Spherical crystalline silica particles, method for producing same, and resin composite composition and resin composite comprising same

By performing specific heat treatment on spherical silica particles, the crystallization rate and moisture release amount are improved, the problem of large dielectric loss tangent in the prior art is solved, and the excellence of spherical crystalline silica particles in high-frequency equipment is achieved. Dielectric properties and thermal properties.

CN118946527APending Publication Date: 2024-11-12NIPPON STEEL CHEM & MATERIAL CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202380030260.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-25
Filing Date
2023-03-24
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing spherical silica particles have a large dielectric loss tangent in high-frequency equipment, which is difficult to meet the low dielectric loss requirements in the millimeter wave band. The thermal expansion rate and thermal conductivity are insufficient, which affects the performance of the equipment.

Method used

By performing heat treatment of amorphous spherical silica particles at a temperature of 450°C or more than 830°C in an atmosphere containing water vapor, the crystallization rate and moisture release amount are improved. It makes it a spherical crystalline silica particle with high crystallinity, enhancing its dielectric properties.

Benefits of technology

It significantly reduces the dielectric loss tangent, improves the thermal expansion and thermal conductivity, and is suitable for semiconductor sealing materials in high-frequency equipment, enhancing the performance and stability of the equipment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005059103850000231
    Figure BDA0005059103850000231
Patent Text Reader

Abstract

The present invention provides spherical silica particles which are preferably used as a filler for a semiconductor sealing material having excellent dielectric properties in the millimeter wave band, that is, have a high crystallization rate, and have excellent dielectric properties in the millimeter wave band. The present invention relates to spherical crystalline silica particles which have a high content of water released when heated to 800 DEG C or higher by a temperature-rising desorption gas analyzer, a method for producing the spherical crystalline silica particles, and a resin composite composition and a resin composite containing the spherical crystalline silica particles. Provided are: spherical crystalline silica particles characterized by having a circularity of 0.80 or more, containing crystalline silica in an amount of 50.0% or more relative to the total amount of the spherical crystalline silica particles, and having a crystallinity of 0.80 or more, a crystallinity of 0.80 or more relative to the total amount of the spherical crystalline silica particles, a method for producing the spherical crystalline silica particles, and a resin composite composition and a resin composite comprising the spherical crystalline silica particles; and the amount of water released when heated from 800 DEG C to 1000 DEG C by a temperature-rising desorption gas analyzer is 4.5 [mu] g / m2 or more.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to spherical silica particles and a method for producing the same, and in particular, to spherical crystalline silica particles that release more water when heated from 800°C to 1000°C than conventional spherical crystalline silica particles and a method for producing the same, as well as a resin composite composition and a resin composite body containing the spherical crystalline silica particles. Background Art

[0002] Due to the increase in the amount of information accompanying the advancement of communication technology, the rapid expansion of the use of millimeter wave bands such as millimeter wave radar, etc., the frequency is becoming higher. The circuit substrate that transmits these high-frequency signals is composed of electrodes and dielectric substrates as circuit patterns. In order to suppress the energy loss during the transmission of high-frequency signals, the dielectric material needs to have a smaller dielectric loss tangent (tanδ). In order to have low dielectric loss, the dielectric material should have low polarity and low dipole moment.

[0003] As dielectric materials, ceramic particles, resins and composites obtained by compounding them are mainly used. In particular, with the expansion of the use of millimeter wave bands in recent years, ceramic particles and resins with further low dielectric loss tangent (tanδ) are needed. The relative dielectric constant (εr) of the resin is relatively small, which is suitable for high-frequency devices, but the dielectric loss tangent (tanδ) and thermal expansion coefficient are larger than those of ceramic particles. Therefore, for the composite of ceramic particles and resins used in millimeter wave bands, it is suitable for (1) the low dielectric loss tangent (tanδ) of the ceramic particles themselves and (2) the high filling of the ceramic particles and the reduction of the amount of resin representing a larger dielectric loss tangent (tanδ).

[0004] As ceramic particles, silica (SiO2) particles have been used for a long time. When the shape of silica particles is angular, the fluidity, dispersibility and filling property in the resin will deteriorate, and the wear of the manufacturing device will also progress. In order to improve these, spherical silica particles are widely used. It is believed that the closer the spherical silica particles are to a true sphere, the better the filling property, fluidity and mold wear resistance in the resin will be, and particles with higher roundness are constantly sought. Furthermore, research is also constantly being conducted on further improvement of filling property based on the optimization of the particle size distribution of the particles.

[0005] Generally, as a method for preparing spherical silica, a melt-blowing method is used. During spraying, the particles are passed through a high temperature area such as a flame, whereby the particles are melted and the shape of the particles becomes spherical due to surface tension. The melted spherical particles are transported by air flow in a manner that the particles are not melted to each other and are recovered, but the particles after spraying are quenched. Because it is quenched from a molten state, the silica does not crystallize, has an amorphous structure, and becomes glass-like particles generally referred to as quartz glass.

[0006] Because the spherical silica particles based on the melt-blowing method are amorphous, their thermal expansion coefficient and thermal conductivity are low. The thermal expansion coefficient of amorphous silica particles is 0.5ppm / K, and the thermal conductivity is 1.4W / mK. Its thermal expansion coefficient is roughly the same as that of quartz glass, which has an amorphous (amorphous) structure but does not have a crystal structure. Roughly, the thermal expansion coefficient of Si, which is the main raw material of the IC chip, is 3-5ppm / K, and the thermal expansion coefficient of the sealing resin used to seal the IC chip is extremely large compared to Si. Therefore, due to the difference in the thermal expansion behavior of the two materials (Si and the sealing resin), the IC chip will be warped and cause obstacles to production. On the other hand, when the spherical silica with a smaller thermal expansion coefficient is highly filled in the resin with a larger thermal expansion coefficient, the effect of reducing the thermal expansion of the sealing material (the composite of spherical silica and resin) itself will be obtained. By setting the thermal expansion coefficient of the sealing material to a value close to Si, the deformation caused by the thermal expansion behavior when the IC chip is sealed can be suppressed. In addition, with respect to thermal conductivity, from the perspective of improving the heat dissipation from the IC chip, it is preferred to have high thermal conductivity.

[0007] As described above, the properties required of silica particles for sealing materials include excellent dielectric properties at high frequencies in the millimeter wave band, in addition to being able to be mixed with resins in large quantities to maintain the performance of the composite, such as filling properties, fluidity, and mold wear resistance. Dielectric properties are physical properties of the material, so it is difficult to reduce the dielectric loss tangent of amorphous silica particles.

[0008] On the other hand, it is known that there are cristobalite, quartz, tridymite, keatite, etc. as the crystal structure of silicon dioxide, and silicon dioxide having these crystal structures has a high thermal expansion coefficient and thermal conductivity and a low dielectric loss tangent compared with amorphous silicon dioxide. Therefore, various methods for crystallizing amorphous silicon dioxide to increase the thermal expansion coefficient and thermal conductivity and reduce the dielectric loss tangent have been proposed (Patent Documents 1 to 4).

[0009] Patent document 1 discloses a method for producing spherical crystalline silica particles, characterized in that the silica powder is adjusted to contain 400 to 5000 ppm of aluminum, the adjusted silica powder is sprayed, and the sprayed spherical silica particles are protected and fixed at 1100°C to 1600°C for 1 to 12 hours, and the cooled spherical silica particles have a crystal phase of 80% or more. It is recorded that 95% to 100% of the crystal phase is a cristobalite crystal phase.

[0010] Patent Document 2 describes a method for producing a spherical silica filler, characterized in that a spherical silica filler having a specific surface area of ​​40 m 2 / g or more, and the bulk density is 0.1g / cm 3 The following alumina powder is mixed with spherical amorphous silica having an average circularity of 0.90 or more so as to be 1000 ppm to 10000 ppm in terms of aluminum, and heated at 1200° C. to 1350° C. for 1 to 8 hours.

[0011] Patent document 3 describes a method for producing a porous powder whose main crystal phase is composed of quartz, which is characterized in that 0.5 mass % or more of a Zn compound calculated as ZnO is added to silica gel having an average particle size of 0.1 to 20 μm, and the mixture is heat treated at 900 to 1100°C.

[0012] In patent document 4, a method for producing spherical crystalline silica particles is shown, characterized in that it includes the following steps: in amorphous spherical silica particles, an alkali metal compound is mixed at a ratio of 0.4 to 5% by mass relative to the total mass of the amorphous spherical silica particles and the mass obtained by converting the alkali metal into oxides, or an alkaline earth metal is mixed at a ratio of 1 to 5% by mass relative to the total mass of the amorphous spherical silica particles and the mass obtained by converting the alkaline earth metal into oxides, and the mixed spherical silica particles are heat treated at 800°C to 1300°C, and the heat-treated spherical silica particles are cooled, and the cooled spherical silica particles have a crystal phase of more than 90% by mass, and quartz crystals account for more than 70% by mass of the whole. However, when the amount of alkali metal added is less than 0.4% by mass and the amount of alkaline earth metal is less than 1% by mass, the probability of quartz appearing will be lowered.

[0013] Prior art literature

[0014] Patent Literature

[0015] Patent Document 1: International Publication No. 2016 / 031823

[0016] Patent Document 2: Japanese Patent Application Publication No. 2019-19222

[0017] Patent Document 3: Japanese Patent Application Publication No. 2002-20111

[0018] Patent Document 4: International Publication No. 2018 / 186308

[0019] Patent Document 5: Japanese Patent Application Laid-Open No. 4-114065 Summary of the invention

[0020] Technical problem to be solved by the invention

[0021] The present inventors aim to explore filler particles for semiconductor sealing having excellent dielectric properties in the millimeter wave band of 30 GHz to 80 GHz, and to prepare resin composites for high-frequency equipment purposes obtained by mixing them with resin. In order to obtain a resin composite with a low dielectric loss tangent, first, spherical molten (amorphous) silica is heat-treated and crystallized. That is, it is confirmed that: for crystalline silica, the dielectric loss tangent in the millimeter wave band (30 GHz to 80 GHZ) is greatly reduced compared with the amorphous silica that has been widely used in the past. As a result, spherical crystalline silica particles will become silica particles showing excellent dielectric properties for high-frequency equipment purposes. The crystalline silica obtained in the heat treatment is quartz, cristobalite or a mixture thereof. Because the physical property values ​​are different in quartz and cristobalite, when used as a filler, it is preferred that the phase of crystalline silica is a single phase.

[0022] In the resin composition used for semiconductor sealing in the past, in order to improve the thermal shock strength, a method of filling as much as possible the silicon dioxide particles with a thermal expansion coefficient close to the silicon chip as the filling material of the sealing resin is adopted, and its filling rate reaches 70-90% of the entire resin composition by weight. At this time, it has become a common technique (for example, patent document 5) to add a silane coupling agent to the resin composition to improve the adhesion of the filling material and the resin. However, it is known that: in the silicon dioxide powder obtained by heat-treating the spherical amorphous silicon dioxide particles and crystallizing at least a part of it, even if a silane coupling agent is added, the adhesion with the resin will not be fully improved.

[0023] It is known that the reaction site of the silane coupling agent and the silica particles is the silanol group (Si-OH) present on the surface of the silica particles. On the other hand, in the method of crystallizing spherical amorphous silica described in the prior patent documents, Patent Document 1 discloses heat treatment at 1100°C to 1600°C, Patent Document 2 discloses heat treatment at 1200°C to 1350°C, Patent Document 3 discloses heat treatment at 900°C to 1100°C, and further Patent Document 4 discloses heat treatment at 800°C to 1300°C. Therefore, as the reason why the adhesion with the resin is not sufficiently improved even if the silane coupling agent is added, it is presumed that the silanol group on the surface of the silica forms a siloxane bond (Si-O-Si) through a dehydration condensation reaction, and the silanol group as the reaction site with the silane coupling agent almost disappears. The silanol group on the particle surface undergoes a dehydration condensation reaction when heated at 800°C or above. The silanol groups on the particle surfaces can be measured by analyzing the silica powder using a temperature-increasing desorption gas analyzer and detecting the amount of water released when heated to 800° C. or higher. Therefore, in order to improve the reactivity with the silica coupling agent in the spherical crystalline silica particles preferred as fillers for semiconductor sealing materials having excellent dielectric properties in the millimeter wave band, it is considered that a silica particle is required whose amount of water released when heated to 800° C. or higher using a temperature-increasing desorption gas analyzer is greater than that of conventional spherical crystalline silica.

[0024] Therefore, the object of the present invention is to provide a spherical crystalline silica particle and a method for producing the same, as well as a resin composite composition and a resin composite containing the spherical crystalline silica particles, wherein the spherical crystalline silica particles are preferably used as fillers for semiconductor sealing materials having excellent dielectric properties in the millimeter wave band, that is, spherical silica particles with a high crystallization rate and a larger amount of water released when heated to above 800°C by a temperature-raising desorption gas analyzer than conventional spherical crystalline silica particles.

[0025] Technical means for solving technical problems

[0026] The inventors of the present application have conducted intensive research for the purpose of solving the above-mentioned problems. As a result, it was found that: a powder composed of amorphous spherical silica particles is heat-treated at a temperature of 900°C to 1550°C to be crystallized, and then heat-treated at a temperature of 450°C to 830°C in an atmosphere containing at least water vapor. Thus, compared with the previous crystalline silica, the amount of water released when it is heated to above 800°C by a temperature-raising degassing gas analyzer can be increased, and it can be restored to the same amount as the amorphous silica particles before crystallization or to a higher amount. The circularity of the crystalline silica obtained in the heat treatment is above 0.80. In addition, the seed crystals may also be quartz, cristobalite or a mixture thereof. Because the physical property values ​​are different in quartz and cristobalite, when used as a filler, it is preferred that the phase of the crystalline silica is a single phase. Here, so-called single phase refers to that quartz or cristobalite accounts for more than 80.0% mass % of crystalline silicon dioxide. In addition, in order to distinguish the heat treatment of the former from the latter, it is also possible to refer to the former as the first heat treatment, or crystallization heat treatment, and the latter as the second heat treatment, or water vapor atmosphere heat treatment.

[0027] According to the present invention, the following spherical silica particles and a method for producing the same are provided.

[0028] (1) A spherical crystalline silica particle characterized by having a circularity of 0.80 or more, containing 50.0% or more of the whole crystalline silica, and releasing a moisture content of 4.5 μg / m when heated from 800° C. to 1000° C. by a temperature-elevated desorption gas analyzer. 2 above.

[0029] (2) The spherical crystalline silica particles according to (1), wherein the water content is 7.0 μg / m 2 above.

[0030] (3) The spherical crystalline silica particles according to any one of (1) to (2), wherein the proportion of quartz or cristobalite in the crystalline silica is 80.0% by mass or more.

[0031] (4) The spherical crystalline silica particles according to any one of (1) to (3), comprising 75.0% or more of the entire crystalline silica.

[0032] (5) The spherical crystalline silica particles according to any one of (1) to (4), wherein the water content is 50.0 μg / m 2 the following.

[0033] (6) A method for producing spherical crystalline silica particles as described in any one of (1) to (5), comprising: after crystallizing spherical amorphous silica particles by heat treating them at a temperature of not less than 900°C and not more than 1550°C, heat treating them at a temperature of not less than 450°C and not more than 830°C in an atmosphere containing water vapor.

[0034] (7) A resin composite composition, characterized in that the spherical crystalline silica particles according to any one of (1) to (5) are contained in a resin.

[0035] (8) A resin composite, characterized in that it is obtained by curing the resin composite composition described in (7).

[0036] Effects of the Invention

[0037] According to the present invention, it is possible to provide spherical silica particles which are preferably used as fillers for semiconductor sealing materials having excellent dielectric properties in the millimeter wave band, that is, spherical crystalline silica particles which have a high crystallization rate and release more water than conventional spherical crystalline silica particles when heated to 800° C. or higher by a temperature-increasing desorption gas analysis device, and a method for producing the same. Furthermore, it is possible to increase the proportion of cristobalite or quartz. DETAILED DESCRIPTION

[0038] The spherical crystalline silica according to one embodiment of the present invention is a spherical crystalline silica particle, characterized in that the spherical crystalline silica particle has a circularity of 0.80 or more, contains 50.0% or more of the whole crystalline silica, and the amount of water released when heated from 800° C. to 1000° C. by a temperature-increasing desorption gas analysis device is quantified, and the quantified water amount is 4.5 μg / m 2 The so-called crystalline silica phase of 50.0% or more mentioned here refers to the proportion of the crystalline silica phase in the spherical silica particles, and the method for obtaining it will be described later. In addition, the water (H2O) released when the silica particles are heated from 800°C to 1000°C is quantified by a temperature-desorbed gas analyzer.

[0039] As the crystal structure of silicon dioxide (SiO2), there are cristobalite, quartz, etc. The silicon dioxide with these crystal structures has high thermal conductivity compared with amorphous silicon dioxide. Therefore, it is possible to improve the heat dissipation from IC chip by replacing the amorphous silicon dioxide of an appropriate amount with crystalline silicon dioxide in the semiconductor sealing filler. And then, because the dielectric loss tangent in the millimeter wave band of crystalline silicon dioxide is low, the more amorphous silicon dioxide is replaced with crystalline silicon dioxide in the semiconductor sealing filler, the more the dielectric loss tangent of semiconductor sealing material will be reduced. In the past, spherical crystalline silicon dioxide was made by heat-treating spherical amorphous silicon dioxide and crystallizing it. About the crystalline silicon dioxide obtained, even if it is reacted with a silane coupling agent, the adhesion with resin will not be fully improved. This is believed to be because spherical amorphous silica is calcined at a high temperature of 800° C. or higher during crystallization, so that silanol groups on the surface of silica undergo a dehydration condensation reaction, which reduces or eliminates the silanol groups, resulting in almost no reactive sites with the silane coupling agent.

[0040] On the other hand, the crystalline silica of the present invention can be produced by heat treating at a temperature of 900°C to 1550°C, and after crystallization, heat treating at a temperature of 450°C to 830°C in an atmosphere containing water vapor. The spherical crystalline silica can be set to have a water content of 4.5 μg / m3 when heated from 800°C to 1000°C by a temperature-elevated desorption gas analyzer. 2 The more water is released, the higher the concentration of silanol groups (Si-OH) on the surface of silica. Therefore, the more reactive sites for silane coupling treatment increase. Therefore, the more preferably the amount of released water is 7.0 μg / m 2 On the other hand, when the amount of water released is too much, the dielectric loss tangent may increase due to the increase of functional groups, and the dielectric loss tangent reduction effect brought about by the introduction of crystalline silica may be lost. Therefore, the upper limit of the water content may also be 50 μg / m 2 More preferably, the density may be 30 μm / m, which is equivalent to that of spherical amorphous silica. 2 In addition, the amount of water released from the spherical amorphous silica powder produced by the flame melting method as a conventional technique when heated to 800°C to 1000°C by a temperature-increasing desorption gas analyzer was 7.4 μg / m 2 ~27.9 μg / m 2 .

[0041] (Spherical amorphous silica particles)

[0042] Amorphous spherical silica particles as raw materials can be produced by methods such as melt-blowing. In the melt-blowing method, natural silica powder that has been crushed and adjusted to a desired particle size is passed through a flame, whereby the particles are melted and the shape of the particles becomes spherical due to surface tension. Spherical amorphous silica particles can be produced by this melt-blowing method.

[0043] Regarding the composition of the spherical amorphous silica particles, the main component is silicon dioxide, and as long as the final spherical crystalline silica particles are within the desired range, they are not particularly limited. As a scheme, the composition of the spherical amorphous silica particles can also be 98.0% by mass or more of silicon dioxide (SiO2), and in addition, as trace elements, Ca, Li, Al, Na, Mg, Ba, Zn, etc. can also be included.

[0044] (Method for producing spherical crystalline silica particles)

[0045] [Crystallization heat treatment]

[0046] The spherical crystalline silica particles of the present invention are manufactured by heat treating spherical amorphous silica. In order to promote crystallization into quartz, for example, it can also be mixed with calcium element or lithium element, and the mixture (also referred to as mixed raw material) is heat treated to manufacture. The crystallization temperature into quartz is preferably above 900°C and below 1200°C. Regarding the crystallization temperature, the preferred range varies depending on the type of crystallization promoter. In the case of adding calcium element, the crystallization temperature can also be set to the range of 1050°C to 1200°C. In the case of adding lithium element, the crystallization temperature can also be set to 950°C to 1100°C. On the other hand, even if a crystallization promoter is not added, crystallization into cristobalite can be carried out when the heat treatment temperature exceeds 1200°C. However, when the temperature exceeds 1550°C, the particles are fixed to each other due to sintering. Therefore, for crystallization into cristobalite, a heat treatment temperature of 1250°C to 1500°C is preferred. The heat treatment atmosphere for crystallization can be carried out in an oxidizing atmosphere such as air and an inert gas atmosphere such as nitrogen or argon. Because heat treatment is performed in large quantities in industry, the atmospheric pressure is preferably atmospheric pressure. On the other hand, the atmospheric pressure can be increased by a hot isostatic pressing device or the like. Typically, when the atmospheric pressure is above 125 MPa and below 200 MPa, the crystallization rate to quartz can be increased by setting the heat treatment temperature to above 1125°C and below 1300°C, thereby not using alkali metal elements such as lithium as a crystallization promoter. The heat treatment time for crystallization can be appropriately adjusted. It is 0.5 hours to 24 hours, preferably 1 hour to 12 hours. In addition, when heat treatment is performed in an electric furnace, the heating rate and cooling rate during the heat treatment for crystallization will not have a significant effect on the appearance of spherical crystalline silica particles.

[0047] [Heat treatment in steam atmosphere]

[0048] The spherical crystalline silica particles of the present invention can be manufactured in the following manner: after the spherical amorphous silica is crystallized by heat treatment, heat treatment is performed in an atmosphere containing water vapor at a temperature of at least 450°C to 830°C. The heat treatment in an atmosphere containing water vapor can be carried out separately from the heat treatment for crystallization, or water vapor can be introduced into the atmosphere during the cooling process of the heat treatment for crystallization. For the water vapor pressure, there is a maximum value determined by the gas temperature, and at a pressure exceeding this value, it cannot exist in the state of water vapor. This maximum value is called the saturated water vapor pressure, and the saturated water vapor pressure (Pa) can be approximately calculated according to the Tetens formula.

[0049] Pa(hPa)=6.1078×10 7.5T / (T+237.3)

[0050] T: Temperature [℃]

[0051] The water vapor atmosphere during the heat treatment can be formed by passing the atmosphere through a foaming device having a temperature adjustment function, and can be supplied to the furnace. By doing so, the volume ratio of water vapor to the total volume of atmospheric gas and water vapor (water vapor content) can be varied in the range of 5% to 90% by controlling the temperature of the bubble device. Considering the change in water vapor pressure relative to the foaming temperature, it is preferred that the water vapor content is in the range of 10% to 70%. The heat treatment in an atmosphere containing water vapor can also be carried out under pressure, but atmospheric pressure is industrially preferred. The heat treatment time in the water vapor atmosphere is 1 hour to 48 hours. Preferably, it is 5 hours to 25 hours.

[0052] (Quartz crystallization accelerator)

[0053] (Calcium raw materials)

[0054] Regarding the calcium raw material, for example, it can also be mixed with spherical amorphous silica particles and heat-treated. Regarding the composition and mixing amount of the calcium raw material, as long as the spherical crystalline silica particles finally obtained become the desired range, it is not particularly limited and will be appropriately adjusted. The calcium raw material can be calcium hydroxide or calcium oxide, etc., which exist stably in the atmosphere, or it can be a natural mineral. The calcium raw material can be added in a state such as a powder or an aqueous solution in order to be uniformly mixed with the spherical amorphous silica particles. In addition, it can also be that at least a part of the calcium raw material is a trace element contained in the spherical amorphous silica particles. For example, when the spherical amorphous silica particles fully contain calcium and become the desired calcium content in the spherical crystalline silica particles finally obtained, the spherical amorphous silica particles can also be used as a calcium raw material. In addition, in the case where the spherical amorphous silica particles contain calcium but are not enough, the calcium raw material can be added so that the desired calcium content is obtained in the spherical crystalline silica particles finally obtained.

[0055] (Lithium raw materials)

[0056] Regarding the lithium raw material, for example, it can also be mixed with spherical amorphous silica particles and heat-treated. Regarding the composition and mixing amount of the lithium raw material, as long as the spherical crystalline silica particles finally obtained are within the desired range, they are not particularly limited and will be appropriately adjusted. Regarding the lithium raw material, the form of oxides, carbonates, hydroxides, nitrates, etc., added is not particularly limited. In order to be uniformly mixed with amorphous spherical silica particles, it can be added in a state such as a powder or an aqueous solution. In addition, it can also be that at least a part of the lithium raw material is a trace element contained in the spherical amorphous silica particles. For example, the spherical amorphous silica particles fully contain lithium, and as long as the desired lithium content is obtained in the spherical crystalline silica particles finally obtained, the spherical amorphous silica particles can also be used as a lithium raw material. In addition, in the case where the spherical amorphous silica particles contain lithium but are not enough, a lithium raw material can be added so that the desired lithium content is obtained in the spherical crystalline silica particles finally obtained.

[0057] (Mixed with crystallization accelerator)

[0058] It is also possible that the spherical amorphous silica particles are mixed with one or both of the calcium raw material and the lithium raw material. In addition, the calcium raw material and / or the lithium raw material may also be contained in the spherical amorphous silica. As long as the raw materials are evenly dispersed and mixed in the mixture, the method for mixing is not particularly limited. The mixing may also be carried out by a powder mixer. By mixing, the calcium raw material and the lithium raw material are in contact with at least a portion of the spherical amorphous silica, and in the subsequent heat treatment process, the crystallization of the spherical amorphous silica, especially the crystallization to quartz, is promoted.

[0059] Furthermore, since mixing causes the calcium raw material and the lithium raw material to contact at least a part of the spherical amorphous silica, the pulverization of the spherical amorphous silica is not promoted, and therefore the circularity thereof is hardly reduced before and after mixing.

[0060] The circularity of the spherical crystalline silica of the present invention may be reduced slightly before and after the heat treatment for crystallization and the heat treatment in a water vapor atmosphere. Amorphous silica particles may be combined by welding or sintering, and the circularity may be greatly reduced. However, since the spherical crystalline silica particles of the present invention are crystalline (no longer amorphous), it is possible to suppress the particles from being combined by welding or sintering.

[0061] (Circularity)

[0062] The circularity of the spherical crystalline silica particles of the present invention is 0.80 or more. When the circularity is less than 0.80, when the silica particles of the resin composite composition used as semiconductor sealing materials are used, the fluidity, dispersibility and filling property are insufficient, and the wear of the sealing material manufacturing machine is sometimes promoted. Regarding the spherical amorphous silica particles obtained by the melt-blowing method, particles with a higher average circularity can be obtained. After the heat treatment for crystallization and the heat treatment in the water vapor atmosphere, the circularity of the silica particles will change slightly, but in the present invention, after the heat treatment, the circularity of the spherical amorphous silica particles before the heat treatment will be adjusted so that the circularity becomes 0.80 or more. From the viewpoint of improving fluidity, dispersibility, filling property and reducing the wear of the machine, the higher the circularity after the heat treatment, the better, it can also be 0.85 or more, and it can also be 0.90 or more. On the other hand, sometimes the circularity is set to 1.0, that is, there is a situation where it is difficult to set it to a perfect circle, so the upper limit of the circularity can also be set to less than 0.99 or less than 0.97.

[0063] The circularity is calculated as "the circumference of the circle equivalent to the projected area of ​​the photographic particles ÷ the circumference of the photographic particle image", and the closer the value is to 1, the closer it is to a true sphere. The circularity of the present invention is calculated by flow particle image analysis. In the flow particle image analysis, spherical crystalline silica particles are made to flow through a liquid and photographed as a still image of the particles, and image analysis is performed based on the obtained particle image to calculate the circularity of the spherical crystalline silica particles. The average value of these multiple circularities is taken as the average circularity. When the number of particles is too small when measuring the average circularity by the flow particle image analysis method, the average value cannot be obtained correctly. At least 100 particles are required, preferably 500 or more, and more preferably 1000 or more. In the present invention, a flow particle image analyzer "FPIA-3000" (manufactured by Spectris) is used, and about 100 particles are used. In addition, the circularity of spherical amorphous silica particles is also calculated in the same way.

[0064] (Properties of crystals)

[0065] The spherical crystalline silica particles of the present invention contain a crystalline silica phase, and the proportion of the crystalline silica phase in the spherical crystalline silica particles (as a whole) is 50.0% or more. In the case where the silica particles obtained by heat treatment are composed of amorphous and crystalline silica, the existence ratio of amorphous and crystalline silica (the so-called "degree of crystallinity", which is sometimes referred to as such in this specification) and the type of crystalline silica and its ratio can be obtained by XRD. In the XRD measurement, the proportion of the crystalline phase can be calculated by the following formula based on the sum of the integrated intensities of the crystalline peaks (Ic) and the integrated intensity of the amorphous halo part (Ia). More specifically, the proportion of the crystalline silica phase contained in the spherical crystalline silica particles can be obtained.

[0066] X (crystal phase ratio) = Ic / (Ic+Ia)×100(%)

[0067] In the present invention, XRD measurement was performed in the range of 2θ = 10° to 90°. The crystal phase ratio was obtained based on the sum of the crystalline peak intensities appearing in the 2θ measurement range and the integrated intensity of the halo part caused by the wider amorphous phase appearing near 2θ = 22°.

[0068] In the spherical crystalline silica of the present invention, the proportion of quartz or cristobalite in the phase of crystalline silica can also be 80.0% by mass or more. The types of crystalline phases of quartz, cristobalite, etc. and their respective proportions (mass %) can be obtained by quantitative analysis using X-ray diffraction. In the present invention, regarding the quantitative analysis based on X-ray diffraction, an analysis method based on the Rietveld method is used, and quantitative analysis is performed without using a standard sample. In the present invention, an X-ray diffraction device "D2PHASER" (manufactured by Bruker) is used. The quantitative analysis of the crystalline phase based on the Rietveld method is performed using the crystal structure analysis software "TOPAS" (manufactured by Bruker).

[0069] The spherical crystalline silica particles of the present invention contain a crystalline silica phase, and the ratio of the crystalline silica phase in the spherical crystalline silica particles (as a whole) is 50.0% or more, that is, it has a high crystallinity of 50.0% or more, and the dielectric loss tangent is preferably significantly lower than that of amorphous silica. From the viewpoint of reducing the dielectric loss tangent, the higher the crystallinity, the better, and it can be 70.0% or more, more preferably, it can be 75.0% or more, and further preferably, it can be 90.0% or more.

[0070] The spherical crystalline silica particles of the present invention include the phase of crystalline silica, and the ratio of quartz or cristobalite to the phase of the crystalline silica is relatively high, and may be more than 80.0% by mass, or may be substantially a single phase of quartz or cristobalite. Therefore, each characteristic of the spherical crystalline silica particles, such as the coefficient of thermal expansion and thermal conductivity, is substantially determined according to the characteristics of quartz or cristobalite, that is, it will not change, and is preferably used for fillers, etc. From the above viewpoint, the higher the ratio of quartz or cristobalite, the better, and may be more than 85.0% by mass, and further preferably, may be more than 90.0% by mass.

[0071] (Average particle size)

[0072] In one embodiment of the present invention, the average particle size (D50) of the spherical crystalline silica particles may also be 1 to 100 μm. When the average particle size is less than 1 μm, the agglomeration of the particles will increase and the fluidity will be significantly reduced, so it is not preferred. When the average particle size exceeds 100 μm, the gaps between the particles will easily remain, making it difficult to improve the filling property, which is not preferred. An average particle size of 2 to 50 μm is a more preferred range.

[0073] Regarding the average particle size (D50), in the volume-based particle size distribution measured by the laser diffraction and scattering particle size distribution measurement method, the median particle size D50 with a cumulative volume of 50% is calculated. In addition, the laser diffraction and scattering particle size distribution measurement method is a method as follows: a dispersion obtained by dispersing spherical crystalline silica particles is irradiated with a laser, and the particle size distribution is calculated based on the intensity distribution pattern of the diffraction and scattered light emitted from the dispersion. In the present invention, a laser diffraction and scattering particle size distribution measuring device "CILAS920" (manufactured by CILAS) is used. In addition, the average particle size of spherical amorphous silica particles can also be calculated in the same way.

[0074] (Specific surface area)

[0075] The specific surface area was measured by the BET method using Tristar II manufactured by Micromeritics. The BET method is an analytical method in which nitrogen gas molecules with a known adsorption area are adsorbed on the surface of powder particles and the specific surface area of ​​the sample is determined from the amount of adsorbed nitrogen gas molecules.

[0076] (Temperature-rising gas analysis)

[0077] The amount of water released when the silica particles are heated is analyzed by temperature desorption gas analysis. Temperature desorption gas analysis is a mass spectrometry method that can monitor the gas generated when heating / heating in a high vacuum for each temperature. The temperature desorption gas analysis device used is the TDS1200 manufactured by Electronic Science Co., Ltd. After the silica powder sample is placed in a quartz sample holder, it is placed on a sample stand and placed under high vacuum (10 -7 Pa) was heated from the bottom of the table by a halogen lamp. In the temperature-increasing desorption gas analyzer manufactured by Electronic Science Co., Ltd., there are two types of thermocouples: one inserted into the sample table and the other arranged above the sample table. Heating control is performed using the sample table thermocouple. In addition, the sample temperature is measured using a thermocouple (W-Re) arranged on the top of the table, and the tip of the thermocouple is brought into contact with the bottom of the quartz rack. The amount of released gas from the quartz boat was measured in advance (blank measurement). For the gas generated by heating, the ion current intensity of m / z 18 obtained by the quadrupole mass analyzer was accumulated, and the moisture content was calculated using the TDS1200 analysis software (TDS data processing application Ver5.2.0.5). The moisture content was quantified from room temperature to 1000°C. Since the amount of water caused by dehydration condensation of silanol groups on the surface of silica is released by heating at 800°C or higher, the amount of water released at 800°C to 1000°C is focused on.

[0078] (Application example)

[0079] According to the present invention, a composite composition of finally obtained spherical crystalline silica particles and a resin can be produced, and further, a resin composite obtained by curing the resin composite composition can be produced. The composition of the resin composite composition will be described below.

[0080] The slurry composition containing spherical crystalline silica particles and resin can be used to obtain a resin composite composition such as a semiconductor sealing material (especially, a solid sealing material), an interlayer insulating film, etc. Furthermore, by curing these resin composite compositions, a resin composite such as a sealing material (cured body) and a semiconductor packaging substrate can be obtained.

[0081] When manufacturing the resin composite composition, for example, in addition to the spherical crystalline silica particles and the resin, a curing agent, a curing accelerator, a flame retardant, a silane coupling agent, etc. may be mixed as needed, and compounded by a known method such as kneading. Furthermore, the resin composite composition may be formed into a granular shape, a film shape, etc. according to the application.

[0082] In addition, when manufacturing the resin composite composition, in addition to the spherical crystalline silica particles and the resin, other inorganic fillers may be mixed, and examples of the inorganic fillers include amorphous spherical silica particles, aluminum oxide particles, titanium dioxide particles, magnesium oxide particles, aluminum nitride particles, boron nitride particles, barium titanate particles, and calcium titanate particles. The mixing ratio of the inorganic filler can be appropriately adjusted according to the use of the resin composite composition.

[0083] Furthermore, when the resin composite composition is cured to produce a resin composite, for example, the resin composite composition can be heated to melt it, processed into a shape corresponding to the application, and then a higher heat than that during melting is applied to completely cure it. In this case, a known method such as transfer molding can be used.

[0084] For example, in the case of manufacturing semiconductor-related materials such as a substrate for packaging or an interlayer insulating film, as a resin used in a resin composite composition, a known resin can be applied, but preferably, an epoxy resin is used. The epoxy resin is not particularly limited, but for example, bisphenol A type epoxy resin, bisphenol F type epoxy resin, biphenyl type epoxy resin, phenol novolac type epoxy resin, cresol novolac type epoxy resin, naphthalene type epoxy resin, phenoxy type epoxy resin, etc. can be used. One of them can be used alone, or two or more types with different molecular weights can be used in combination. Among them, from the viewpoint of curability, heat resistance, etc., an epoxy resin having two or more epoxy groups in one molecule is also preferred. Specifically, biphenyl epoxy resins, phenol novolac epoxy resins, o-cresol novolac epoxy resins, resins obtained by epoxidizing phenolic and aldehyde novolac resins, glycidyl ethers such as bisphenol A, bisphenol F, and bisphenol S, glycidyl acid epoxy resins obtained by reacting polyacids such as phthalic acid or dimer acid with epichlorohydrin, linear aliphatic epoxy resins, alicyclic epoxy resins, heterocyclic epoxy resins, alkane-modified multifunctional epoxy resins, β-naphthol novolac epoxy resins, 1,6-dihydroxynaphthalene epoxy resins, 2,7-dihydroxynaphthalene epoxy resins, bishydroxybiphenyl epoxy resins, and epoxy resins into which halogens such as bromine are introduced for imparting flame retardancy, etc. Among these epoxy resins having two or more epoxy groups in one molecule, bisphenol A epoxy resins are particularly preferred.

[0085] In addition, resins other than epoxy resins can also be used for applications other than composite materials for semiconductor sealing materials, such as prepregs for printed circuit boards, various engineering plastics, and other resin composite compositions. Specifically, in addition to epoxy resins, polyamides such as silicone resins, phenolic resins, melamine resins, urea resins, unsaturated polyesters, fluororesins, polyimides, polyamide-imides, and polyetherimides; polyesters such as polybutylene terephthalate and polyethylene terephthalate; polyphenylene sulfide, aromatic polyesters, polysulfones, liquid crystal polymers, polyether sulfones, polycarbonates, maleimide-modified resins, ABS resins, AAS (acrylonitrile-acrylic rubber·styrene) resins, and AES (acrylonitrile·ethylene·propylene·diene rubber-styrene) resins can also be cited.

[0086] As the curing agent used for the resin composite composition, a known curing agent may be used to cure the resin, and for example, a phenolic curing agent may be used. As the phenolic curing agent, phenol novolac resin, alkylphenol novolac resin, polyvinylphenol, etc. may be used alone or in combination of two or more.

[0087] The equivalent ratio of the amount of the phenol curing agent to the epoxy resin (phenolic hydroxyl equivalent / epoxy equivalent) is preferably 0.1 or more and less than 1.0. This eliminates the residual unreacted phenol curing agent and improves the moisture absorption heat resistance.

[0088] Regarding the amount of spherical crystalline silica particles added to the resin composite composition of the present invention, from the viewpoint of heat resistance and thermal expansion coefficient, it is preferably more, but usually, it is 70% by mass or more and 95% by mass or less, preferably, 80% by mass or more and 95% by mass or less, and more preferably, 85% by mass or more and 95% by mass or less is appropriate. The reason is that when the amount of silica powder is too small, it is difficult to obtain the effects of improving the strength of the sealing material or inhibiting thermal expansion. In addition, on the contrary, the reason is that when it is too much, it has nothing to do with the surface treatment of the silica powder. In the composite material, segregation caused by the agglomeration of silica powder will be easily caused, and the viscosity of the composite material will also be too large. Starting from these problems, it will become difficult to be practical as a sealing material.

[0089] As the silane coupling agent, a known silane coupling agent can be used, but a silane coupling agent having an epoxy functional group is preferred.

[0090] [Example]

[0091] The present invention will be described below with reference to the following examples and comparative examples, but the present invention is not to be construed as being limitative of the following examples.

[0092] (Example 1 to Example 6)

[0093] Amorphous silica particles were produced by melt blowing. After calcium hydroxide particles were mixed with the spherical amorphous silica particles (average particle size d50: 3.5 μm), they were filled in an alumina container and heat treated in an air atmosphere (atmospheric pressure) using an electric furnace SUPER-BURN (produced by Motoyama Co., Ltd.). The amount of calcium hydroxide mixed was set to 0.9% by mass in terms of oxide conversion relative to the total mass of the spherical amorphous silica and the mass obtained by converting calcium into oxide. The temperature was raised to 1080°C at a rate of 300°C / hour and maintained for 24 hours. Then, the temperature was cooled to room temperature at a rate of about 100°C / hour. By performing atmospheric heat treatment, a silica powder containing crystalline silica was obtained. The silica powder was filled in an alumina crucible and reheated in an electric furnace with a silicon carbon rod heating element having a water vapor foaming device. The temperature increase rate was set to 250°C / hour. When the temperature in the furnace reaches 100°C, air containing water vapor is flowed into the furnace through the water vapor foaming device. The temperature reached in the furnace is set to 500°C (Example 1), 700°C (Examples 2, 5, 6), 750°C (Example 3), 800°C (Example 4), and the holding time at the reached temperature is set to 24 hours (Examples 1 to 5) and 6 hours (Example 6). The water vapor content in the air introduced into the furnace is set to 50% (Examples 1 to 4, Example 6) and 10% (Example 5). The cooling rate is about 100°C / hour, and it is cooled to room temperature. Air containing water vapor is introduced into the furnace until it is cooled to room temperature.

[0094] (Example 7, Example 8)

[0095] Amorphous silica particles were produced by melt-blowing. The spherical amorphous silica particles (average particle size d50: 10.4 μm) were obtained. As for the crystallization promoting material, it was not added, but filled in an alumina container, and heat-treated in an air atmosphere (atmospheric pressure) using an electric furnace SUPER-BURN (produced by Motoyama Co., Ltd.). The heating rate was 300°C / hour, the temperature was raised to 1300°C, and maintained for 24 hours. Then, the cooling rate was about 100°C / hour, and it was cooled to room temperature. By performing atmospheric heat treatment, a silica powder containing crystalline silica was obtained. The silica powder was filled in an alumina crucible and heated in an electric furnace with a silicon carbon rod heating element having a water vapor foaming device. The heating rate was set to 250°C / hour. When the temperature in the furnace reached 100°C, air gas containing water vapor was flowed into the furnace through the water vapor foaming device. The furnace reached a temperature of 700°C (Example 7) and 800°C (Example 8), and the holding time at the reached temperature was set to 24 hours. The water vapor content in the air gas introduced into the furnace was set to 50%. The temperature was lowered at a rate of about 100°C / hour until it was cooled to room temperature. The air containing water vapor was introduced into the furnace until it was cooled to room temperature.

[0096] (Example 9 to Example 12)

[0097] Amorphous silica particles were prepared by melt blowing. Calcium hydroxide particles and lithium carbonate particles were mixed with the spherical amorphous silica particles (average particle size d50: 15.4 μm). Relative to the total mass of the mass of the spherical amorphous silica and the mass obtained by converting calcium into oxide and lithium into oxide, 0.6% by mass of lithium carbonate particles and 0.05% by mass of lithium carbonate particles were mixed in terms of oxide. The heating rate was 300°C / hour, and the temperature was increased to 1050°C (Example 9), 1100°C (Example 10), 1150°C (Example 11), and 1230°C (Example 12), and maintained for 24 hours. Then, it was cooled to room temperature at a heating rate of 100°C / hour. By performing atmospheric heat treatment, a silica powder containing crystalline silica was obtained. The silica powder was filled in an alumina crucible and reheated in an electric furnace with a silicon carbon rod heating element having a water vapor foaming device. The heating rate was set at 250°C / hour. When the temperature in the furnace reached 100°C, air gas containing water vapor was introduced into the furnace through a water vapor foaming device. The temperature reached in the furnace was 750°C (Example 9) and 700°C (Examples 10 to 12), and the holding time was set to 24 hours. At a cooling rate of about 100°C / hour, it was cooled to room temperature. Air containing water vapor was introduced into the furnace until it was cooled to room temperature.

[0098] (Example 13)

[0099] Amorphous silica particles were produced by melt-blowing. In the spraying, a powder obtained by mixing crushed silica and calcium hydroxide was sprayed. The mixed powder is a powder as follows: 0.80 mass% of calcium is mixed in terms of oxide conversion relative to the total mass of the mass of crushed silica and the mass obtained by converting calcium into oxide. The average particle size d50 of the spherical amorphous silica particles obtained by spraying is 39.0 μm. The powder was filled in a container made of BN and heat-treated with a hot isostatic pressing (HIP: Hot Isostatic Pressing) device to obtain a silica powder containing crystalline silica. The atmospheric gas was nitrogen, the pressure was 196 MPa, the reaching temperature was set to 1250°C, and the holding time was set to 24 hours. The obtained silica powder containing crystalline silica was filled in an alumina crucible and reheated in an electric furnace with a silicon carbon rod heating element having a water vapor foaming device. The heating rate was set to 250°C / hour. When the temperature in the furnace reaches 100°C, air containing water vapor is introduced into the furnace through the water vapor foaming device. The furnace reaches a temperature of 700°C and the holding time is set to 24 hours. It is cooled to room temperature at a cooling rate of about 100°C / hour. Air containing water vapor is introduced into the furnace until it is cooled to room temperature.

[0100] (Comparative Example 1 to Comparative Example 3)

[0101] Amorphous silica particles were produced by melt blowing. After calcium hydroxide particles were mixed with the spherical amorphous silica particles (average particle size d50: 3.5 μm), they were filled in an alumina container and heat treated in an air atmosphere (atmospheric pressure) using an electric furnace SUPER-BURN (produced by Motoyama Co., Ltd.). The amount of calcium hydroxide mixed was set to 0.9% by mass in terms of oxide conversion relative to the total mass of the spherical amorphous silica and the mass obtained by converting calcium into oxide. The temperature was raised to 1080°C at a rate of 300°C / hour and maintained for 24 hours. Then, the temperature was cooled to room temperature at a rate of about 100°C / hour. By performing atmospheric heat treatment, a silica powder containing crystalline silica was obtained. The silica powder was filled in an alumina crucible and reheated in an electric furnace with a silicon carbon rod heating element having a water vapor foaming device. The temperature increase rate was set to 250°C / hour. When the temperature in the furnace reaches 100°C, air containing water vapor is flowed into the furnace through the water vapor foaming device. The temperature reached in the furnace is set to 400°C (Comparative Example 1), 860°C (Comparative Example 2), and 900°C (Comparative Example 3), and the holding time at the reached temperature is set to 24 hours. The water vapor content in the air introduced into the furnace is set to 50%. Cool to room temperature at a cooling rate of about 100°C / hour. Air containing water vapor is introduced into the furnace until it is cooled to room temperature.

[0102] (Comparative Example 4, Comparative Example 5)

[0103] Amorphous silica particles were produced by melt-blowing. The spherical amorphous silica particles (average particle size d50: 10.4 μm) were obtained. As for the crystallization promoting material, it was not added, but filled in an alumina container, and heat-treated in an air atmosphere (atmospheric pressure) using an electric furnace SUPER-BURN (produced by Motoyama Co., Ltd.). The heating rate was 300°C / hour, the temperature was raised to 1300°C, and maintained for 24 hours. Then, the cooling rate was about 100°C / hour, and it was cooled to room temperature. By performing atmospheric heat treatment, a silica powder containing crystalline silica was obtained. The silica powder was filled in an alumina crucible and heated in an electric furnace with a silicon carbon rod heating element having a water vapor foaming device. The heating rate was set to 250°C / hour. When the temperature in the furnace reached 100°C, air gas containing water vapor was flowed into the furnace through the water vapor foaming device. The furnace reached a temperature of 400°C (Comparative Example 4) and 900°C (Comparative Example 5), and the holding time at the reached temperature was set to 24 hours. The water vapor content in the air gas introduced into the furnace was set to 50%. The temperature was lowered at a rate of about 100°C / hour until it was cooled to room temperature. The air containing water vapor was introduced into the furnace until it was cooled to room temperature.

[0104] (Reference Example 1 to Reference Example 4)

[0105] Amorphous silica particles were produced by melt-blowing. The average particle diameters of the spherical amorphous silica particles were d50: 2.2 μm (reference 1), d50: 10.2 μm (reference 2), d50: 15.2 μm (reference 3), and d50: 37.0 μm (reference 4).

[0106] The ratio of amorphous and crystalline silica in the silica particles obtained by heat treatment (Examples 1 to 13 and Comparative Examples 1 to 4), as well as the type of crystalline silica and its ratio were determined by XRD. In the present invention, an X-ray diffraction device "D2PHASER" (manufactured by Bruker) was used. Quantitative analysis of the crystalline phase based on the Litwald method was performed using the crystal structure analysis software "TOPAS" (manufactured by Bruker).

[0107] The circularity is determined by flow particle image analysis. In the present invention, a flow particle image analyzer "FPIA-3000" (manufactured by Spectris Corporation) is used.

[0108] The average particle size (D50) of the spherical quartz particles is measured by a laser diffraction / scattering particle size distribution measuring method. In the present invention, a laser diffraction / scattering particle size distribution measuring apparatus "CILAS920" (manufactured by CILAS) is used.

[0109] (Temperature-rising gas analysis)

[0110] The amount of water released when the silica particles are heated is analyzed by temperature desorption gas analysis. Temperature desorption gas analysis is a mass spectrometry method that can monitor the gas generated when heating / heating in a high vacuum for each temperature. The temperature desorption gas analysis device used is the TDS1200 manufactured by Electronic Science Co., Ltd. After the silica powder sample is placed in a quartz sample holder, it is placed on a sample stand and placed under high vacuum (10 -7Pa) was heated from the bottom of the table by a halogen lamp. In the temperature-increasing desorption gas analyzer manufactured by Electronic Science Co., Ltd., there are two types of thermocouples: one inserted into the sample table and the other arranged above the sample table. Heating control is performed using the sample table thermocouple. In addition, the sample temperature is measured using a thermocouple (W-Re) arranged on the top of the table, and the tip of the thermocouple is brought into contact with the bottom of the quartz rack. The amount of released gas from the quartz boat was measured in advance (blank measurement). For the gas generated by heating, the ion current intensity of m / z 18 obtained by the quadrupole mass analyzer was accumulated, and the moisture content was calculated using the TDS1200 analysis software (TDS data processing application Ver5.2.0.5). The moisture content was quantified from room temperature to 1000°C. Since the amount of water derived from the dehydration condensation of the silanol groups on the surface of silica is released by heating at 800°C or higher, the amount of water released at 800°C to 1000°C was calculated.

[0111] (Amount of moisture released per unit area)

[0112] The surface area per unit weight can be determined by measuring the specific surface area based on BET. Furthermore, the amount of released water per weight can be quantified by temperature-elevated desorption gas analysis, so the amount of released water per unit area (μg / m 2 ).

[0113] The spherical crystalline silica particles obtained in the examples of the present invention all had a circularity of 0.80 or more, contained 50.0% or more of the whole crystalline silica, and the amount of water released when heated from 800°C to 1000°C by a temperature-elevated desorption gas analyzer (after heat treatment in a water vapor atmosphere) was 4.5 μg / m 2 Furthermore, the ratio of quartz or cristobalite to the crystalline silicon dioxide is 80.0% by mass or more.

[0114] Regarding the average particle size, the spherical amorphous silica particles were 3.5 μm, while the spherical crystalline silica particles (Examples 1 to 6) of the present invention using the raw material were 3.4 μm to 3.6 μm. In addition, the average particle size of the spherical amorphous silica particles was 10.4 μm, while the spherical crystalline silica particles (Examples 7 to 8) of the present invention using the raw material were 10.3 μm and 10.4 μm.

[0115] Furthermore, the spherical amorphous silica particles had a diameter of 15.4 μm, whereas the spherical crystalline silica particles of the present invention (Examples 9 to 12) using the raw material had a diameter of 15.2 μm to 15.6 μm.

[0116] Furthermore, the average particle size of the spherical amorphous silica particles was 39.0 μm, whereas the average particle size of the spherical crystalline silica particles of the present invention (Example 13) using the mixed raw material powder was 39.5 μm.

[0117] By comparing Examples 1 to 4 with Comparative Examples 1 to 3, it can be seen that after the spherical amorphous silica particles having a circularity of 0.80 or more are heat-treated at a temperature of 900° C. to 1550° C. to crystallize them, they are heat-treated in an atmosphere containing water vapor at a temperature range of 450° C. to 830° C., and the amount of water released when heated from 800° C. to 1000° C. by a temperature-increasing desorption gas analysis device (after the water vapor atmosphere heat treatment) becomes 4.5 μg / m 2 In Comparative Example 1, the heat treatment temperature in the water vapor atmosphere was 400°C, and in Comparative Examples 2 and 3, it was 860°C and 900°C, respectively. However, when the temperature was lower than 450°C or higher than 830°C, the moisture content (after the water vapor atmosphere heat treatment) did not increase compared to before the water vapor atmosphere, but became less than 4.5 μg / m 2 The proportion of crystalline silica in Examples 1 to 4 and Comparative Examples 1 to 3 was 77% of the total, and the proportion of quartz in the crystalline silica was 84.5%.

[0118] Comparing Example 2 with Example 5, even if the water vapor content is changed to 10% or 50% for the water vapor atmosphere of the water vapor atmosphere heat treatment, the spherical crystalline silica of the present invention can be obtained. In addition, comparing Example 2 with Example 6, it can be seen that the spherical crystalline silica of the present invention can be obtained when the treatment time of the water vapor atmosphere heat treatment is 24 hours or 6 hours.

[0119] By comparing Examples 7 to 8 with Comparative Examples 4 to 5, it can be seen that after the spherical amorphous silica particles having a circularity of 0.80 or more are heat-treated at a temperature of 1300° C. to be crystallized, the heat treatment is then performed in an atmosphere containing water vapor within a temperature range of 450° C. to 830° C., and the amount of water released when heated from 800° C. to 1000° C. by a temperature-increasing desorption gas analysis device (after the water vapor atmosphere heat treatment) becomes 4.5 μg / m 2 In Comparative Example 4, the heat treatment temperature in the water vapor atmosphere was 400°C, and in Comparative Example 5, it was 900°C. However, when the temperature was lower than 450°C or higher than 830°C, the moisture content (after the water vapor atmosphere heat treatment) did not increase compared to before the water vapor atmosphere, but became less than 4.5 μg / m 2 The proportion of crystalline silica in Examples 7 and 8 and Comparative Examples 4 and 5 was 90.2% of the total, and the proportion of cristobalite in the crystalline silica was 100%.

[0120] In Examples 9 to 13, the spherical crystalline silica of the present invention is obtained by changing the proportion of crystalline silica in the whole and the proportion of quartz or cristobalite in the crystalline silica. It is known that after the spherical amorphous silica particles with a circularity of 0.80 or more are heat-treated at a temperature of 1050 to 1250°C to crystallize, they are heat-treated in an atmosphere containing water vapor within a temperature range of 450°C to 830°C, whereby the amount of water released when heated from 800°C to 1000°C by a temperature-raising desorption gas analyzer (after heat treatment in a water vapor atmosphere) becomes 4.5 μg / m 2 above.

[0121] Spherical amorphous silica powders produced by a conventional flame fusion method are shown in Reference Examples 1 to 4. The moisture content detected in the desorbed gas analysis at 800°C to 1000°C was 7.4 to 27.9 μg / m 2 When the heat-treated silica powder used for crystallization of spherical crystalline silica described in Examples 1 to 13 was subjected to TDS analysis, the amount of moisture released in the temperature range of 800°C to 1000°C (before water vapor atmosphere treatment) was 0.0 to 3.5 μg / m 2 , lower than the moisture content of 4.5 μg / m 2 .

[0122]

Table 1

[0123] Table 1: Appendix (Examples and Comparative Examples)

[0124]

[0125] INDUSTRIAL APPLICABILITY The spherical crystalline silica particles of the present invention are not limited to semiconductor sealing materials, but can also be used for other purposes. Specifically, they can also be used as prepregs for printed circuit boards or various engineering plastics.

Claims

1. A spherical crystalline silica particle, characterized in that: The circularity is 0.80 or more, and the total amount of the crystalline silicon dioxide is 50.0% or more. When the crystalline silicon dioxide is heated from 800°C to 1000°C by a temperature-elevated desorption gas analyzer, the amount of water released is 4.5 μg / m 2 above.

2. The spherical crystalline silica particles according to claim 1, characterized in that The water content is 7.0 μg / m 2 above.

3. The spherical crystalline silica particles according to claim 1 or 2, wherein The ratio of quartz or cristobalite to the crystalline silicon dioxide is 80.0% by mass or more.

4. The spherical crystalline silica particles according to any one of claims 1 to 3, wherein The crystalline silicon dioxide accounts for 75.0% or more of the whole.

5. The spherical crystalline silica particles according to any one of claims 1 to 4, characterized in that The water content is 50.0 μg / m 2 the following.

6. A method for producing spherical crystalline silica particles, the method for producing spherical crystalline silica particles according to any one of claims 1 to 5, comprising: The spherical amorphous silica particles are heat treated at a temperature of 900° C. to 1550° C. to be crystallized, and then heat treated at a temperature of 450° C. to 830° C. in an atmosphere containing water vapor.

7. A resin composite composition, characterized in that: The spherical crystalline silica particles according to any one of claims 1 to 5 are contained in a resin.

8. A resin composite, characterized in that: The resin composite composition according to claim 7 is cured.

Citation Information

Patent Citations

  • Spherical crystalline silica particles and method for producing same

    CN110636989A

  • Spherical crystalline silica particles, spherical silica particle mixture, and composite material

    CN113905984A