation process further includes the following steps:

[0020] A second micro-etching process is performed on the flexible substrate.

[0021] In one embodiment, the specific operation steps of electroplating the flexible substrate after the second black hole treatment are:

[0022] Degreasing the flexible substrate;

[0023] Performing a third micro-etching process on the flexible substrate after the degreasing process;

[0024] Performing pickling treatment on the flexible substrate after the third micro-etching treatment;

[0025] The flexible substrate after pickling is immersed in a copper plating tank through a fixture for electroplating.

[0026] In one embodiment, after the step of electroplating the flexible substrate after the second black hole treatment, the preparation process further includes the following steps:

[0027] The flexible substrate is subjected to circuit fabrication processing to obtain the ultra-thin FPC board.

[0028] In one embodiment, the specific operation steps of obtaining the flexible substrate are:

[0029] The flexible material is cut to obtain a PI board layer;

[0030] The first copper foil layer, the PI board layer and the second copper foil layer are sequentially stacked and pressed to obtain a flexible substrate;

[0031] Drying the flexible substrate;

[0032] The flexible substrate after the drying process is subjected to drilling process, so that a plurality of through holes are formed on the flexible substrate.

[0033] In one embodiment, the current density of the electroplating is 32ASF to 42ASF;

[0034] The electroplating current is 250A-540A.

[0035] In one embodiment, the first black hole liquid further includes potassium carbonate and polyethylene glycol, the mass proportion of the potassium carbonate is 1%, and the mass proportion of the polyethylene glycol is 7%.

[0036] In one embodiment, the second black hole liquid further includes potassium carbonate and polyethylene glycol, the mass proportion of the potassium carbonate is 1%, and the mass proportion of the polyethylene glycol is 7%.

[0037] An ultra-thin FPC board is prepared by using the preparation process of the ultra-thin FPC board described in any of the above embodiments.

[0038] Compared with the prior art, the present invention has at least the following advantages:

[0039] 1. The flexible substrate is subjected to a roughening treatment under the conditions that the concentration of the first PI adjuster is 5% to 10%, the concentration of the second PI adjuster is 10% to 20%, and the roughening treatment time is 30s to 90s, which can effectively increase the roughness of the hole wall surfaces of several through holes of the flexible substrate. Then, by cleaning and modifying the flexible substrate, the grease on the board surface can be removed and the negative charge attached to the hole wall on the flexible substrate can be adjusted to a positive charge. In this way, when the first black hole liquid is used to perform the first black hole treatment on the flexible substrate, the carbon black carrying the negative charge in the first black hole liquid can be electrostatically adsorbed on the surface of the hole wall and form a carbon layer.

[0040] 2. By performing whole-hole treatment on the flexible substrate, the charge of the area without carbon hanging or the area with poor carbon hanging effect in the hole wall is adjusted to ensure that the charge of the area without carbon hanging or the area with poor carbon hanging effect in the hole wall is positive. In this way, when the second black hole liquid is used to perform the second black hole treatment on the flexible substrate, the carbon black carrying negative charge in the second black hole liquid can be electrostatically adsorbed on the surface of the hole wall. Because the mass proportion of carbon black in the first black hole liquid is 2.5%, and the mass proportion of carbon black in the second black hole liquid is 7.5%, the carbon layer on the surface of the hole wall can be thickened by increasing the mass proportion of carbon black in the second black hole liquid, and at the same time, a thickened carbon layer is formed in the area without carbon hanging on the hole wall, thereby ensuring that a thickened carbon layer can be formed in each area of ​​the hole wall, and when the flexible substrate is electroplated, the through hole near the pinch point will not be broken, ensuring that the ultra-thin FPC board has good conductivity. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] In order to more clearly illustrate the technical solutions of the embodiments of the present disclosure, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present disclosure and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without paying creative work.

[0042] Figure 1 The present invention is a flow chart of the preparation process of the ultra-thin FPC board;

[0043] Figure 2 for Figure 1 The flowchart of S700 in the manufacturing process of the ultra-thin FPC board shown;

[0044] Figure 3 Schematic diagram of a cross section of the ultra-thin FPC board of Example 1;

[0045] Figure 4 This is a schematic cross-sectional view of the ultra-thin FPC board of comparative example 1. DETAILED DESCRIPTION

[0046] In order to facilitate the understanding of the present disclosure, the present disclosure will be described more fully below with reference to the relevant drawings. The preferred embodiments of the present disclosure are given in the drawings. However, the present disclosure can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the disclosure of the present disclosure more thoroughly and comprehensively understood.

[0047] It should be noted that when an element is referred to as being "fixed to" another element, it may be directly on the other element or there may be a central element. When an element is considered to be "connected to" another element, it may be directly connected to the other element or there may be a central element at the same time. The terms "vertical", "horizontal", "left", "right" and similar expressions used herein are for illustrative purposes only and do not represent the only implementation method.

[0048] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present disclosure. The terms used herein in the specification of the present disclosure are only for the purpose of describing specific embodiments and are not intended to limit the present disclosure. The term "and / or" used herein includes any and all combinations of one or more related listed items.

[0049] The present disclosure provides a preparation process of an ultra-thin FPC board, comprising the following steps: obtaining a flexible substrate, on which a plurality of through holes are formed; roughening the flexible substrate using a PI adjuster; cleaning and modifying the flexible substrate after the roughening treatment; performing a first black hole treatment on the flexible substrate after the cleaning and modification treatment using a first black hole liquid; performing a hole-filling treatment on the flexible substrate after the first black hole treatment; performing a second black hole treatment on the flexible substrate after the hole-filling treatment using a second black hole liquid; and electroplating the flexible substrate after the second black hole treatment to obtain an ultra-thin FPC board; wherein the PI adjuster comprises a first PI adjuster and a second PI adjuster, the concentration of the first PI adjuster is 5% to 10%, the concentration of the second PI adjuster is 10% to 20%, and the time of the roughening treatment is 30s to 90s; the mass proportion of carbon black in the first black hole liquid is 2.5%, and the mass proportion of carbon black in the second black hole liquid is 7.5%.

[0050] The above-mentioned preparation process of the ultra-thin FPC board, under the conditions that the concentration of the first PI adjuster is 5% to 10%, the concentration of the second PI adjuster is 10% to 20%, and the roughening treatment time is 30s to 90s, the flexible substrate is roughened, which can effectively increase the roughness of the hole wall surface of several through holes of the flexible substrate. Then, by cleaning and modifying the flexible substrate, the grease on the board surface can be removed and the negative charge attached to the hole wall on the flexible substrate can be adjusted to a positive charge. In this way, when the first black hole liquid is used to perform the first black hole treatment on the flexible substrate, the carbon black carrying the negative charge in the first black hole liquid can be electrostatically adsorbed on the surface of the hole wall and form a carbon layer.

[0051] Furthermore, by performing whole-hole treatment on the flexible substrate, the charge of the non-carbonized area or the area with poor carbon-hanging effect in the hole wall is adjusted to ensure that the charge carried by the non-carbonized area or the area with poor carbon-hanging effect in the hole wall is positive. In this way, when the second black hole liquid is used to perform the second black hole treatment on the flexible substrate, the carbon black carrying negative charge in the second black hole liquid can be electrostatically adsorbed on the surface of the hole wall. Because the mass proportion of carbon black in the first black hole liquid is 2.5% and the mass proportion of carbon black in the second black hole liquid is 7.5%, the carbon layer on the surface of the hole wall can be thickened by increasing the mass proportion of carbon black in the second black hole liquid, and at the same time, a thickened carbon layer can be formed in the non-carbonized area of ​​the hole wall, thereby ensuring that a thickened carbon layer can be formed in each area of ​​the hole wall, and when the flexible substrate is electroplated, the through hole near the pinch point will not be broken, ensuring that the ultra-thin FPC board has good conductivity.

[0052] See also Figure 1 In order to better understand the preparation process of the ultra-thin FPC board disclosed in the present invention, the preparation process of the ultra-thin FPC board is further explained as follows:

[0053] A process for preparing an ultra-thin FPC board according to an embodiment of the present invention comprises the following steps:

[0054] S100, obtaining a flexible substrate, wherein a plurality of through holes are formed on the flexible substrate.

[0055] In this embodiment, a number of through holes have been formed on the flexible substrate after the previous process, and the through holes are conductive holes. The function of the conductive holes is to achieve circuit conduction on the FPC board, that is, the circuit conduction of the upper and lower layers of copper foil, ensuring that the FPC board has good conductive properties.

[0056] It should be noted that the flexible substrate includes a first copper foil layer, a PI board layer and a second copper foil layer stacked in sequence, wherein the thickness of the first copper foil layer, the PI board layer and the second copper foil layer are all 12 μm.

[0057] S200, roughening the flexible substrate using a PI adjuster.

[0058] In this embodiment, the PI adjusting agent is used to corrode the hole wall surface in the flexible substrate, making the hole wall surface rough, increasing the carbon hanging area of ​​the hole wall, thereby ensuring a better carbon hanging effect. Specifically, the flexible substrate is immersed in the PI adjusting cylinder, that is, the roughening treatment time is the immersion time of the flexible substrate in the PI adjusting cylinder.

[0059] Furthermore, since the PI adjuster can corrode the PI board layer in the flexible substrate, if the concentration is too high or the roughening time is too long, pits will appear in the hole wall of the FPC board. On the one hand, it will cause the copper thickness of the hole wall after subsequent copper plating to be inconsistent, that is, the copper thickness of the pit is thinner, which reduces the conductivity of the FPC board. On the other hand, it will cause the first copper foil layer and the second copper foil layer to be concave. In severe cases, the first copper foil layer and the second copper foil layer will directly contact, resulting in a short circuit, reducing the qualified rate of the FPC board. Therefore, in one embodiment, the PI adjuster includes a first PI adjuster and a second PI adjuster, the concentration of the first PI adjuster is 5% to 10%, the concentration of the second PI adjuster is 10% to 20%, and the roughening treatment time is 30s to 90s. Among them, the concentration of the first PI adjuster refers to the concentration of the first PI adjuster in the solution of the PI adjusting cylinder, and the concentration of the second PI adjuster refers to the concentration of the second PI adjuster in the solution of the PI adjusting cylinder. Under this roughening condition, the surface roughness of the hole wall of the FPC board can be increased, and at the same time, pits in the hole wall can be avoided, thereby obtaining a better roughening effect, thereby further improving the carbon hanging effect of the hole wall, improving the copper plating effect of the ultra-thin FPC board, avoiding the hole breaking near the pinch point during electroplating, ensuring that the ultra-thin FPC board has good conductivity, and thereby improving the yield rate of the ultra-thin FPC board.

[0060] Furthermore, the first PI adjuster includes potassium hydroxide and ethanolamine, wherein the mass proportion of the potassium hydroxide is 19%, and the mass proportion of the ethanolamine is 6%. It should be noted that the model of the first PI adjuster is PI adjuster M103A.

[0061] Furthermore, the second PI adjuster includes potassium hydroxide and ethanolamine, wherein the mass proportion of the potassium hydroxide is 20%, and the mass proportion of the ethanolamine is 5%. It should be noted that the model of the second PI adjuster is PI adjuster M103D.

[0062] It should be noted that by mixing the PI adjuster M103A and the PI adjuster M103D in a preset ratio and combining the control of the roughening time, the flexible substrate of the ultra-thin FPC board has a better roughening effect, thereby improving the carbon hanging effect of the hole wall of the flexible substrate, thereby ensuring that the hole wall of the flexible substrate can be plated with a copper layer during subsequent electroplating, avoiding the hole breakage near the pinch point, and thus ensuring that the ultra-thin FPC board has better conductivity.

[0063] Furthermore, the roughening treatment time is preferably 45 seconds. When the roughening treatment time is 45 seconds, the flexible substrate can have the best carbon hanging effect.

[0064] Furthermore, after the flexible substrate is roughened with the PI adjuster, the flexible substrate needs to be washed with three levels of water. Specifically, the roughened flexible substrate passes through three washing tanks in sequence, and the washing time is 20s to 40s. The washing method of each washing tank is spray washing, which can effectively remove the residual PI adjuster on the flexible substrate and ensure the cleanliness of the surface of the flexible substrate.

[0065] S300, performing a cleaning and modification treatment on the flexible substrate after the roughening treatment.

[0066] In this embodiment, the flexible substrate after roughening treatment is immersed in a cleaning tank for cleaning and modification treatment, and the immersion time is 30s to 90s, that is, the grease on the surface of the flexible substrate is removed by the detergent in the cleaning tank, and the negative charge in the pore wall is adjusted to a positive charge, so that electrostatic adsorption can be formed with the carbon black carrying the negative charge, thereby effectively improving the carbon hanging effect of the flexible substrate.

[0067] Furthermore, the concentration of the cleaning agent is 8% to 12%, that is, the concentration of the cleaning agent refers to the mass proportion of the cleaning agent in the solution of the cleaning tank, wherein the cleaning agent includes malic acid, polyethylene glycol and hydroxyethylethylenediamine, the mass proportion of malic acid is 5%, the mass proportion of polyethylene glycol is 10%, and the mass proportion of hydroxyethylethylenediamine is 15%. It should be noted that malic acid releases protons (H + ), while hydroxyethylethylenediamine can neutralize the negative charge in the flexible substrate by interacting with negatively charged molecules, such as ion pair formation or salt bridge. At the same time, polyethylene glycol, as a modifier, affects the charge state by changing the surface properties of the molecules in the pore wall. In combination with the protons released by malic acid, the pore wall of the flexible substrate can be changed from negatively charged to positively charged, thereby increasing the carbon hanging effect of the pore wall of the flexible substrate. It should be noted that the model of the cleaner is black pore cleaner M8501.

[0068] Furthermore, the cleaning and modification time is preferably 60 s.

[0069] Furthermore, when the flexible substrate after the roughening treatment is cleaned and modified, the flexible substrate needs to be washed with three levels of water. Specifically, the cleaned and modified flexible substrate passes through three washing tanks in sequence, and the washing time is 20s to 40s. The washing method of each washing tank is spray washing, which can effectively remove the residual detergent on the flexible substrate and ensure the cleanliness of the board surface of the flexible substrate.

[0070] S400, performing a first black hole treatment on the flexible substrate after the cleaning and modification treatment using a first black hole liquid.

[0071] In this embodiment, the pore walls of the cleaned and modified flexible substrate carry positive charges, and the first black pore treatment is performed on the flexible substrate by the first black pore liquid, so that a carbon layer is formed in the pore walls of the flexible substrate. Specifically, the flexible substrate is immersed in the first black pore tank, and the carbon black in the first black pore liquid in the first black pore tank carries a negative charge. The carbon black is attached to the pore walls and a carbon layer is formed by the principle of electrostatic adsorption. Since the mass proportion of carbon black in the first black pore liquid is 2.5%, the formed carbon layer is the root layer, which lays a solid foundation for forming a dense and thickened carbon layer.

[0072] Furthermore, the first black hole treatment time is 30s to 90s.

[0073] Furthermore, the time for the first black hole treatment is preferably 30 seconds.

[0074] Furthermore, after the flexible substrate after the cleaning and modification treatment is subjected to the first black hole treatment with the first black hole liquid, it is necessary to absorb the moisture of the flexible substrate through the water-absorbing cotton layer, that is, to absorb the moisture in the first black hole liquid hanging on the hole wall, so that a carbon layer is retained in the hole wall, and then the flexible substrate is subjected to a first strong wind drying treatment, and after the first strong wind drying treatment, the flexible substrate is subjected to a first hot air drying treatment, so that the moisture in the carbon layer can be removed and the carbon layer on the flexible substrate can be solidified to form a stable conductive carbon layer.

[0075] It should be noted that the pressure of the first strong air drying process is 4 kPa to 6 kPa, and the temperature of the first hot air drying process is 60° C. to 70° C.

[0076] S500, performing a hole-filling treatment on the flexible substrate after the first black hole treatment.

[0077] In this embodiment, since there are areas without carbon or with poor carbon hanging effect on the hole wall of the flexible substrate after the first black hole treatment, the charge in the hole wall of the flexible substrate is fine-tuned and modified by the hole-sizing agent, so that the charge carried in the hole wall of the flexible substrate is adjusted to positive charge, ensuring that the secondary carbon hanging has a good carbon hanging effect. Specifically, the flexible substrate is immersed in the hole-sizing cylinder for hole-sizing treatment, and the immersion time is 30s to 90s, that is, the negative charge in the hole wall of the flexible substrate is adjusted to positive charge by the hole-sizing agent in the hole-sizing cylinder, that is, the surface of the area with the carbon layer also carries positive charge, which is convenient for thickening the carbon layer while forming a denser conductive carbon layer, and can also remove grease on the board surface.

[0078] Furthermore, the concentration of the pore-forming agent is 6% to 8%, that is, the concentration of the pore-forming agent refers to the mass proportion of the pore-forming agent in the potion of the pore-forming tank, wherein the pore-forming agent includes malic acid, polyethylene glycol and hydroxyethylethylenediamine, the mass proportion of malic acid is 4%, the mass proportion of polyethylene glycol is 7%, and the mass proportion of hydroxyethylethylenediamine is 40%. It should be noted that malic acid releases protons (H + ), while hydroxyethylethylenediamine can neutralize the negative charge in the flexible substrate by interacting with negatively charged molecules, such as ion pair formation or salt bridge. At the same time, polyethylene glycol, as a modifier, affects the charge state by changing the surface properties of the molecules in the pore wall. In combination with the protons released by malic acid, the charge state of the non-carbonized area in the pore wall of the flexible substrate can be changed from negative charge to positive charge, and the charge state of the carbon layer surface can be changed from negative charge to positive charge, thereby further increasing the carbonization effect of the pore wall of the flexible substrate. It should be noted that the model of the pore-forming agent is black pore-forming agent M8502.

[0079] Furthermore, the time for the whole hole treatment is 30s to 90s.

[0080] Furthermore, the time for the whole-hole treatment is preferably 55 s.

[0081] Furthermore, after the first black hole treatment is performed on the flexible substrate for hole filling treatment, the flexible substrate needs to be subjected to three-stage water washing. Specifically, the flexible substrate after the hole filling treatment is passed through three water washing tanks in sequence, and the washing time is 20s to 40s. The washing method of each water washing tank is spray water washing, which can effectively remove the hole filling agent remaining on the flexible substrate and ensure the cleanliness of the board surface of the flexible substrate.

[0082] S600, performing a second black hole treatment on the flexible substrate after the whole hole treatment using a second black hole liquid.

[0083] In this embodiment, the pore wall and carbon layer of the flexible substrate that has been subjected to the whole-pore treatment carry positive charges. The second black hole treatment is performed on the flexible substrate through the second black hole liquid, so that a thickened carbon layer is formed in the non-carbon-attached area in the pore wall of the flexible substrate, and the carbon layer that has been carbon-attached can also be thickened, so that a thickened carbon layer is formed in the pore wall. Specifically, the flexible substrate is immersed in the second black hole cylinder, and the carbon black in the second black hole liquid in the second black hole cylinder carries a negative charge. The carbon black is attached to the pore wall through the principle of electrostatic adsorption. Since the mass proportion of carbon black in the second black hole liquid is 7.5%, the thickness of the carbon layer is increased by increasing the solid content in the second black hole liquid, so that a thickened carbon layer can be formed in the pore wall, so that the flexible substrate will not have a hole break phenomenon near the pinch point during copper electroplating, so that the flexible substrate has a better copper plating effect, ensuring that the ultra-thin FPC board has better conductivity.

[0084] Furthermore, the second black hole treatment time is 30s to 90s.

[0085] Furthermore, the time for the second black hole treatment is preferably 60 seconds.

[0086] Furthermore, after the flexible substrate after the whole hole treatment is subjected to the second black hole treatment with the second black hole liquid, it is necessary to dry the moisture of the flexible substrate through the water-absorbing cotton layer, that is, to dry the moisture in the second black hole liquid hanging on the hole wall, so that a thickened carbon layer is retained in the hole wall, and then the flexible substrate is subjected to a second strong wind drying treatment, and after the second strong wind drying treatment, the flexible substrate is subjected to a second hot air drying treatment, so that the moisture in the thickened carbon layer can be removed and the thickened carbon layer on the flexible substrate can be solidified to form a stable and dense conductive carbon layer.

[0087] It should be noted that the pressure of the second strong air drying process is 4 kPa to 6 kPa, and the temperature of the second hot air drying process is 60° C. to 70° C.

[0088] S700, performing electroplating treatment on the flexible substrate after the second black hole treatment to obtain an ultra-thin FPC board.

[0089] In this embodiment, a stable and dense thickened carbon layer is formed in the hole wall of the flexible substrate after the second black hole treatment, and no hole breakage near the pinch point will occur during the electroplating treatment, ensuring that each hole has a good copper plating effect, thereby ensuring that the ultra-thin FPC board has good conductivity, thereby effectively improving the yield rate of the ultra-thin FPC board.

[0090] In one embodiment, after the step of roughening the flexible substrate with a PI adjuster and before the step of cleaning and modifying the roughened flexible substrate, the preparation process further comprises the following steps:

[0091] A first micro-etching process is performed on the flexible substrate.

[0092] It should be noted that the two sides of the flexible substrate are copper foil layers, and the surface of the copper foil layer will be oxidized to form copper oxide. By performing the first micro-etching treatment on the flexible substrate, the copper oxide on the surface of the copper foil layer can be removed, and the burrs at the opening of the through hole can be removed, thereby ensuring the consistency of the opening. Specifically, the flexible substrate is immersed in the first micro-etching tank for the first micro-etching treatment, and the immersion time is 30s to 90s, that is, the surface copper layer oxide of the flexible substrate is removed by the first micro-etching agent in the first micro-etching tank, and the burrs at the opening of the through hole are removed.

[0093] Furthermore, the time of the first micro-etching treatment is preferably 30 seconds.

[0094] Furthermore, the first micro-etching agent includes sulfuric acid and sodium persulfate, wherein the concentration of the sulfuric acid is 2% to 4%, and the concentration of the sodium persulfate is 50 g / L to 70 g / L.

[0095] Furthermore, the etching layer of the first micro-etching treatment is 0.5 μm to 1.0 μm. It should be noted that the oxide layer on the surface of the copper foil layer on both sides can be etched away in the first micro-etching treatment, that is, the etching layer on both sides is 0.5 μm to 1.0 μm, avoiding excessive etching and reducing the conductive effect of the copper foil layer, thereby ensuring that the ultra-thin FPC board has good conductive performance.

[0096] Furthermore, after the flexible substrate is subjected to the first micro-etching treatment, it is necessary to perform three-stage water washing on the flexible substrate. Specifically, the flexible substrate after the first micro-etching treatment is passed through three water washing tanks in sequence, and the water washing time is 20s to 40s. The water washing method of each water washing tank is spray water washing, which can effectively remove the first micro-etching agent remaining on the flexible substrate and ensure the cleanliness of the board surface of the flexible substrate.

[0097] In one embodiment, after the second black hole treatment is performed on the flexible substrate after the whole hole treatment using the second black hole liquid, and before the step of electroplating the flexible substrate after the second black hole treatment, the preparation process further includes the following steps:

[0098] A second micro-etching process is performed on the flexible substrate.

[0099] It should be noted that the surface of the flexible substrate after the second black hole treatment also has a carbon layer. By performing the second micro-etching treatment on the flexible substrate, that is, etching the copper surface of the copper foil layer, the carbon layer attached to the copper surface is removed to ensure the cleanliness of the surface of the copper foil layer. Specifically, the flexible substrate is immersed in the second micro-etching tank for the second micro-etching treatment, and the immersion time is 30s to 90s, that is, the carbon layer on the surface of the flexible substrate is removed by the second micro-etching agent in the second micro-etching tank.

[0100] Furthermore, the second micro-etching treatment time is preferably 30 seconds.

[0101] Furthermore, the second micro-etching agent includes sulfuric acid and sodium persulfate, wherein the concentration of the sulfuric acid is 2% to 4%, and the concentration of the sodium persulfate is 60 g / L to 100 g / L.

[0102] Furthermore, the etching layer of the second micro-etching treatment is 0.5μm to 1.0μm. It should be noted that the carbon layer on the surface of the copper foil layer on both sides can be etched away under the first micro-etching treatment. Although the second micro-etching agent cannot directly etch the carbon layer, by etching the copper surface of the copper foil layer, the carbon layer attached to the copper surface is removed. The etching layers on both sides are 0.5μm to 1.0μm, which avoids excessive etching and reduces the conductive effect of the copper foil layer, thereby ensuring that the ultra-thin FPC board has good conductive properties.

[0103] Furthermore, after the flexible substrate is subjected to the second micro-etching treatment, it is necessary to perform three-stage water washing on the flexible substrate. Specifically, the flexible substrate after the second micro-etching treatment is passed through three water washing tanks in sequence, and the water washing time is 20s to 40s. The water washing method of each water washing tank is spray water washing, which can effectively remove the second micro-etching agent remaining on the flexible substrate and ensure the cleanliness of the board surface of the flexible substrate.

[0104] Furthermore, after the second micro-etching treatment and the three-stage water washing, the flexible substrate needs to remove moisture on the flexible substrate through the water-absorbing cotton layer, and then the flexible substrate is subjected to the third strong wind drying treatment to dry the surface moisture on the flexible substrate. Finally, the flexible substrate is subjected to the third hot air drying treatment to remove the residual moisture in the hole wall of the flexible substrate, thereby ensuring that no moisture remains on the flexible substrate.

[0105] It should be noted that the pressure of the second strong air drying process is 4 kPa to 6 kPa, and the temperature of the second hot air drying process is 70° C. to 80° C.

[0106] See also Figure 2 In one embodiment, S700, the specific operation steps of electroplating the flexible substrate after the second black hole treatment are:

[0107] S710, performing degreasing treatment on the flexible substrate.

[0108] In this embodiment, since there is grease on the surface of the flexible substrate, the grease on the surface of the flexible substrate can be effectively removed by degreasing the flexible substrate, thereby ensuring the cleanliness of the surface of the flexible substrate. Specifically, the flexible substrate is immersed in a degreasing tank for degreasing, and the immersion time is 15s to 60s, that is, the surface grease of the flexible substrate is removed by the degreasing agent in the degreasing tank, thereby ensuring the cleanliness of the surface of the flexible substrate.

[0109] Further, the concentration of the degreasing agent is 2% to 4%, wherein the concentration of the degreasing agent refers to the mass proportion of the degreasing agent in the solution of the degreasing tank, and the solution of the degreasing tank also includes sulfuric acid, and the concentration of sulfuric acid is 2% to 4%. Further, the degreasing agent includes a surfactant and citric acid, the mass proportion of the surfactant is 12%, and the mass proportion of the citric acid is 12%. It should be noted that the model of the degreasing agent is acidic degreasing agent M401.

[0110] Furthermore, the time for the oil removal treatment is preferably 25 s.

[0111] Furthermore, after the flexible substrate is degreased, it is necessary to perform three-stage water washing on the flexible substrate. Specifically, the degreased flexible substrate is passed through three water washing tanks in sequence, and the washing time is 20s to 40s. The washing method of each water washing tank is spray water washing, which can effectively remove the residual degreaser on the flexible substrate and ensure the cleanliness of the board surface of the flexible substrate.

[0112] S720, performing a third micro-etching process on the flexible substrate after the degreasing process.

[0113] In this embodiment, since the copper layer on the surface of the flexible substrate is easily oxidized, that is, there is still a copper oxide layer on the surface of the flexible substrate, the copper oxide layer on the surface of the flexible substrate can be removed by performing the third micro-etching treatment on the flexible substrate, and the degreasing agent still remaining on the flexible substrate can be removed. Specifically, the flexible substrate is immersed in the third micro-etching tank for the third micro-etching treatment, and the immersion time is 15s to 60s, that is, the oxide of the copper layer on the surface of the flexible substrate is removed by the third micro-etching agent in the third micro-etching tank.

[0114] Furthermore, the time of the first micro-etching treatment is preferably 15 seconds.

[0115] Furthermore, the third micro-etching agent includes sulfuric acid and sodium persulfate, wherein the concentration of the sulfuric acid is 2% to 4%, and the concentration of the sodium persulfate is 20 g / L to 40 g / L.

[0116] Furthermore, the etching layer of the third micro-etching treatment is 0.2 μm to 0.4 μm. It should be noted that the oxide layer on the surface of the copper foil layer on both sides can be etched away in the first micro-etching treatment, that is, the etching layer on both sides is 0.2 μm to 0.4 μm, avoiding excessive etching and reducing the conductive effect of the copper foil layer, thereby ensuring that the ultra-thin FPC board has good conductive performance.

[0117] Furthermore, after the third micro-etching treatment is performed on the flexible substrate, the flexible substrate needs to be subjected to three-stage water washing. Specifically, the flexible substrate after the third micro-etching treatment passes through three water washing tanks in sequence, and the water washing time is 20s to 40s. The water washing method of each water washing tank is spray water washing, which can effectively remove the third micro-etching agent remaining on the flexible substrate and ensure the cleanliness of the board surface of the flexible substrate.

[0118] S730, performing an acid wash process on the flexible substrate after the third micro-etching process.

[0119] In this embodiment, since the flexible substrate after the third micro-etching treatment needs to undergo a three-stage water washing treatment, so that there is moisture on the surface of the flexible substrate, in order to reduce the influence of the water film on the copper plating and activate the copper surface of the flexible substrate, the flexible substrate after the third micro-etching treatment is pickled to effectively remove the moisture on the surface of the flexible substrate and make the copper surface contact the acid in advance to activate the copper surface, which plays a buffering role, thereby ensuring the smoothness of the subsequent electroplating treatment. Specifically, the flexible substrate is immersed in an acid washing tank for pickling treatment, and the immersion time is 15s to 60s, that is, the flexible substrate is cleaned by sulfuric acid in the acid washing tank, which effectively removes the moisture on the surface of the flexible substrate and can activate the copper surface of the flexible substrate, thereby avoiding the situation where watermarks appear on the board surface when the ultra-thin FPC board is formed.

[0120] It should be noted that the concentration of sulfuric acid in the pickling tank is 3% to 5%.

[0121] Furthermore, the pickling treatment time is preferably 30 seconds.

[0122] S740, immersing the pickled flexible substrate in a copper plating tank through a fixture for electroplating.

[0123] In this embodiment, the flexible substrate is immersed in a copper plating tank by a clamp, and the clamp is energized, electrons are transferred to the thickened carbon layer in the hole wall through the copper surface, and the copper ions free in the copper plating tank obtain two electrons on the thickened carbon layer and adhere to the thickened carbon layer of the flexible substrate to form a stable and dense conductive copper layer.

[0124] Furthermore, the chemical solution in the copper plating tank mainly contains sulfuric acid, copper sulfate and chloride ions, the concentration of sulfuric acid is 10% to 12%, the concentration of copper sulfate is 80g / L to 120g / L, and the concentration of chloride ions is 40ppm to 80ppm.

[0125] Furthermore, after the flexible substrate after pickling is immersed in a copper plating tank for electroplating by a fixture, the flexible substrate needs to be washed in three stages. Specifically, the flexible substrate after electroplating passes through three washing tanks in sequence, and the washing time is 20s to 40s. The washing method of each washing tank is spray washing, which can effectively remove the residual copper plating liquid on the flexible substrate and ensure the cleanliness of the board surface of the flexible substrate. The flexible board after washing is dried to ensure that there is no water residue on the surface of the flexible substrate, avoid the appearance of watermarks on the flexible substrate after molding, and further improve the yield rate of ultra-thin FPC boards.

[0126] In one embodiment, after the step of electroplating the flexible substrate after the second black hole treatment, the preparation process further includes the following steps:

[0127] The flexible substrate is subjected to circuit fabrication processing to obtain the ultra-thin FPC board.

[0128] It should be noted that the flexible substrate after hole metallization goes through the steps of dry film lamination, exposure, development, etching and film stripping in sequence, so that circuits are formed on the copper foil layers on both sides of the flexible substrate.

[0129] Furthermore, after the flexible substrate is processed for circuit fabrication, it is also necessary to perform pressing, curing and surface treatment on the flexible substrate to obtain an ultra-thin FPC board, wherein the surface treatment is gold immersion or gold plating.

[0130] In one embodiment, the specific operation steps of obtaining the flexible substrate are:

[0131] The flexible material is cut to obtain a PI board layer;

[0132] The first copper foil layer, the PI board layer and the second copper foil layer are sequentially stacked and pressed to obtain a flexible substrate;

[0133] Drying the flexible substrate;

[0134] The flexible substrate after the drying process is subjected to drilling process, so that a plurality of through holes are formed on the flexible substrate.

[0135] It should be noted that the flexible material is PI material, that is, polyimide. After pre-treatment of the flexible substrate, a flexible feed board with holes is obtained.

[0136] In one embodiment, the current density of the electroplating is 32ASF to 42ASF. The current of the electroplating is 250A to 540A. It is understandable that under this electroplating condition, copper can be plated on the thickened carbon layer. Furthermore, in order to improve the conductivity of the ultra-thin FPC board, the thickness of the copper plating is often increased, that is, the electroplating time needs to be increased, but the traditional preparation process is limited by the carbon hanging effect, resulting in the electroplating time being limited, resulting in the copper layer thickness generally being 10μm to 20μm, and even pinch point holes may occur. In this embodiment, the electroplating treatment time is 20min to 40min to obtain a copper layer thickness of 25μm to 30μm. It is precisely because of the combination of the above-mentioned roughening treatment, the first black hole treatment and the second black hole treatment that the thickened carbon layer in the hole wall of the flexible substrate can be treated during this electroplating treatment time without the carbon layer being broken. In other words, the conductivity of the ultra-thin FPC board is closely related to the roughening treatment, the first black hole treatment and the second black hole treatment, so that the flexible substrate can be treated during the electroplating time of 20min to 40min without the hole breaking phenomenon, further improving the conductivity of the ultra-thin FPC board, and further improving the yield rate of the ultra-thin FPC board in the thick copper preparation process.

[0137] In one embodiment, the first black hole liquid also includes potassium carbonate and polyethylene glycol, the mass proportion of potassium carbonate is 1%, and the mass proportion of polyethylene glycol is 7%. It should be noted that potassium carbonate can adjust the pH value of the first black hole liquid, improve the stability of the first black hole liquid, and can also adjust the surface tension of the first black hole liquid, so that the first black hole liquid can be evenly attached to the pore wall of the flexible substrate. Polyethylene glycol can increase the wettability and stability of the first black hole liquid, so that carbon black can be evenly dispersed in the system, making the formation of the carbon layer more dense and uniform.

[0138] In one embodiment, the second black hole liquid also includes potassium carbonate and polyethylene glycol, the mass proportion of potassium carbonate is 1%, and the mass proportion of polyethylene glycol is 7%. It should be noted that potassium carbonate can adjust the pH value of the second black hole liquid, improve the stability of the second black hole liquid, and can also adjust the surface tension of the second black hole liquid, so that the second black hole liquid can be evenly attached to the pore wall of the flexible substrate. Polyethylene glycol can increase the wettability and stability of the second black hole liquid, so that carbon black can be evenly dispersed in the system, making the formation of the thickened carbon layer more dense and uniform.

[0139] The present disclosure also provides an ultra-thin FPC board, which is prepared by using the preparation process of the ultra-thin FPC board described in any of the above embodiments.

[0140] In this embodiment, the ultra-thin FPC board obtained by using the above-mentioned ultra-thin FPC board preparation process has stronger conductive performance and higher yield rate.

[0141] Examples are listed below, but it should be noted that the following examples do not exhaust all possible situations, and the materials used in the following examples can be obtained from commercial channels unless otherwise specified.

[0142] Example 1

[0143] Step 1: Obtain a flexible substrate, on which a plurality of through holes are formed, wherein the thickness of the flexible substrate is 36 μm.

[0144] Step 2: After the flexible substrate is immersed in the PI adjuster in the PI adjustment tank for 45 seconds, it is passed into three water washing tanks in turn for spray water washing, and the washing time is 40 seconds. Among them, the PI adjuster solution includes a first PI adjuster and a second PI adjuster. The concentration of the first PI adjuster is 10%, and the concentration of the second PI adjuster is 20%. The first PI adjuster is PI adjuster M103A, and the second PI adjuster is PI adjuster M103D.

[0145] Step 3: After the flexible substrate is immersed in the first micro-etching agent of the first micro-etching tank for 30 seconds, it is sequentially passed into three water washing tanks for spray washing for 40 seconds. The concentration of sulfuric acid in the first micro-etching agent is 4%, and the concentration of sodium persulfate is 70g / L.

[0146] Step 4: After the flexible substrate is immersed in the detergent in the cleaning tank for 60 seconds, it is sequentially passed into three water washing tanks for spray washing. The washing time is 40 seconds. The concentration of the detergent is 12%, and the model of the detergent is black hole cleaner M8501.

[0147] Step 5: After the flexible substrate is immersed in the first black hole liquid of the first black hole cylinder for 30 seconds, the moisture of the flexible substrate is absorbed by the water absorbent cotton layer, and then the flexible substrate is subjected to the first strong wind drying treatment, and finally the flexible substrate is subjected to the first hot air drying treatment, wherein the mass proportion of carbon black in the first black hole liquid is 2.5%, the pressure of the first strong wind drying treatment is 5 kPa, and the temperature of the first hot air drying is 70°C.

[0148] Step 6: After the flexible substrate is immersed in the pore-forming agent in the pore-forming tank for 55 seconds, it is sequentially passed into three water washing tanks for spray washing. The washing time is 40 seconds. The concentration of the pore-forming agent is 8%, and the model of the pore-forming agent is black hole pore-forming agent M8502.

[0149] Step 7: After the flexible substrate is immersed in the second black hole liquid in the second black hole cylinder for 60 seconds, the moisture of the flexible substrate is absorbed by the water absorbent cotton layer, and then the flexible substrate is subjected to a second strong wind drying treatment, and finally the flexible substrate is subjected to a second hot air drying treatment, wherein the mass proportion of carbon black in the second black hole liquid is 7.5%, the pressure of the second strong wind drying treatment is 5 kPa, and the temperature of the second hot air drying is 70°C.

[0150] Step 8: After the flexible substrate is immersed in the second micro-etching agent of the second micro-etching tank for 30 seconds, it is sequentially passed into three water washing tanks for spray water washing, and the washing time is 40 seconds. The moisture of the flexible substrate is absorbed by the water absorbent cotton layer, and then the flexible substrate is subjected to a third strong wind drying treatment. Finally, the flexible substrate is subjected to a third hot air drying treatment, wherein the concentration of sulfuric acid in the second micro-etching agent is 4%, the concentration of sodium persulfate is 100g / L, the pressure of the third strong wind drying treatment is 5kPa, and the temperature of the third hot air drying is 80°C.

[0151] Step 9: After the flexible substrate is immersed in the degreasing agent in the degreasing tank for 25 seconds, it is sequentially passed into three water washing tanks for spray washing. The washing time is 40 seconds. The concentration of the degreasing agent is 4%, and the model of the degreasing agent is acid degreasing agent M401.

[0152] Step 10: After the flexible substrate is immersed in the third micro-etching agent in the third micro-etching tank for 15 seconds, it is sequentially passed into three water washing tanks for spray washing. The washing time is 40 seconds. The concentration of sulfuric acid in the third micro-etching agent is 4%, and the concentration of sodium persulfate is 40g / L.

[0153] Step 11: Soak the flexible substrate in sulfuric acid in a pickling tank for 30 seconds, and the concentration of sulfuric acid is 5%.

[0154] Step 12: Immerse the flexible substrate in a copper plating tank through a clamp for electroplating for 30 minutes, and then pass it into three water washing tanks for spray washing in turn. The washing time is 40 seconds, wherein the current density is 32ASF, the current size is 250A, the copper plating thickness is 28μm, the concentration of sulfuric acid in the copper plating solution is 12%, the concentration of copper sulfate is 120g / L, and the concentration of chloride ions is 80ppm.

[0155] Step 13: After the flexible substrate is dried, circuit fabrication, lamination curing and surface treatment are performed in sequence to obtain an ultra-thin FPC board.

[0156] Example 2

[0157] The difference from Example 1 is that the soaking time in step 2 is 30 seconds.

[0158] Example 3

[0159] The difference from Example 1 is that the soaking time in step 2 is 90 seconds.

[0160] Example 4

[0161] The difference from Example 1 is that the immersion time of step 5 is 90 seconds, step 6 and step 7 are deleted, the electroplating treatment time is 20 minutes, and the copper plating thickness is 20 μm.

[0162] Example 5

[0163] The difference from Example 1 is that step 2 is deleted, the electroplating treatment time is 20 minutes, and the copper plating thickness is 20 μm.

[0164] Comparative Example 1

[0165] The difference from Example 1 is that step 2, step 6 and step 7 are deleted.

[0166] Comparative Example 2

[0167] The difference from Example 1 is that the soaking time in step 2 is 120 s.

[0168] Comparative Example 3

[0169] The difference from Example 4 is that the electroplating treatment time is 30 minutes and the copper plating thickness is 30 μm.

[0170] Comparative Example 4

[0171] The difference from Example 5 is that the electroplating treatment time is 30 minutes and the copper plating thickness is 30 μm.

[0172] The hole wall conditions of the through holes near the pinch points after electroplating in Examples 1-5 and Comparative Examples 1-4 were observed, and the results are shown in Table 1.

[0173] Table 1

[0174]

[0175]

[0176] It can be seen from Table 1 that by comparing the data performance of Example 1 and Comparative Example 1, the ultra-thin FPC board disclosed in the present invention can not only overcome the hole breakage problem compared to the traditional process, but also adapt to the preparation requirements of thick copper, thereby improving the production yield of the ultra-thin FPC board.

[0177] By comparing the data performance of Examples 1-3 and Comparative Example 2, insufficient or excessive coarsening will affect the uniformity of the distribution of the copper layer, that is to say, insufficient or excessive coarsening will affect the uniformity of the adsorption of the carbon layer. In order to adapt to more sophisticated conductive needs and high conductive performance requirements, the thicker the copper layer and the more uniform its distribution is the key. Therefore, in the preparation process of the ultra-thin FPC board, the ultra-thin FPC board with the best copper plating effect can be obtained when the coarsening time is controlled at 45s. At the same time, under the conditions of the coarsening treatment, the first black hole treatment and the second black hole treatment, it can also meet the needs of users with thick copper, thereby greatly improving the yield rate of the ultra-thin FPC board with high conductive performance in the preparation.

[0178] By comparing the data performance of Example 4, Example 5, Comparative Example 3 and Comparative Example 4, although increasing the roughening treatment or increasing the solid content of the carbon layer can adapt to the preparation requirements of ordinary copper thickness, the requirement for high conductivity is that the thicker the copper thickness, the better. It is obvious from the data of Comparative Examples 3 and 4 that simply increasing the roughening treatment or increasing the solid content of the carbon layer can only make the carbon layer evenly distributed, but cannot increase the thickness of the carbon layer. Once the electroplating time increases, the carbon layer will still be punctured and holes will appear. This also shows that the roughening treatment and increasing the solid content of the carbon layer need to exist at the same time to meet the electroplating requirements of thick copper.

[0179] Compared with the prior art, the present invention has at least the following advantages:

[0180] 1. The flexible substrate is subjected to a roughening treatment under the conditions that the concentration of the first PI adjuster is 5% to 10%, the concentration of the second PI adjuster is 10% to 20%, and the roughening treatment time is 30s to 90s, which can effectively increase the roughness of the hole wall surfaces of several through holes of the flexible substrate. Then, by cleaning and modifying the flexible substrate, the grease on the board surface can be removed and the negative charge attached to the hole wall on the flexible substrate can be adjusted to a positive charge. In this way, when the first black hole liquid is used to perform the first black hole treatment on the flexible substrate, the carbon black carrying the negative charge in the first black hole liquid can be electrostatically adsorbed on the surface of the hole wall and form a carbon layer.

[0181] 2. By performing whole-hole treatment on the flexible substrate, the charge of the area without carbon hanging or the area with poor carbon hanging effect in the hole wall is adjusted to ensure that the charge carried by the area without carbon hanging or the area with poor carbon hanging effect in the hole wall is positive. In this way, when the second black hole liquid is used to perform the second black hole treatment on the flexible substrate, the carbon black carrying negative charge in the second black hole liquid can be electrostatically adsorbed on the surface of the hole wall. Because the mass proportion of carbon black in the first black hole liquid is 2.5%, and the mass proportion of carbon black in the second black hole liquid is 7.5%, the carbon layer on the surface of the hole wall can be thickened by increasing the mass proportion of carbon black in the second black hole liquid, and at the same time, a thickened carbon layer is formed in the area without carbon hanging on the hole wall, thereby ensuring that a thickened carbon layer can be formed in each area of ​​the hole wall, and when the flexible substrate is electroplated, the through hole near the pinch point will not be broken, ensuring that the ultra-thin FPC board has good conductivity.

[0182] The above-mentioned embodiments only express several implementation methods of the present disclosure, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the disclosed patent. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present disclosure, and these all belong to the protection scope of the present disclosure. Therefore, the protection scope of the disclosed patent shall be subject to the attached claims.

Claims

1. A preparation process for an ultra-thin FPC board, It is characterized in that The steps include: Obtaining a flexible substrate, wherein a plurality of through holes are formed on the flexible substrate; The flexible substrate is roughened by using a PI adjusting agent; Performing a cleaning and modification treatment on the flexible substrate after the roughening treatment; Using a first black hole liquid to perform a first black hole treatment on the flexible substrate after the cleaning and modification treatment; Performing a whole hole treatment on the flexible substrate after the first black hole treatment; Performing a second black hole treatment on the flexible substrate after the whole hole treatment using a second black hole liquid; Performing electroplating treatment on the flexible substrate after the second black hole treatment to obtain an ultra-thin FPC board; The PI adjuster includes a first PI adjuster and a second PI adjuster, the concentration of the first PI adjuster is 5% to 10%, the concentration of the second PI adjuster is 10% to 20%, and the roughening treatment time is 30s to 90s; The mass proportion of carbon black in the first black pore liquid is 2.5%, and the mass proportion of carbon black in the second black pore liquid is 7.5%.

2. The preparation process of the ultra-thin FPC board according to claim 1, It is characterized in that After the step of roughening the flexible substrate with a PI adjuster and before the step of cleaning and modifying the roughened flexible substrate, the preparation process further includes the following steps: A first micro-etching process is performed on the flexible substrate.

3. The preparation process of the ultra-thin FPC board according to claim 1, It is characterized in that After the second black hole treatment is performed on the flexible substrate after the whole hole treatment using the second black hole liquid, and before the operation step of electroplating the flexible substrate after the second black hole treatment, the preparation process further includes the following steps: The flexible substrate is subjected to a second micro-etching process.

4. The preparation process of the ultra-thin FPC board according to claim 1, It is characterized in that The specific operation steps of electroplating the flexible substrate after the second black hole treatment are as follows: Degreasing the flexible substrate; Performing a third micro-etching process on the flexible substrate after the degreasing process; Performing pickling treatment on the flexible substrate after the third micro-etching treatment; The flexible substrate after pickling is immersed in a copper plating tank through a fixture for electroplating.

5. The preparation process of the ultra-thin FPC board according to claim 1, It is characterized in that After the step of electroplating the flexible substrate after the second black hole treatment, the preparation process further includes the following steps: The flexible substrate is subjected to circuit fabrication processing to obtain the ultra-thin FPC board.

6. The preparation process of the ultra-thin FPC board according to claim 1, It is characterized in that The specific operation steps of obtaining the flexible substrate are: The flexible material is cut to obtain a PI board layer; The first copper foil layer, the PI board layer and the second copper foil layer are sequentially stacked and pressed to obtain a flexible substrate; Drying the flexible substrate; The flexible substrate after the drying process is subjected to drilling process, so that a plurality of through holes are formed on the flexible substrate.

7. The process for preparing the ultra-thin FPC board according to claim 4, It is characterized in that The current density of the electroplating is 32ASF to 42ASF; The electroplating current is 250A-540A.

8. The process for preparing the ultra-thin FPC board according to claim 1, It is characterized in that The first black hole liquid also includes potassium carbonate and polyethylene glycol, the mass proportion of the potassium carbonate is 1%, and the mass proportion of the polyethylene glycol is 7%.

9. The process for preparing the ultra-thin FPC board according to claim 1, It is characterized in that The second black hole liquid also includes potassium carbonate and polyethylene glycol, the mass proportion of the potassium carbonate is 1%, and the mass proportion of the polyethylene glycol is 7%.

10. An ultra-thin FPC board, It is characterized in that The ultra-thin FPC board is prepared by the preparation process of any one of claims 1 to 9.

Citation Information

Cited By

  • Circuit board black hole process and circuit board

    CN119855049A

  • Rigid-flex board manufacturing process optimization method for improving circuit reliability

    CN120692760A