Adhesive composition for wet friction material and wet friction plate
By adding carboxylic acid with 1 to 6 carbon atoms to the adhesive of the wet friction material, combining the A-order phenolic resin and polyvinyl butyral, the adhesive for wet friction material at high temperature is solved. The problem of lower bonding strength decreases, high heat resistance and excellent bonding performance are achieved, while avoiding environmental pollution.
Patent Information
- Application Number
- CN202380030268.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-04-05
- Filing Date
- 2023-04-05
- Publication Date
- 2024-11-12
AI Technical Summary
The problem of the existing bonding strength of the wet friction materials deteriorates at high temperatures, making it difficult to meet the ever-increasing bonding strength and heat resistance requirements.
The phenolic resin is added with carboxylic acids with 1 to 6 carbon atoms and an alcohol-based solvent to form a carboxylic acids with 1 to 6 carbon atoms and an alcohol-based solvent to form a phenolic resin, a phenolic resin, a phenolic butyral resin, a carboxylic acids with 1 to 6 carbon atoms and 6 to form a carboxylic acids with 1 to 6 carbon atoms and 6 to form a The adhesive composition of solvent avoids the use of substances with high environmental burden such as nickel and cobalt.
The adhesive composition for wet friction materials with excellent bonding strength and high heat resistance is achieved, ensuring the stability of bonding strength at high temperatures and reducing the risk of environmental pollution.
Smart Images

Figure BDA0005059140680000101
Abstract
Description
Technical Field
[0001] The present invention relates to an adhesive composition for a wet friction material and a wet friction plate. Background Art
[0002] In the automatic transmission of automobiles, a clutch is installed between the engine and the transmission in order to transmit the engine force to the transmission or cut off the engine force when starting, stopping, or changing speed. In order to make the clutch function properly, a friction material is used, and the friction material is generally divided into "wet friction material" using oil and "dry friction material" not using oil. Wet friction material can suppress the rise of friction heat by using oil. Wet friction material can be manufactured by applying an adhesive on a metal called a core plate and bonding it with a friction component composed of phenolic resin or the like.
[0003] As an adhesive used in manufacturing friction materials such as clutches and brakes, a resol type phenolic resin is generally used as a resin material having excellent mechanical properties, electrical properties, and adhesiveness. Therefore, various studies have been conducted on resol type phenolic resins in order to improve the friction properties and wear resistance of the obtained wet friction material and to improve curing properties such as adhesive strength.
[0004] Examples of resol-type phenolic resins used in wet friction materials include those described in Patent Documents 1 and 2. Patent Document 1 discloses an adhesive composition as an adhesive for a friction material having a short curing time and high heat resistance, the adhesive composition comprising a resol-type phenolic resin, a polyvinyl butyral resin, nickel acetate or cobalt acetate as a polyvalent metal salt, and a metal salt of nitrous acid or an ester of nitrous acid.
[0005] Patent Document 2 discloses an adhesive for a wet friction plate that exhibits excellent bonding strength and contains a resol-type phenolic resin and a nitrate or nitric acid.
[0006] Prior art literature
[0007] Patent Literature
[0008] Patent Document 1: Japanese Patent Application Publication No. 2014-24881
[0009] Patent Document 2: Japanese Patent Application Publication No. 2006-83892 Summary of the invention
[0010] Technical problem to be solved by the invention
[0011] In recent years, the requirements for adhesives for wet friction materials have been increasing. The present invention has been developed in response to these requirements and provides an adhesive composition for wet friction materials having excellent adhesive strength and heat resistance (suppressing the decrease in adhesive strength at high temperatures).
[0012] Means for solving technical problems
[0013] The present inventors have found that by adding a carboxylic acid having 1 to 6 carbon atoms to a resin composition containing a phenolic resin, an adhesive having excellent adhesive force and heat resistance (suppression of a decrease in adhesive strength at high temperatures) and suitable for use in wet friction materials can be obtained, thereby completing the present invention.
[0014] According to the present invention, there are provided the adhesive composition for a wet friction material and the wet friction plate shown below.
[0015] [1] An adhesive composition for a wet friction material, comprising a resol-type phenolic resin, polyvinyl butyral, a carboxylic acid having 1 to 6 carbon atoms, and an alcohol solvent.
[0016] [2] The adhesive composition for a wet friction material according to item [1], wherein the content of the carboxylic acid having 1 to 6 carbon atoms is 0.1% by mass to 10% by mass based on the solid content of the adhesive composition for a wet friction material.
[0017] [3] The adhesive composition for a wet friction material according to item [1] or [2], wherein the carboxylic acid having 1 to 6 carbon atoms includes acetic acid.
[0018] [4] The adhesive composition for a wet friction material according to any one of items [1] to [3], wherein the alcohol solvent comprises at least one selected from the group consisting of methanol, ethanol, 1-propanol, 2-propanol, n-butanol, isobutanol, sec-butanol, and tert-butanol.
[0019] [5] The adhesive composition for a wet friction material according to any one of items [1] to [4], which does not substantially contain nickel.
[0020] [6] The adhesive composition for a wet friction material according to any one of items [1] to [5], which does not substantially contain cobalt.
[0021] [7] The adhesive composition for a wet friction material according to any one of items [1] to [6], wherein the methanol resistance at 25° C. is 1000% or more.
[0022] [8] A wet friction plate comprising: a metal substrate; and a friction material bonded to the metal substrate via the adhesive composition for a wet friction material according to any one of items [1] to [7].
[0023] Effects of the Invention
[0024] According to the present invention, there can be provided an adhesive composition for a wet friction material having excellent bonding strength and high heat resistance, and a wet friction plate produced using the composition. DETAILED DESCRIPTION
[0025] Hereinafter, embodiments of the present invention will be described.
[0026] [Adhesive composition for wet friction material]
[0027] The adhesive composition for wet friction material of the present embodiment (hereinafter also referred to as "adhesive composition") contains a resol-type phenolic resin, polyvinyl butyral, a carboxylic acid having 1 to 6 carbon atoms, and an alcohol solvent. Each component is described below.
[0028] (Resol type phenolic resin)
[0029] The resol type phenolic resin used in the adhesive composition of the present embodiment is a resol type phenolic resin obtained by reacting a phenolic resin and an aldehyde in the presence of a basic catalyst.
[0030] Examples of the phenols used for synthesizing the resol-type phenolic resin used in the present embodiment include phenol; cresols such as o-cresol, m-cresol, and p-cresol; ethylphenols such as o-ethylphenol, m-ethylphenol, and p-ethylphenol; butylphenols such as isopropylphenol, butylphenol, and p-tert-butylphenol; alkylphenols such as p-tert-amylphenol, p-octylphenol, p-nonylphenol, and p-cumylphenol; halogenated phenols such as fluorophenol, chlorophenol, bromophenol, and iodinephenol; monophenol substituted products such as p-phenylphenol, aminophenol, nitrophenol, dinitrophenol, and trinitrophenol; monophenols such as 1-naphthol and 2-naphthol; and polyphenols such as resorcinol, alkylresorcinol, pyrogallol, catechol, alkylpyrocatechol, hydroquinone, alkylhydroquinone, pyrogallol, bisphenol A, bisphenol F, bisphenol S, and dihydroxynaphthalene. These can be used alone or in combination of two or more.
[0031] As the aldehydes used for synthesizing the resol type phenolic resin used in this embodiment, formaldehyde, paraformaldehyde, trioxane, acetaldehyde, propionaldehyde, polyoxymethylene, trichloroacetaldehyde, hexamethylenetetramine, furfural, glyoxal, n-butyraldehyde, hexanal, allyl aldehyde, benzaldehyde, crotonaldehyde, acrolein, tetracarboxaldehyde, phenylacetaldehyde, o-tolualdehyde, salicylaldehyde etc. can be enumerated. These can be used alone, or two or more can be used in combination. In addition, the precursor of these aldehydes or the solution of these aldehydes can also be used. Wherein, from the viewpoint of manufacturing cost, preferably formaldehyde solution is used.
[0032] Examples of the alkaline catalyst used for synthesizing the resol type phenolic resin used in the present embodiment include hydroxides of alkali metals or alkaline earth metals such as sodium hydroxide, potassium hydroxide, and calcium hydroxide; carbonates such as sodium carbonate and calcium carbonate; oxides such as lime; sulfites such as sodium sulfite; phosphates such as sodium phosphate; amines such as ammonia, trimethylamine, triethylamine, monoethanolamine, diethanolamine, triethanolamine, hexamethylenetetramine, and pyridine, and the like.
[0033] The reaction solvent used for synthesizing the resol type phenolic resin used in the present embodiment is generally water, but an organic solvent may also be used. Specific examples of such organic solvents include alcohols, ketones, aromatics, etc. Furthermore, specific examples of alcohols include methanol, ethanol, propanol, ethylene glycol, diethylene glycol, triethylene glycol, glycerol, etc. Specific examples of ketones include acetone, methyl ethyl ketone, etc. Specific examples of aromatics include toluene, xylene, etc.
[0034] Examples of the form of the resol type phenolic resin include a solid, an aqueous solution, a solvent solution, and an aqueous dispersion. Among them, a solution dissolved in a solvent such as methanol, ethanol, methyl ethyl ketone, and acetone is preferred from the viewpoint of good handleability.
[0035] The resol type phenolic resin used in the adhesive composition of the present embodiment preferably has a weight average molecular weight of 1000 to 3000, and more preferably has a weight average molecular weight of 1200 to 2000. The resol type phenolic resin having a weight average molecular weight within the above range can have both excellent adhesiveness and solvent solubility. As a result, the adhesive composition containing such a resol type phenolic resin has excellent adhesiveness and can have excellent coating or handling properties.
[0036] In the resol type phenolic resin used in the present embodiment, the amount of free phenol contained therein is preferably less than 5.0 mass % relative to the overall resol type phenolic resin, and more preferably less than 4.0 mass %. The lower limit of the amount of free phenol contained in the resol type phenolic resin is not particularly limited, but is, for example, more than 0.1 mass %, preferably more than 0.5 mass % relative to the overall resol type phenolic resin. By making the amount of free phenol below the above upper limit, the resol type phenolic resin has excellent storage stability. In addition, by making the amount of free phenol above the above lower limit, there is no need for a special device or process for completely removing free aldehydes, so the manufacturing cost can be suppressed.
[0037] The resol type phenolic resin used in the present embodiment can be obtained by adding phenols (P) and aldehydes (F) in a ratio of 1.5 or more, preferably 1.5 or more and 2.0 or less, and more preferably 1.6 or more and 1.9 or less to a reactor, further adding the above-mentioned alkaline catalyst as a polymerization catalyst, and refluxing for a suitable time (for example, 3 to 6 hours). When the molar ratio (F / P) of phenols (P) and aldehydes (F) is less than 1.5, the weight average molecular weight of the generated resol type phenolic resin is sometimes less than 1000. In addition, when the molar ratio (F / P) of phenols (P) and aldehydes (F) is greater than 2.0, the gelation of the resin is easy to proceed during the reaction, so the reaction efficiency will decrease, and a high molecular weight resol type phenolic resin with a weight average molecular weight greater than 3000 will be generated, which is not preferred. The reaction temperature is, for example, 40°C to 120°C, preferably 60°C to 100°C. Thereby, gelation can be suppressed and a resol-type phenolic resin having a target molecular weight can be obtained.
[0038] (Polyvinyl butyral)
[0039] The polyvinyl butyral used in the adhesive composition of the present embodiment is an elastomer obtained by butyralizing polyvinyl alcohol with butyraldehyde in the presence of an acid catalyst. The weight average molecular weight of the polyvinyl butyral is not particularly limited, but is preferably 1.0×10 4 ~1.0×10 5 , more preferably 2.0×10 4 ~8.0×10 4 , and more preferably 3.3×10 4 ~5.5×10 4 In addition, the weight average molecular weight refers to the molecular weight based on polystyrene conversion measured by gel permeation chromatography (GPC).
[0040] The degree of polymerization of polyvinyl butyral is preferably 200 to 3000. By using polyvinyl butyral having a degree of polymerization of 200 or more, the obtained adhesive composition has a sufficient bonding strength for use as a friction material, and by using polyvinyl butyral having a degree of polymerization of 3000 or less, the viscosity of the obtained adhesive composition when melted can be suppressed to a low level, thereby improving the handling properties when applied to a metal substrate, and enabling the metal substrate and the friction material to be firmly bonded.
[0041] The content of polyvinyl butyral is preferably 1 part by weight or more and 50 parts by weight or less, and more preferably 5 parts by weight or more and 30 parts by weight or less, relative to 100 parts by weight of the resol-type phenolic resin. When the content of polyvinyl butyral is equal to or greater than the lower limit, the adhesive composition obtained has sufficient bonding strength for use as a friction material, and when the content of polyvinyl butyral is equal to or less than the upper limit, the viscosity of the adhesive composition when melted can be suppressed to a low level, thereby improving coating properties and handling properties.
[0042] (Carboxylic acid having 1 to 6 carbon atoms)
[0043] The adhesive composition of the present embodiment includes a carboxylic acid having a carbon number of 1 to 6. As the carboxylic acid having a carbon number of 1 to 6, formic acid, acetic acid, propionic acid, valeric acid, etc. can be cited. These can be used alone or in combination of two or more. Among them, acetic acid is preferably used from the viewpoint of improvement of the bonding strength of the obtained adhesive composition, handleability and ease of acquisition. By including the above-mentioned carboxylic acid, an adhesive composition with further improved bonding strength can be obtained.
[0044] The content of the carboxylic acid in the adhesive composition is preferably 0.1% by mass to 10% by mass, more preferably 1% by mass to 10% by mass, and more preferably 2% by mass to 10% by mass, relative to the total solid content of the composition. By making the content of the iron salt within the above range, the obtained adhesive composition has sufficient bonding strength for use as a friction material and has excellent heat resistance (suppressing the decrease in bonding strength at high temperatures).
[0045] The adhesive composition of the embodiment substantially does not contain substances with high environmental burdens, such as nickel or cobalt, which are used in conventional adhesives to improve adhesion. The adhesive composition of the embodiment does not contain these substances with high environmental burdens in the abrasive powder generated during braking of the friction plate manufactured using the adhesive composition, so there is no concern about environmental pollution. Furthermore, the adhesive composition of the embodiment can have high adhesion and heat resistance (suppressing the decrease in bonding strength at high temperatures) by containing iron salts even if it does not contain nickel or cobalt.
[0046] (Alcohol solvent)
[0047] The adhesive composition of the present embodiment can be provided in the form of a liquid in which the above-mentioned components are dissolved or dispersed in an alcoholic solvent. Alcohols used as solvents for the adhesive composition of the present embodiment include methanol, ethanol, 1-propanol, 2-propanol, n-butanol, isobutanol, sec-butanol, and tert-butanol. These can be used alone or in combination of two or more. Among them, methanol is preferably used from the viewpoint of the simplicity of handling.
[0048] (Iron Salt)
[0049] The adhesive composition of the present embodiment may include an iron salt. As the iron salt, a divalent iron salt or a trivalent iron salt may be mentioned. Preferably, the iron salt is a sulfate such as iron (II) sulfate or iron (III) sulfate. As specific examples of sulfates, iron (II) sulfate, iron (II) sulfate 7 hydrate, and iron (III) sulfate ammonium may be mentioned. These may be used alone or in combination of two or more.
[0050] When an iron salt is used, its content is preferably 0.1% by mass to 10% by mass, more preferably 0.5% by mass to 8% by mass, and more preferably 0.8% by mass to 6% by mass, relative to the total solid content of the composition. By making the content of the iron salt within the above range, the obtained adhesive composition has sufficient bonding strength for use as a friction material and has excellent heat resistance (suppressing the decrease in bonding strength at high temperatures).
[0051] (Other ingredients)
[0052] The adhesive composition of this embodiment may contain, in addition to the above-mentioned components, elastomers such as nitrile rubber and styrene butadiene rubber, surfactants, flame retardants, antioxidants, colorants, silane coupling agents and other additives within the range that does not impair the effects of the present invention.
[0053] (Manufacture of Adhesive Composition)
[0054] The adhesive composition of the present embodiment can be obtained by mixing the above-mentioned components in the above-mentioned alcohol solvent using a known method.
[0055] The adhesive composition of the present embodiment has excellent adhesiveness and heat resistance by including the above-mentioned components, and has excellent solvent solubility. The adhesive composition of the present embodiment has a methanol tolerance (25°C) of 1000% or more, which is an indicator of solubility. Therefore, the operability and coating properties during use are excellent. In addition, the higher the value of methanol tolerance, the higher the solubility in methanol. In the use of adhesives for wet friction materials, 100% or more is required.
[0056] In addition, methanol resistance can be measured in the following manner.
[0057] First, 10 ml of the adhesive composition was measured in a 500 ml graduated cylinder, and methanol was slowly added while stirring at 25° C. The amount (volume) of methanol added when the mixed solution of the adhesive composition and methanol became cloudy was calculated by the following formula.
[0058] Methanol tolerance (%) = (methanol addition amount (ml) / adhesive composition 10ml) × 100
[0059] The viscosity of the adhesive composition of the present embodiment is, for example, 300 mPa to 10000 mPa, preferably 450 mPa to 8000 mPa, and more preferably 600 mPa to 6000 mPa. An adhesive composition having a viscosity within such a range has high bonding strength and is excellent in workability and coating properties.
[0060] The viscosity can be measured according to JIS Z8803 using an E-type viscometer (manufactured by TOKI SANGYO CO., LTD.).
[0061] [Wet friction plate]
[0062] The adhesive composition of the present embodiment can be suitably used for manufacturing a wet friction plate. A wet friction plate can be manufactured by bonding a metal substrate (steel plate) and a friction plate using the adhesive composition of the present embodiment. More specifically, a wet friction plate can be manufactured by coating the adhesive composition of the present embodiment on a metal substrate, and arranging a friction material on the surface of the metal substrate coated with the adhesive composition and bonding them. The adhesive composition of the present embodiment is excellent in coating properties and workability, so the above steps can be smoothly carried out. In addition, the wet friction plate obtained in this way has excellent strength because the friction plate and the metal substrate are firmly bonded.
[0063] As mentioned above, although embodiment of this invention was described, these are illustrations of this invention, and various structures other than the above-mentioned can also be adopted.
[0064] Example
[0065] Hereinafter, the present invention will be described with reference to Examples and Comparative Examples, but the present invention is not limited thereto.
[0066] [Preparation of Adhesive Composition]
[0067] (Example 1)
[0068] In a reaction apparatus equipped with a stirring device, a reflux cooler and a thermometer, 100 parts by weight of phenol, 151 parts by weight of a 37% formalin aqueous solution (F / P molar ratio = 1.7), and 5 parts by weight of triethylamine were added, and reacted for 40 minutes under reflux conditions. Thereafter, while dehydrating under a reduced pressure of 91 kPa, 40 parts by weight of methanol was added when the temperature in the system reached 70°C, and reacted at 80°C for 2 hours to obtain a resol type phenolic resin with a weight average molecular weight of 1382. 120 parts by weight of methanol, 30 parts by weight of a polyvinyl butyral resin, and 4.5 parts by weight of acetic acid were added thereto, dissolved and mixed, to obtain an adhesive composition with 1.5% free phenol and 50% non-volatile components.
[0069] (Example 2)
[0070] An adhesive composition was obtained in the same manner as in Example 1 except that the amount of acetic acid added was changed to 9.0 parts by weight.
[0071] (Example 3)
[0072] An adhesive composition was obtained in the same manner as in Example 1 except that 1.5 parts by weight of iron (II) sulfate was added in addition to 4.5 parts by weight of acetic acid.
[0073] (Comparative Example 1)
[0074] In a reaction apparatus equipped with a stirring device, a reflux cooler and a thermometer, 100 parts by weight of phenol, 151 parts by weight of a 37% formalin aqueous solution (F / P molar ratio = 1.7), and 5 parts by weight of triethylamine were added and reacted under reflux conditions for 40 minutes. Thereafter, while dehydrating under reduced pressure conditions of 91 kPa, 40 parts by weight of methanol was added when the temperature in the system reached 70°C, and the reaction was carried out at 80°C for 2 hours to obtain a resol type phenolic resin with a weight average molecular weight of 1382. 120 parts by weight of methanol and 30 parts by weight of polyvinyl butyral resin were added thereto, dissolved and mixed, to obtain a wet friction material adhesive composition having a free phenol content of 1.5% and a non-volatile component content of 50%.
[0075] (Comparative Example 2)
[0076] In a reaction apparatus equipped with a stirring device, a reflux cooler and a thermometer, 100 parts by weight of phenol, 117 parts by weight of a 37% formalin aqueous solution (F / P molar ratio = 1.2), and 4 parts by weight of a 30% ammonia aqueous solution were added, and reacted for 40 minutes under reflux conditions. Thereafter, while dehydrating under a reduced pressure of 91 kPa, 20 parts by weight of methanol was added when the temperature in the system reached 70°C, and reacted at 80°C for 1 hour. Next, 80 parts by weight of methanol was added to obtain a resol type phenolic resin having a non-volatile content of 50%.
[0077] 100 parts by weight of the obtained resol-type phenolic resin, 12 parts by weight of a polyvinyl butyral resin, and 12 parts by weight of methanol were dissolved and mixed to obtain an adhesive composition.
[0078] (Comparative Example 3)
[0079] In a reaction apparatus equipped with a stirring device, a reflux cooler and a thermometer, 100 parts by weight of phenol, 117 parts by weight of a 37% formalin aqueous solution (F / P molar ratio = 1.2), and 4 parts by weight of a 30% ammonia aqueous solution were added, and reacted for 40 minutes under reflux conditions. Thereafter, while dehydrating under a reduced pressure of 91 kPa, 20 parts by weight of methanol was added when the temperature in the system reached 70°C, and reacted at 80°C for 1 hour. Next, 80 parts by weight of methanol was added to obtain a resol type phenolic resin having a non-volatile content of 50%.
[0080] 100 parts by weight of the obtained resol-type phenolic resin, 13 parts by weight of polyvinyl butyral resin, 2 parts by weight of resorcinol, and 15 parts by weight of methanol were dissolved and mixed to obtain an adhesive composition containing 3% by weight of resorcinol based on the total solid content.
[0081] [evaluate]
[0082] The following physical properties of the adhesive compositions obtained in Examples 1 to 3 and Comparative Examples 1 to 3 were measured to evaluate their performance.
[0083] (Solvent solubility)
[0084] The solvent solubility was evaluated by measuring the methanol resistance. A larger value of the methanol resistance indicates that the resin composition has higher solubility in methanol.
[0085] Measurement of methanol resistance: First, 10 ml of the adhesive composition was measured in a 500 ml graduated cylinder, and methanol was slowly added while being stirred at 25°C. The amount of methanol added (volume) at the time when the mixed solution of the adhesive composition and methanol became turbid was calculated by the following formula. The results are shown in Table 1.
[0086] Methanol tolerance (%) = (methanol addition amount (ml) / adhesive composition 10ml) × 100
[0087] (Viscosity)
[0088] Measurement of viscosity: The viscosity of the adhesive composition was measured using an E-type viscometer (manufactured by Toki Sangyo Co., Ltd.) in accordance with JIS Z8803. The results are shown in Table 1.
[0089] (Adhesion Strength)
[0090] The adhesive strength of the adhesive composition was evaluated by measuring the non-peeled area ratio when bonding at 250° C. and the non-peeled area ratio when bonding at 300° C. A larger non-peeled area ratio indicates a higher adhesive strength.
[0091] Determination of non-peeling area ratio (bonding temperature 250°C): The above-mentioned adhesive composition was applied to an acid-washed steel plate, and the impregnated paper prepared by impregnating the phenolic resin in an aramid substrate and curing it was bonded under hot pressing (250°C, 10 MPa). The area of the bonding surface that was not peeled when bent at 90°C was measured, and the ratio (%) to the bonding area before bending was calculated. The results are shown in Table 1.
[0092] Determination of non-peeling area ratio (bonding temperature 300°C): The above-mentioned adhesive composition was applied to an acid-washed steel plate, and the impregnated paper prepared by impregnating the phenolic resin in an aramid substrate and curing it was bonded under hot pressing (300°C, 10MPa). The area of the bonding surface that was not peeled when bent at 90°C was measured, and the ratio (%) to the bonding area before bending was calculated. The results are shown in Table 1.
[0093] Table 1
[0094]
[0095] The adhesive composition of the example had high bonding strength both when bonding was performed at a temperature of 250°C and when bonding was performed at a temperature of 300°C.
[0096] This application claims priority based on Japanese patent application No. 2022-062802, filed on April 5, 2022, and all the disclosed contents are incorporated herein by reference.
Claims
1. An adhesive composition for a wet friction material, characterized in that: Include: Resol type phenolic resin; Polyvinyl butyral; A carboxylic acid having 1 to 6 carbon atoms; and Alcohol solvent.
2. The adhesive composition for wet friction material according to claim 1, characterized in that: The content of the carboxylic acid having 1 to 6 carbon atoms is 0.1% to 10% by mass based on the solid content of the adhesive composition for a wet friction material.
3. The adhesive composition for wet friction material according to claim 1 or 2, characterized in that: The carboxylic acid having 1 to 6 carbon atoms includes acetic acid.
4. The adhesive composition for wet friction material according to any one of claims 1 to 3, characterized in that: The alcohol solvent includes at least one selected from the group consisting of methanol, ethanol, 1-propanol, 2-propanol, n-butanol, isobutanol, sec-butanol, and tert-butanol.
5. The adhesive composition for wet friction material according to any one of claims 1 to 4, characterized in that: Contains substantially no nickel.
6. The adhesive composition for wet friction material according to any one of claims 1 to 5, characterized in that: Contains substantially no cobalt.
7. The adhesive composition for a wet friction material according to any one of claims 1 to 6, characterized in that: The methanol tolerance at 25°C is over 1000%.
8. A wet friction plate, characterized in that: include: Metal substrate; and A friction material bonded to the metal substrate via the adhesive composition for wet friction materials according to any one of claims 1 to 7.