Window material and translucent roof material
By using a temperature-sensitive non-crosslinked polymer and crosslinked particles in the window material, the white turbidity is adjusted according to the temperature, the problems of complex window structure and labor-consuming production in the prior art are solved, and the problem of the above-mentioned window structure is realized. Simple structure and efficient manufacturing window materials.
Patent Information
- Application Number
- CN202380029678.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-24
- Filing Date
- 2023-03-24
- Publication Date
- 2024-11-12
AI Technical Summary
The window structure of the existing temperature-sensitive dimming liquid laminate has a complex window structure, which takes time to manufacture, and requires a dedicated structure to maintain the shape, resulting in difficulty in setting up and maintaining.
Adhesive compositions containing temperature-sensitive non-crosslinked polymers and temperature-sensitive crosslinked particles are used to adjust the white turbidity of the window material through temperature changes, simplifying the structure and reducing manufacturing complexity.
It realizes window materials or translucent roof materials that automatically change the white turbidity according to temperature. It has a simple structure and easy manufacturing. It is suitable for buildings, vehicles, ships and aircraft.
Smart Images

Figure CN118946709A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a window material and a light-transmitting roof material and also to a building, a vehicle, a ship or an aircraft equipped with the window material and / or the light-transmitting roof material. Background Art
[0002] In buildings such as office buildings and arcades, or in vehicles such as vehicles, ships, and aircraft, there is a need to mitigate direct sunlight during high temperatures in summer and to take in sunlight during low temperatures in winter. In response to this, a temperature-sensitive dimming liquid laminate whose white turbidity changes autonomously in response to temperature stimulation has been proposed as a structure to be installed in a window (Patent Document 1).
[0003] Prior art literature
[0004] Patent Literature
[0005] Patent Document 1: Japanese Patent No. 3337810 Summary of the invention
[0006] Problem that the invention aims to solve
[0007] In order to provide the above-mentioned stacked body, a dedicated structure for maintaining the shape of the temperature-sensitive light-adjusting liquid is required, and there is a problem that the structure of the window provided with the above-mentioned stacked body becomes complicated, and the manufacturing process is labor-intensive.
[0008] The present invention has been completed in view of the above-mentioned problems, and its purpose is to provide a window material or a translucent roof material that can autonomously change the white turbidity according to the temperature, has a simple structure and is easy to manufacture, a building having the window material and / or the translucent roof material, and a vehicle, a ship or an aircraft.
[0009] Solutions for solving problems
[0010] A first aspect of the present invention is a window material, wherein:
[0011] It comprises at least one light-transmitting substrate layer and at least one adhesive layer,
[0012] The adhesive layer includes an adhesive composition containing 1 to 20 parts by mass of a temperature-sensitive non-crosslinked polymer and 1 to 100 parts by mass of temperature-sensitive crosslinked fine particles relative to 100 parts by mass of an adhesive.
[0013] The refractive index of the thermosensitive cross-linked microparticles decreases as the temperature increases, and
[0014] The amount of refractive index reduction per 1°C, that is, the refractive index reduction rate of the temperature-sensitive crosslinked fine particles is greater near the melting point of the temperature-sensitive crosslinked fine particles than in a temperature range other than near the melting point of the temperature-sensitive crosslinked fine particles.
[0015] The adhesive force of the adhesive composition decreases with increasing temperature, and
[0016] The amount of adhesive strength reduction per 1° C., that is, the adhesive strength reduction rate of the adhesive composition is greater near the melting point of the temperature-sensitive non-crosslinked polymer than in a temperature range other than near the melting point of the temperature-sensitive non-crosslinked polymer.
[0017] A second aspect of the present invention is a light-transmitting roof material, wherein:
[0018] It comprises at least one light-transmitting substrate layer and at least one adhesive layer,
[0019] The adhesive layer includes an adhesive composition containing 1 to 20 parts by mass of a temperature-sensitive non-crosslinked polymer and 1 to 100 parts by mass of temperature-sensitive crosslinked fine particles relative to 100 parts by mass of an adhesive.
[0020] The refractive index of the thermosensitive cross-linked microparticles decreases as the temperature increases, and
[0021] The amount of refractive index reduction per 1°C, that is, the refractive index reduction rate of the temperature-sensitive crosslinked fine particles is greater near the melting point of the temperature-sensitive crosslinked fine particles than in a temperature range other than near the melting point of the temperature-sensitive crosslinked fine particles.
[0022] The adhesive force of the adhesive composition decreases with increasing temperature, and
[0023] The amount of adhesive strength reduction per 1° C., that is, the adhesive strength reduction rate of the adhesive composition is greater near the melting point of the temperature-sensitive non-crosslinked polymer than in a temperature range other than near the melting point of the temperature-sensitive non-crosslinked polymer.
[0024] A third aspect of the present invention is a building comprising the window material according to the first aspect and / or the light-transmitting roofing material according to the second aspect.
[0025] A fourth aspect of the present invention is a vehicle, a ship, or an aircraft, comprising the window material according to the first aspect and / or the light-transmitting roof material according to the second aspect.
[0026] A fifth aspect of the present invention is an adhesive composition comprising 1 to 20 parts by mass of a temperature-sensitive non-crosslinked polymer and 1 to 100 parts by mass of temperature-sensitive crosslinked fine particles per 100 parts by mass of an adhesive, wherein:
[0027] The refractive index of the thermosensitive cross-linked microparticles decreases as the temperature increases, and
[0028] The amount of refractive index reduction per 1°C, that is, the refractive index reduction rate of the temperature-sensitive crosslinked fine particles is greater near the melting point of the temperature-sensitive crosslinked fine particles than in a temperature range other than near the melting point of the temperature-sensitive crosslinked fine particles.
[0029] The adhesive force of the adhesive composition decreases with increasing temperature, and
[0030] The amount of adhesive strength reduction per 1° C., that is, the adhesive strength reduction rate of the adhesive composition is greater near the melting point of the temperature-sensitive non-crosslinked polymer than in a temperature range other than near the melting point of the temperature-sensitive non-crosslinked polymer.
[0031] A sixth aspect of the present invention is a pressure-sensitive adhesive sheet, wherein:
[0032] A pressure-sensitive adhesive layer comprising the pressure-sensitive adhesive composition according to the fifth aspect is provided.
[0033] Effects of the Invention
[0034] According to the present invention, there can be provided a window material or a light-transmitting roof material which can autonomously change the white turbidity according to the temperature, has a simple structure and is easy to manufacture, and a building, a vehicle, a ship or an aircraft having the window material and / or the light-transmitting roof material. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 : is a cross-sectional view showing a first window material as an example of a window material.
[0036] Figure 2 : is a cross-sectional view showing a second window material as an example of a window material.
[0037] Figure 3 This is a cross-sectional view showing an example of a light-transmitting roofing material.
[0038] Figure 4 This is a graph showing the results of measuring the refractive index of the temperature-sensitive cross-linked fine particles produced in Examples.
[0039] Figure 5 It is a schematic explanatory diagram showing the evaluation test method of the heat insulation in the examples.
[0040] Figure 6 The photographs show the evaluation test method of the heat insulation properties in the examples.
[0041] Figure 7 The photographs show the evaluation test method of the heat insulation properties in the examples. DETAILED DESCRIPTION
[0042] The specific embodiments of the present invention are described in detail below, but the present invention is not limited by the following embodiments and can be implemented by appropriate changes within the scope of the purpose of the present invention. In addition, the following figures are schematically shown, and the size and shape of each part are appropriately exaggerated or omitted for easy understanding.
[0043] <<Window materials>>
[0044] exist Figure 1 , a cross-sectional view of a first window material 10 is shown as an example of a window material. Figure 1 As shown, in the first window material 10, a light-transmitting base material layer 11, an adhesive layer 12, and a base sheet 13 are sequentially laminated. The adhesive layer 12 is composed of an adhesive composition including an adhesive, a temperature-sensitive non-crosslinked polymer, and temperature-sensitive crosslinked fine particles 12a.
[0045] exist Figure 2 , as another example of a window material, a cross-sectional view of a second window material 20 is shown. Figure 2 As shown, in the second window material 20, an adhesive layer 22 is disposed between two light-transmitting base material layers 21a and 21b. The adhesive layer 22 is composed of an adhesive composition including an adhesive, a temperature-sensitive non-crosslinked polymer, and temperature-sensitive crosslinked fine particles 22a.
[0046] exist Figure 1 and Figure 2 In the embodiment, the refractive index of the temperature-sensitive crosslinked particles 12a and 22a decreases as the temperature rises, and the amount of refractive index reduction per 1°C, i.e., the refractive index reduction rate, is greater near the melting point than in the temperature range other than the melting point. Therefore, when the temperature of the adhesive layers 12 and 22 rises due to sunlight or air temperature, the refractive index difference between the temperature-sensitive crosslinked particles 12a and 22a and the adhesive becomes larger, and the haze value becomes higher. On the other hand, when the temperature of the adhesive layers 12 and 22 decreases, the refractive index difference between the temperature-sensitive crosslinked particles 12a and 22a and the adhesive becomes smaller, and the haze value becomes lower. As a result, the white turbidity can be changed autonomously according to the temperature, and direct sunlight can be mitigated during high temperatures in summer and sunlight can be taken in during low temperatures in winter.
[0047] Furthermore, it is also possible to design the structure so that the difference in refractive index between the temperature-sensitive crosslinked fine particles 12 a and 22 a and the binder decreases as the temperature rises.
[0048] In this case, for example, in conditions where the temperature is relatively low and the amount of sunlight is small, such as in the morning or at night, the window material functions as frosted glass. On the other hand, during the day, when the temperature rises as the amount of sunlight increases, the window material becomes transparent and can efficiently let light into the room.
[0049] In addition, when the above-mentioned window material is constructed to a position in contact with external air, the above-mentioned window material becomes cloudy or transparent as the temperature of the external air rises, and therefore also has the function of allowing people living in an air-conditioned room to visually recognize the increase in the temperature of the external air.
[0050] Moreover, the adhesive force of the adhesive composition constituting the adhesive layers 12 and 22 decreases as the temperature rises, and the amount of decrease in adhesive force per 1°C, i.e., the adhesive force decrease rate, is greater near the melting point of the temperature-sensitive non-crosslinked polymer in the adhesive composition than in a temperature range other than the melting point. Therefore, even if bubbles are involved or wrinkles occur when configuring the adhesive layers 12 and 22, the adhesive layers 12 and 22 can be peeled off and configured again by increasing the temperature of the adhesive layers 12 and 22. Thus, the manufacture of the window material can be made easier.
[0051] Hereinafter, each layer constituting the first window material 10 and the second window material 20 will be described.
[0052] [Light-transmitting base material layer]
[0053] As the light-transmitting substrate constituting the light-transmitting substrate layer, as long as it can be used as a substrate for building, vehicle, ship, or aircraft window material, it is not particularly limited, and for example, a glass plate or a resin plate can be used. As the material of the glass plate, soda-lime glass, borosilicate glass, high silica glass, etc. can be cited. In addition, as the material of the resin plate, polymethacrylate alkyl esters such as polymethyl methacrylate, polyacrylate alkyl esters, polycarbonate, polymethyl styrene, acrylonitrile-styrene copolymers, etc. can be cited.
[0054] The thickness of the light-transmitting base material layer is not particularly limited, and is, for example, 0.1 mm to 10 mm. Examples of the shape of the light-transmitting base material layer include a flat surface shape such as the first window material 10 and the second window material 20 , and a curved surface shape.
[0055] The light-transmitting substrate layer is composed of at least one layer, and may be composed of a single layer as in the first window material 10, or may be composed of two or more layers as in the second window material 20. When composed of two or more layers, each layer may be composed of the same type of substrate, or may be composed of different types of substrates. In addition, each layer may be of the same thickness, or may be of different thicknesses.
[0056] [Adhesive layer]
[0057] The adhesive layer is a layer comprising an adhesive composition containing 1 to 20 parts by mass of a temperature-sensitive non-crosslinked polymer and 1 to 100 parts by mass of temperature-sensitive crosslinked fine particles per 100 parts by mass of the adhesive, and has the function of autonomously changing white turbidity and adhesive strength according to temperature.
[0058] The thickness of the adhesive layer is not particularly limited, but is preferably 5 μm or more and 1 mm or less, and more preferably 10 μm or more and 100 μm or less. In addition, the thicker the adhesive layer, the more likely it is that a dimming function will be exhibited by adding a small amount of temperature-sensitive cross-linked particles. The thinner the thickness, the more likely it is that a large amount of temperature-sensitive cross-linked particles need to be added in order to exhibit the dimming function.
[0059] The adhesive layer is composed of at least one layer. The adhesive layer may be composed of a single layer as in the first window material 10 and the second window material 20, or may be composed of two or more layers. The configuration of the adhesive layer relative to the light-transmitting substrate layer is not particularly limited. The adhesive layer may be configured on the side where sunlight is incident relative to the light-transmitting substrate layer, or may be configured on the opposite side thereof. In the case where the light-transmitting substrate layer is composed of two or more layers, the adhesive layer may be configured between the light-transmitting substrate layers as in the second window material 20.
[0060] Furthermore, the adhesive layer may cover the entire surface of the surface in contact with the light-transmitting base layer, or may cover a portion of it.
[0061] In the case where the adhesive layer covers a part of the surface where the adhesive layer and the light-transmitting substrate layer are in contact, text, marks, patterns, graphics, designs, etc. can also be drawn on the light-transmitting substrate layer through the adhesive layer. In this case, the text or pattern can be formed by the adhesive layer, or the text or pattern can be formed in the area surrounded by the adhesive layer. Such a window material has excellent appearance design when the haze appears or disappears at high temperature.
[0062] Furthermore, the adhesive layer may have a plurality of regions having different haze values at high temperatures or low temperatures. The haze value of the adhesive layer can be changed by changing the type of adhesive or the thermosensitive crosslinked fine particles or by changing the amount of the thermosensitive crosslinked fine particles used.
[0063] For example, by continuously forming a plurality of adhesive layers having different haze values at high or low temperatures in a strip shape on a light-transmitting substrate, a window material having excellent design properties showing a gradated haze at high or low temperatures can be provided.
[0064] The difference between the haze value of the adhesive layer at 23°C and the haze value at 60°C is preferably 10% or more. In particular, it is more preferred that the haze value of the adhesive layer at 60°C is 10% or more higher than the haze value at 23°C. Thus, there is a tendency that the change in white turbidity corresponding to temperature is easily visually recognized. In this specification, the haze value of the adhesive layer is a value measured by the method described in the examples described later.
[0065] The haze value of the adhesive layer at 23°C is preferably 10% or less. The lower limit of the haze value at 23°C is not particularly limited. In addition, the haze value of the adhesive layer at 60°C is preferably 12% or more, more preferably 20% or more, and further preferably 30% or more. The upper limit of the haze value at 60°C is not particularly limited, for example, 70% or less, 50% or less.
[0066] The difference between the solar transmittance at 23°C and the solar transmittance at 60°C of the adhesive layer is preferably 10% or more. The solar transmittance at 60°C of the adhesive layer is preferably 10% or more lower than the solar transmittance at 23°C. In addition, in this specification, the solar transmittance of the adhesive layer is a value measured by the method described in the Examples described later.
[0067] The solar transmittance of the adhesive layer at 23°C is preferably 50% or more, more preferably 70% or more, and further preferably 80% or more. The upper limit of the solar transmittance at 23°C is not particularly limited, and is, for example, 99% or less, 95% or less. In addition, the solar transmittance of the adhesive layer at 60°C is preferably 80% or less, more preferably 70% or less, and further preferably 60% or less. The lower limit of the solar transmittance at 60°C is not particularly limited.
[0068] (Thermosensitive cross-linked microparticles)
[0069] Figure 4 Graph showing the change in refractive index of the temperature-sensitive crosslinked fine particles (melting point 33° C.) produced in the examples described below with respect to temperature changes. Figure 4 As shown, the refractive index of the temperature-sensitive crosslinked fine particles decreases as the temperature rises, and the amount of decrease in the refractive index per 1° C., that is, the refractive index decrease rate, is greater near the melting point than in a temperature range other than the melting point.
[0070] The refractive index of the thermosensitive crosslinked microparticles at 60°C is preferably 0.02 or more lower than the refractive index of the thermosensitive crosslinked microparticles at 23°C. This makes it easier to visually recognize changes in white turbidity in accordance with temperature. In addition, in this specification, the refractive index is a value measured by the method described in the Examples below.
[0071] The melting point of the temperature-sensitive crosslinked fine particles is preferably 20° C. or higher, more preferably 25° C. or higher. In addition, the melting point is preferably 100° C. or lower, more preferably 60° C. or lower, and further preferably 40° C. or lower. In this specification, the melting point of the temperature-sensitive crosslinked fine particles is a value measured by the method described in the Examples below.
[0072] The melting point of the temperature-sensitive crosslinked microparticles can be adjusted, for example, by changing the composition of the monomer components constituting the side chain crystalline polymer A contained in the temperature-sensitive crosslinked microparticles. To give a specific example, the melting point can be adjusted by changing the length of the side chain in the side chain crystalline polymer A. When the length of the side chain is long, there is a tendency for the melting point of the temperature-sensitive crosslinked microparticles to be high.
[0073] The average particle size of the thermosensitive crosslinked microparticles is preferably 1 μm or more, more preferably 3 μm or more. In addition, the average particle size is preferably 100 μm or less, more preferably 30 μm or less. In particular, from the perspective of easy haze improvement, the average particle size is more preferably 3 μm or more and 10 μm or less, and most preferably 3 μm or more and 6 μm or less. It is easy to suppress the transmission of sunlight. From the perspective of easy heat insulation, the average particle size is more preferably 6 μm or more and 25 μm or less, and most preferably 10 μm or more and 25 μm or less.
[0074] In addition, the D90 particle size of the temperature-sensitive crosslinked fine particles is preferably less than the thickness of the adhesive layer, for example, from 1 μm to 1000 μm, from 3 μm to 100 μm. When the D90 particle size is less than the thickness of the adhesive layer, the surface of the adhesive layer becomes uniform and tends to be less likely to hinder the adhesive force.
[0075] In the present specification, the average particle size and D90 particle size of the thermosensitive crosslinked fine particles are values measured by the method described in Examples below.
[0076] Thermosensitive crosslinked microparticles preferably include side chain crystalline polymer A. Side chain crystalline polymer A preferably includes a constituent unit derived from a (meth) acrylic monomer having a straight-chain alkyl group with a carbon number of 14 or more. In the constituent unit derived from a (meth) acrylic monomer having a straight-chain alkyl group with a carbon number of 14 or more, the straight-chain alkyl group with a carbon number of 14 or more functions as a side chain crystalline site in the side chain crystalline polymer A. That is, the side chain crystalline polymer A is, for example, a comb-shaped polymer having a straight-chain alkyl group with a carbon number of 14 or more in the side chain. The side chain is integrated into an orderly arrangement by intermolecular forces, etc., so that the side chain crystalline polymer A crystallizes. In addition, the above-mentioned (meth) acrylic monomer refers to an acrylic monomer (acrylic monomer) or a methacrylic monomer. The upper limit of the carbon number of the straight-chain alkyl group is preferably less than 50, more preferably less than 30.
[0077] Examples of the (meth)acrylic acid monomer having a linear alkyl group having 14 or more carbon atoms include hexadecyl (meth)acrylate, octadecyl (meth)acrylate, eicosyl (meth)acrylate, and behenyl (meth)acrylate. These monomers may be used alone or in combination of two or more.
[0078] The ratio of the mass of the constituent units derived from the (meth)acrylic acid monomer having a linear alkyl group having 14 or more carbon atoms to the mass of the side chain crystalline polymer A is preferably 70% by mass or more, more preferably 80% by mass or more, and further preferably 90% by mass or more. The above ratio may be 100% by mass, but is preferably 95% by mass or less.
[0079] The side chain crystalline polymer A may also include constituent units derived from other monomers copolymerizable with a (meth)acrylic monomer having a linear alkyl group having 14 or more carbon atoms. Examples of other monomers include monofunctional monomers, polyfunctional monomers, and refractive index adjusting monomers. That is, the side chain crystalline polymer A may also include constituent units derived from monofunctional monomers or polyfunctional monomers and refractive index adjusting monomers.
[0080] As monofunctional monomers, for example, (meth)acrylic acid monomers having an alkyl group with 1 to 12 carbon atoms, such as methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, hexyl (meth)acrylate, lauryl (meth)acrylate, and 2-ethylhexyl acrylate, etc., can be cited. Only one of them can be used, or two or more of them can be used in combination. In addition, when it is desired to add some functions in addition to temperature sensitivity, as long as it can be copolymerized with a (meth)acrylic acid monomer having a linear alkyl group with 14 or more carbon atoms and has the function, the monomer can be freely copolymerized.
[0081] The ratio of the mass of the structural unit derived from the monofunctional monomer to the mass of the side chain crystalline polymer A is preferably 0.1 mass % or more, more preferably 1 mass % or more. The ratio is preferably 20 mass % or less, more preferably 10 mass % or less.
[0082] The multifunctional monomer can crosslink the multiple molecular chains contained in the side chain crystalline polymer A. From the perspective of the dispersion state of the temperature-sensitive crosslinked microparticles during use or the suppression of deformation and the repeatability of the function, the side chain crystalline polymer A preferably contains a constituent unit derived from the multifunctional monomer. That is, it is preferred that the temperature-sensitive crosslinked microparticles or the side chain crystalline polymer A are crosslinked. The multifunctional monomer has two or more, preferably 2 to 4, double bonds that can be free radically polymerized in the molecule. As a multifunctional monomer, for example, bifunctional (meth) acrylates, trifunctional (meth) acrylates, and tetrafunctional (meth) acrylates can be cited. As specific examples, 1,6-hexanediol di(meth) acrylate, 1,9-nonanediol di(meth) acrylate, trimethylolpropane tri(meth) acrylate, pentaerythritol tetra(meth) acrylate, polyethylene glycol 200 di(meth) acrylate, ethoxylated bisphenol A di(meth) acrylate, etc. can be cited. They can be used alone or in combination of two or more. The polyfunctional monomer may be at least one selected from bifunctional (meth)acrylates, trifunctional (meth)acrylates, and tetrafunctional (meth)acrylates.
[0083] The ratio of the mass of the structural unit derived from the polyfunctional monomer to the mass of the side chain crystalline polymer A is preferably 0.1 mass % or more, more preferably 1 mass % or more. The ratio is preferably 20 mass % or less, more preferably 10 mass % or less.
[0084] The refractive index adjusting monomer may be a monomer having a refractive index of 1.300 to 1.600. Examples of the refractive index adjusting monomer include 2-(o-phenylphenoxy)ethyl acrylate (refractive index: 1.577), 2-(3-phenoxyphenyl)methyl acrylate (refractive index: 1.566), 1-naphthyl acrylate (refractive index: 1.595), acrylamide (refractive index: 1.515), hydroxyacrylamide (refractive index: 1.515), EO-modified bisphenol A diacrylate (refractive index: 1.537), acrylamide (refractive index: 1.515), 2,2,2-trifluoroethyl acrylate (refractive index: 1.348), and methacrylic acid-modified polydimethylsiloxane (refractive index: 1.408). These monomers may be used alone or in combination of two or more.
[0085] The ratio of the mass of the constituent units derived from the refractive index adjusting monomer to the mass of the side chain crystalline polymer A is preferably 0.1 mass % or more, more preferably 1 mass % or more. In addition, the above ratio is preferably 30 mass % or less, more preferably 20 mass % or less, and further preferably 10 mass % or less.
[0086] From the aspect of having a good dispersibility in the adhesive, the temperature-sensitive crosslinked microparticles preferably do not contain a constituent unit derived from a reactive emulsifier. A reactive emulsifier refers to an emulsifier having a polymerizable unsaturated bond such as a vinyl group in the molecule. A reactive emulsifier is a polymerizable monomer having an emulsifying function and having a hydrophilic group and a polymerizable group having an unsaturated bond such as a vinyl group in its molecule.
[0087] In the adhesive composition, the content of the temperature-sensitive crosslinked microparticles is 1 part by mass or more and 100 parts by mass or less relative to 100 parts by mass of the adhesive. The above content is preferably 5 parts by mass or more, more preferably 20 parts by mass or more. In addition, the above content is preferably 70 parts by mass or less, more preferably 40 parts by mass or less.
[0088] The method for producing the thermosensitive crosslinked fine particles is not particularly limited, and the fine particles can be obtained by a conventionally known polymerization method such as mini-emulsion polymerization and suspension polymerization.
[0089] (Thermosensitive non-crosslinked polymer)
[0090] The temperature-sensitive non-crosslinked polymer has a melting point. The temperature-sensitive non-crosslinked polymer crystallizes at a temperature below the melting point, and undergoes a phase change and exhibits fluidity at a temperature above the melting point. Thus, the adhesive force of the adhesive composition comprising an adhesive and a temperature-sensitive non-crosslinked polymer decreases as the temperature rises, and the amount of decrease in adhesive force per 1°C, i.e., the rate of decrease in adhesive force, is greater near the melting point of the temperature-sensitive non-crosslinked polymer in the adhesive composition than in a temperature region other than near the melting point. In addition, in this specification, the adhesive force of the adhesive composition refers to the peel strength relative to stainless steel (SUS), which is a value measured by the method described in the embodiments described later.
[0091] The peel strength of the adhesive composition with respect to stainless steel (SUS) at 23° C. is preferably 1.0 N / 25 mm or more. The upper limit of the peel strength is not particularly limited.
[0092] The adhesive composition preferably has a peel strength with respect to stainless steel (SUS) of 0.1 N / 25 mm or less at 60° C. The lower limit of the peel strength is not particularly limited.
[0093] The melting point of the temperature-sensitive non-crosslinked polymer is preferably 20° C. or higher, more preferably 30° C. or higher, and further preferably 40° C. or higher. In addition, the melting point is preferably 100° C. or lower, more preferably 80° C. or lower, and further preferably 60° C. or lower. In the present specification, the melting point of the temperature-sensitive non-crosslinked polymer is a value measured by the method described in the Examples below.
[0094] The melting point of the temperature-sensitive non-crosslinked polymer is preferably higher than the melting point of the temperature-sensitive crosslinked fine particles by 5° C. or more. This allows the white turbidity to change autonomously according to the temperature, and also allows the adhesive layer to be peeled off and rearranged by setting the temperature to a higher level.
[0095] The melting point of the temperature-sensitive non-crosslinked polymer can be adjusted by, for example, changing the composition of the monomer components constituting the side chain crystalline polymer B included in the temperature-sensitive non-crosslinked polymer. To give a specific example, the melting point can be adjusted by changing the length of the side chain in the side chain crystalline polymer B. When the length of the side chain is long, there is a tendency for the melting point of the temperature-sensitive crosslinked fine particles to be high.
[0096] The temperature-sensitive non-crosslinked polymer preferably includes a side chain crystalline polymer B. The side chain crystalline polymer B preferably includes a constituent unit derived from a (meth) acrylic monomer having a straight-chain alkyl group with a carbon number of 14 or more. In the constituent unit derived from a (meth) acrylic monomer having a straight-chain alkyl group with a carbon number of 14 or more, the straight-chain alkyl group with a carbon number of 14 or more functions as a side chain crystalline site in the side chain crystalline polymer B. That is, the side chain crystalline polymer B is, for example, a comb-shaped polymer having a straight-chain alkyl group with a carbon number of 14 or more in the side chain. The side chain is integrated into an orderly arrangement by intermolecular forces, etc., so that the side chain crystalline polymer B is crystallized. In addition, the above-mentioned (meth) acrylic monomer refers to an acrylic monomer or a methacrylic monomer. The upper limit of the carbon number of the straight-chain alkyl group is preferably 50 or less, more preferably 30 or less.
[0097] Examples of the (meth)acrylic acid monomer having a linear alkyl group having 14 or more carbon atoms include hexadecyl (meth)acrylate, octadecyl (meth)acrylate, eicosyl (meth)acrylate, and behenyl (meth)acrylate. These monomers may be used alone or in combination of two or more.
[0098] The ratio of the mass of the constituent units derived from the (meth)acrylic monomer having a linear alkyl group having 14 or more carbon atoms to the mass of the side chain crystalline polymer B is preferably 70% by mass or more. The above ratio may be 100% by mass, but is preferably 90% by mass or less, and more preferably 80% by mass or less.
[0099] The side chain crystalline polymer B may also contain a constituent unit derived from other monomers copolymerizable with a (meth)acrylic monomer having a linear alkyl group having 14 or more carbon atoms. Examples of other monomers include compatible monomers, etc. That is, the side chain crystalline polymer B may also contain a constituent unit derived from a compatible monomer.
[0100] As compatible monomers, for example, (meth)acrylates having an alkyl group with a carbon number of 1 to 12, such as ethylhexyl (meth)acrylate, methyl (meth)acrylate, ethyl (meth)acrylate, and butyl (meth)acrylate; (meth)acrylates having an ethylene glycol group, such as 2-ethylhexyl-diethylene glycol (meth)acrylate, methoxyethyl (meth)acrylate, methoxypolyethylene glycol mono(meth)acrylate, and ethoxy-diethylene glycol (meth)acrylate; (meth)acrylates having a hydroxyalkyl group, such as hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, and hydroxyhexyl (meth)acrylate; ethylenically unsaturated monomers having a carboxyl group, such as acrylic acid, methacrylic acid, crotonic acid, itaconic acid, maleic acid, and fumaric acid; styrene, vinyl acetate, and the like. These may be used alone or in combination of two or more. Among them, (meth)acrylates having an alkyl group with a carbon number of 1 to 12 and ethylenically unsaturated monomers having a carboxyl group are preferred.
[0101] The ratio of the mass of the structural unit derived from the compatible monomer to the mass of the side chain crystalline polymer B is preferably 0.1 mass % or more, more preferably 1 mass % or more. The ratio is preferably 90 mass % or less, more preferably 80 mass % or less.
[0102] The side chain crystalline polymer B may include the same structural unit as that included in the polymer constituting the adhesive. This improves the dispersibility of the non-crosslinked polymer in the adhesive composition and tends to reduce the adhesive force when heated.
[0103] The weight average molecular weight of the temperature-sensitive non-crosslinked polymer is preferably 1000 or more, more preferably 5000 or more. The above-mentioned weight average molecular weight is preferably 100,000 or less, more preferably 10,000 or less. When it is 100,000 or less, there is a tendency to suppress the influence of the temperature-sensitive non-crosslinked polymer on the haze value when it is added. When it is 10,000 or less, there is a tendency to easily reduce the adhesive force when heating. In addition, in this specification, the weight average molecular weight of the temperature-sensitive non-crosslinked polymer is a value measured by the method described in the embodiments described later.
[0104] The weight average molecular weight of the temperature-sensitive non-crosslinked polymer can be adjusted by, for example, using a chain transfer agent during polymerization. As the chain transfer agent, for example, mercaptan compounds such as dodecyl mercaptan, mercaptopropionic acid, mercaptosuccinic acid, ethylhexyl mercaptoacetate, mercaptoethanol, and cyclohexanethiol can be cited. These can be used alone or in combination of two or more.
[0105] In the adhesive composition, the content of the temperature-sensitive non-crosslinked polymer is 1 part by mass or more and 20 parts by mass or less relative to 100 parts by mass of the adhesive. The above content is preferably 3 parts by mass or more. The above content is preferably 10 parts by mass or less.
[0106] The method for producing the temperature-sensitive non-crosslinked polymer is not particularly limited, and the temperature-sensitive non-crosslinked polymer can be obtained by a conventionally known polymerization method such as solution polymerization and UV polymerization.
[0107] (Adhesive)
[0108] The adhesive is not particularly limited, and conventionally known adhesives such as acrylic adhesives, natural rubber adhesives, synthetic rubber adhesives, silicone adhesives, and urethane adhesives can be used. Among them, acrylic adhesives are preferred.
[0109] The polymer constituting the adhesive preferably comprises the constituent units derived from the adhesive monomers that contribute to adhesion, the constituent units derived from the functional group monomers for crosslinking. The polymer constituting the adhesive may also comprise the constituent units derived from other monomers that can copolymerize with these monomers. As other monomers, for example, refractive index adjustment monomers etc. may be enumerated. That is, the polymer constituting the adhesive may also comprise the constituent units derived from the refractive index adjustment monomers.
[0110] Examples of the adhesive monomer include (meth)acrylates having an alkyl group with 1 to 12 carbon atoms, such as ethylhexyl (meth)acrylate, methyl (meth)acrylate, ethyl (meth)acrylate, and butyl (meth)acrylate; (meth)acrylates having an ethylene glycol group, such as 2-ethylhexyl-diethylene glycol (meth)acrylate, methoxyethyl (meth)acrylate, methoxypolyethylene glycol mono(meth)acrylate, and ethoxy-diethylene glycol (meth)acrylate; ethylenically unsaturated monomers such as styrene and vinyl acetate; and the like. These monomers may be used alone or in combination of two or more. Among them, (meth)acrylates having an alkyl group with 1 to 12 carbon atoms are preferred.
[0111] The ratio of the mass of the constituent units derived from the binder monomer to the mass of the polymer constituting the binder is preferably 50% by mass or more, more preferably 70% by mass or more, and preferably 99.9% by mass or less, more preferably 95% by mass or less.
[0112] Examples of the functional group monomer include (meth)acrylates having a hydroxyalkyl group such as hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, and hydroxyhexyl (meth)acrylate; ethylenically unsaturated monomers having a carboxyl group such as acrylic acid, methacrylic acid, crotonic acid, itaconic acid, maleic acid, and fumaric acid; etc. Only one type may be used, or two or more types may be used in combination.
[0113] The mass of the constituent unit derived from the functional group monomer is preferably more than 0.1 mass % relative to the ratio of the mass of the polymer constituting the adhesive, and more preferably more than 1 mass %. In addition, the above ratio is preferably below 30 mass %, more preferably below 20 mass %, and further preferably below 10 mass %. When it is more than 0.1 mass %, there is a good trend of shape retention. When it is less than 30 mass %, there is a trend that viscosity will not excessively become high and coating property is good.
[0114] The refractive index adjusting monomer may be a monomer having a refractive index of 1.300 to 1.600. Examples of the refractive index adjusting monomer include 2-(o-phenylphenoxy)ethyl acrylate (refractive index: 1.577), 2-(3-phenoxyphenyl)methyl acrylate (refractive index: 1.566), 1-naphthyl acrylate (refractive index: 1.595), acrylamide (refractive index: 1.515), hydroxyacrylamide (refractive index: 1.515), EO-modified bisphenol A diacrylate (refractive index: 1.537), acrylamide (refractive index: 1.515), 2,2,2-trifluoroethyl acrylate (refractive index: 1.348), and methacrylic acid-modified polydimethylsiloxane (refractive index: 1.408). These monomers may be used alone or in combination of two or more.
[0115] The ratio of the mass of the constituent units derived from the refractive index adjusting monomer to the mass of the polymer constituting the binder is preferably 0.1 mass % or more, more preferably 1 mass % or more, and further preferably 10 mass % or more. The above ratio is preferably 30 mass % or less.
[0116] The weight average molecular weight of the adhesive is preferably more than 200,000, more preferably more than 300,000. The above-mentioned weight average molecular weight is preferably less than 2,000,000, more preferably less than 1,000,000, and further preferably less than 600,000. When more than 200,000, there is a trend of good shape retention. When less than 2,000,000, there is a trend that the viscosity does not excessively become high and the coating property is good. In addition, in this specification, the weight average molecular weight of the adhesive is a value measured by the method described in the embodiments described later.
[0117] The glass transition temperature (Tg) of the adhesive is preferably 25° C. or less because it tends to exhibit high adhesive strength. In the present specification, the glass transition temperature is a value measured by the method described in Examples below.
[0118] The refractive index difference between the binder and the thermosensitive crosslinked fine particles at 23°C is preferably less than 0.015, more preferably less than 0.010. The refractive index difference at 60°C is preferably 0.015 or more. The upper limit of the refractive index difference at 60°C is not particularly limited, and is, for example, 0.1.
[0119] Thus, in general, in a warm atmosphere where people and pets can live comfortably, the adhesive layer exhibits high light transmittance, whereas in a high temperature atmosphere such as in summer, the light transmittance of the adhesive layer decreases due to the appearance of haze.
[0120] Alternatively, the refractive index of the binder and the thermosensitive crosslinked fine particles can be adjusted so that the difference in refractive index between the binder and the thermosensitive crosslinked fine particles at 23° C. is 0.015 or more and the difference in refractive index at 60° C. is less than 0.015.
[0121] In this case, for example, when the adhesive is applied to window glass, the window glass functions as frosted glass in conditions such as the morning or night when the temperature is relatively low and the amount of sunlight is small. On the other hand, during the day, when the temperature rises as the amount of sunlight increases, the window material becomes transparent and can efficiently let in light into the room. In this way, even without opening or closing the curtain, it is easy to let in light into the room only during the day.
[0122] The ratio of the mass of the adhesive to the mass of the solid content of the adhesive composition is not particularly limited, and is, for example, 50% by mass or more and 95% by mass or less. In addition, in this specification, the solid content of the adhesive composition refers to all components after removing solvents such as aqueous solvents or organic solvents from the adhesive composition.
[0123] The method for producing the adhesive is not particularly limited, and the adhesive can be obtained by a conventionally known polymerization method such as solution polymerization and UV polymerization.
[0124] The adhesive composition may also contain a crosslinking agent for crosslinking the adhesive. That is, the adhesive may be crosslinked. Examples of the crosslinking agent include aziridine-based crosslinking agents, metal chelate-based crosslinking agents, epoxy-based crosslinking agents, and isocyanate-based crosslinking agents.
[0125] In the adhesive composition, the content of the crosslinking agent is not particularly limited, for example, relative to 100 parts by mass of the adhesive, it is 0.1 parts by mass or more and 10 parts by mass or less. When it is 0.1 parts by mass or more, there is a tendency that the shape retention is not easy to become low. In addition, when it is 10 parts by mass or less, there is a tendency that it is easy to exert high adhesive force.
[0126] The adhesive composition may contain other additives such as organic solvents, inhibitors for inhibiting the progress of crosslinking, tackifying resins (tackifiers), ultraviolet (UV) absorbers, light stabilizers (HALS), antioxidants, infrared absorbers, dyes, pigments, etc.
[0127] [use]
[0128] There is no limitation on the mode in which the above-mentioned adhesive composition is used. The mode in which the above-mentioned adhesive composition is used can be appropriately selected according to the purpose.
[0129] The above-mentioned adhesive composition can autonomously change the degree of white turbidity according to the temperature.
[0130] When the adhesive composition is designed so as to develop haze at high temperatures, it can mitigate direct sunlight in the high temperatures of summer and take in sunlight in the low temperatures of winter. Therefore, it can be suitably used, for example, in window materials and translucent roof materials.
[0131] On the other hand, when the adhesive composition is designed to show haze at low temperatures, for example, when the adhesive composition is applied to window glass, the window glass functions as frosted glass under conditions such as morning or night when the temperature is relatively low and the amount of sunlight is small. On the other hand, during the day, when the temperature rises due to an increase in sunlight, the window glass becomes transparent and can efficiently let in light into the room.
[0132] In addition, when the haze of the adhesive composition appears or disappears at high temperatures caused by heat sources such as lighting or sunlight or air temperature, it can make the appearance of words, marks, patterns, graphics, designs, etc. appear or disappear, and can give excellent display properties (appearance designs such as words and marks) or decorative properties (appearance designs such as patterns, graphics, designs, etc.) to objects having an adhesive layer. Therefore, it can be suitable for decoration of lighting covers, decoration of light-transmitting substrates such as window materials or light-transmitting roof materials, display of light-transmitting substrates such as window materials or light-transmitting roof materials, etc.
[0133] [Base sheet]
[0134] The above-mentioned window material may or may not include a base sheet. The base sheet has a function as a support when laminating the adhesive layer on the light-transmitting base layer and a function as a protective layer for the adhesive layer.
[0135] The substrate constituting the substrate sheet is not particularly limited as long as it is a light-transmitting substrate. For example, corona-treated PET, untreated PET, highly transparent PET, annealed PET, UV-cut PET, heat-insulating PET, anti-fog PET, hard-coated PET, sandblasted PET, and other PETs; transparent PI, etc. can be used as the substrate.
[0136] [Method for producing window material]
[0137] The manufacture method of above-mentioned window material is not particularly limited, for example can enumerate after substrate sheet is coated with adhesive composition and made adhesive sheet, the method of bonding adhesive sheet at translucent substrate etc. can also be formed adhesive layer by directly coating adhesive composition at translucent substrate.In this case, preferably with substrate sheet covering the exposed face of the adhesive layer formed on translucent substrate, so that the sticky face that shows adhesive layer can not be exposed indoors or outdoors.In addition, when translucent substrate layer is composed of more than two layers as the second window material 20, the method that adhesive layer is configured between translucent substrate layer etc. can also be enumerated.In this case, as long as after coating adhesive composition on 1 substrate layer and forming adhesive layer, other substrate layers are bonded at the exposed face of adhesive layer.
[0138] Alternatively, the second window material 20 having an adhesive layer between the light-transmitting substrates can be manufactured by preparing two laminates each including a light-transmitting substrate layer and an adhesive layer laminated in contact with each other and bonding the two laminates together with the adhesive layer exposed.
[0139] [use]
[0140] There is no limitation on the scheme in which the above-mentioned window material is used. The scheme in which the above-mentioned window material is used can be appropriately selected according to the purpose. For example, the above-mentioned window material can be applied to buildings such as residences, buildings, warehouses, arcades, vehicles, ships or aircrafts.
[0141] <<Light-transmitting roofing materials>>
[0142] Figure 3 is a cross-sectional view showing an example of a light-transmitting roof material. Figure 3 As shown, in the light-transmitting roof material 30, a light-transmitting base material layer 31, an adhesive layer 32, and a base sheet 33 are sequentially laminated. The adhesive layer 32 is composed of an adhesive composition containing an adhesive, a temperature-sensitive non-crosslinked polymer, and temperature-sensitive crosslinked fine particles 32a.
[0143] exist Figure 3 In the embodiment, the refractive index of the thermosensitive crosslinked microparticles 32a decreases as the temperature rises, and the amount of refractive index reduction per 1°C, i.e., the refractive index reduction rate, is greater near the melting point than in the temperature range other than the melting point. Therefore, when the temperature of the adhesive layer 32 rises due to sunlight or air temperature, the refractive index difference between the thermosensitive crosslinked microparticles 32a and the adhesive becomes larger, and the haze value becomes higher. On the other hand, when the temperature of the adhesive layer 32 decreases, the haze value decreases due to the decrease in the refractive index difference between the thermosensitive crosslinked microparticles 32a and the adhesive. Thus, the turbidity can be changed autonomously according to the temperature, and direct sunlight can be mitigated in the high temperature of summer and sunlight can be taken in in the low temperature of winter.
[0144] Furthermore, it is also possible to design the structure so that the difference in refractive index between the temperature-sensitive crosslinked fine particles 32 a and the binder decreases as the temperature increases.
[0145] Moreover, the adhesive force of the adhesive composition constituting the adhesive layer 32 decreases as the temperature rises, and the decrease in adhesive force per 1°C, i.e., the adhesive force decrease rate, is greater near the melting point of the temperature-sensitive non-crosslinked polymer in the adhesive composition than in a temperature range other than the melting point. Therefore, even if bubbles are involved or wrinkles occur when configuring the adhesive layer 32, the adhesive layer 32 can be peeled off and configured again by increasing the temperature of the adhesive layer 32. Thus, the manufacture of the window material can be made easier.
[0146] Regarding the light-transmitting roofing material, the light-transmitting base material layer, adhesive layer, each layer of the base sheet, the manufacturing method and the use thereof are the same as those of the window material.
[0147] <<Adhesive composition>>
[0148] The adhesive composition contains 1 to 20 parts by mass of a temperature-sensitive non-crosslinked polymer and 1 to 100 parts by mass of temperature-sensitive crosslinked fine particles based on 100 parts by mass of the adhesive.
[0149] The refractive index of the temperature-sensitive crosslinked fine particles decreases as the temperature rises, and the amount of decrease in the refractive index per 1° C., that is, the refractive index decrease rate, is greater near the melting point than in a temperature range other than near the melting point.
[0150] In the case where each refractive index is adjusted in such a way that the refractive index difference between the temperature-sensitive crosslinked microparticles and the adhesive at low temperature becomes small, when the temperature of the adhesive layer formed by the adhesive composition rises due to sunlight or air temperature or heating, the refractive index difference between the temperature-sensitive crosslinked microparticles and the adhesive becomes large, and the haze value becomes high. On the other hand, when the temperature of the adhesive layer decreases, the refractive index difference between the temperature-sensitive crosslinked microparticles and the adhesive becomes small, and the haze value becomes low. Conversely, in the case where each refractive index is adjusted in such a way that the refractive index difference between the temperature-sensitive crosslinked microparticles and the adhesive at high temperature becomes small, when the temperature of the adhesive layer rises, the haze value becomes low, and when the temperature of the adhesive layer decreases, the haze value becomes high.
[0151] Therefore, in the former case, when an adhesive layer is arranged on a window material or a translucent roof material, the turbidity can be autonomously changed according to the temperature, and direct sunlight can be mitigated in the high temperature of summer and sunlight can be taken in in the low temperature of winter.
[0152] In addition, when an adhesive layer is formed by using an adhesive composition to draw a design such as text, a mark, a pattern, a figure, or a pattern, the design can be made to appear or disappear as the haze caused by a heat source such as lighting or a high temperature caused by sunlight or air temperature appears or disappears. Thus, an object having an adhesive layer can be given excellent display properties (text, mark, or other design) or decorative properties (pattern, figure, or other design).
[0153] In any case, when used as a pressure-sensitive adhesive sheet having a pressure-sensitive adhesive layer, the haze value of the pressure-sensitive adhesive layer becomes lower or higher, thereby enabling visual recognition of the following changes in pressure-sensitive adhesive force even in a scenario where there is no contact thermometer.
[0154] The adhesive strength of the adhesive composition decreases as the temperature rises, and the adhesive strength decrease rate per 1°C is greater near the melting point of the temperature-sensitive non-crosslinked polymer in the adhesive composition than in a temperature range other than the melting point.
[0155] Therefore, even when there is air bubble involved or wrinkle etc. when configuring the adhesive layer, by making the temperature of the adhesive layer rise, the adhesive layer can be peeled off and configured again. In addition, the processing components in the manufacturing process can be temporarily fixed firmly, and the processing components can be peeled off without destroying them.
[0156] (Thermosensitive cross-linked microparticles)
[0157] The refractive index of the temperature-sensitive crosslinked fine particles decreases as the temperature rises, and the amount of decrease in the refractive index per 1° C., that is, the refractive index decrease rate, is greater near the melting point than in a temperature range other than near the melting point.
[0158] The refractive index of the temperature-sensitive crosslinked fine particles at 60° C. is preferably 0.02 or more lower than the refractive index of the temperature-sensitive crosslinked fine particles at 23° C. This tends to make it easier to visually recognize changes in white turbidity depending on temperature.
[0159] The melting point of the temperature-sensitive crosslinked fine particles is preferably 20° C. or higher, more preferably 25° C. or higher. The melting point is preferably 100° C. or lower, more preferably 60° C. or lower, and further preferably 40° C. or lower.
[0160] The melting point of the temperature-sensitive crosslinked microparticles can be adjusted, for example, by changing the composition of the monomer components constituting the side chain crystalline polymer A contained in the temperature-sensitive crosslinked microparticles. To give a specific example, the melting point can be adjusted by changing the length of the side chain in the side chain crystalline polymer A. When the length of the side chain is long, there is a tendency for the melting point of the temperature-sensitive crosslinked microparticles to be high.
[0161] The average particle size of the thermosensitive crosslinked microparticles is preferably 1 μm or more, more preferably 3 μm or more. In addition, the average particle size is preferably 100 μm or less, more preferably 30 μm or less. In particular, from the perspective of easy haze improvement, the average particle size is more preferably 3 μm or more and 10 μm or less, and most preferably 3 μm or more and 6 μm or less. It is easy to suppress the transmission of sunlight. From the perspective of easy heat insulation, the average particle size is more preferably 6 μm or more and 25 μm or less, and most preferably 10 μm or more and 25 μm or less.
[0162] In addition, the D90 particle size of the temperature-sensitive crosslinked fine particles is preferably less than the thickness of the adhesive layer, for example, from 1 μm to 1000 μm, from 3 μm to 100 μm. When the D90 particle size is less than the thickness of the adhesive layer, the surface of the adhesive layer becomes uniform and tends to be less likely to hinder the adhesive force.
[0163] Thermosensitive crosslinked microparticles preferably include side chain crystalline polymer A. Side chain crystalline polymer A preferably includes a constituent unit derived from a (meth) acrylic monomer having a straight-chain alkyl group with a carbon number of 14 or more. In the constituent unit derived from a (meth) acrylic monomer having a straight-chain alkyl group with a carbon number of 14 or more, the straight-chain alkyl group with a carbon number of 14 or more functions as a side chain crystalline site in the side chain crystalline polymer A. That is, the side chain crystalline polymer A is, for example, a comb-shaped polymer having a straight-chain alkyl group with a carbon number of 14 or more in the side chain. The side chain is integrated into an orderly arrangement by intermolecular forces, etc., so that the side chain crystalline polymer A crystallizes. In addition, the above-mentioned (meth) acrylic monomer refers to an acrylic monomer or a methacrylic monomer. The upper limit of the carbon number of the straight-chain alkyl group is preferably 50 or less, more preferably 30 or less.
[0164] Examples of the (meth)acrylic acid monomer having a linear alkyl group having 14 or more carbon atoms include hexadecyl (meth)acrylate, octadecyl (meth)acrylate, eicosyl (meth)acrylate, and behenyl (meth)acrylate. These monomers may be used alone or in combination of two or more.
[0165] The ratio of the mass of the constituent units derived from the (meth)acrylic acid monomer having a linear alkyl group having 14 or more carbon atoms to the mass of the side chain crystalline polymer A is preferably 70% by mass or more, more preferably 80% by mass or more, and further preferably 90% by mass or more. The above ratio may be 100% by mass, but is preferably 95% by mass or less.
[0166] The side chain crystalline polymer A may also include constituent units derived from other monomers copolymerizable with a (meth)acrylic monomer having a linear alkyl group having 14 or more carbon atoms. Examples of other monomers include monofunctional monomers, polyfunctional monomers, and refractive index adjusting monomers. That is, the side chain crystalline polymer A may also include constituent units derived from monofunctional monomers or polyfunctional monomers and refractive index adjusting monomers.
[0167] As monofunctional monomers, for example, (meth)acrylic acid monomers having an alkyl group with 1 to 12 carbon atoms, such as methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, hexyl (meth)acrylate, lauryl (meth)acrylate, and 2-ethylhexyl acrylate, etc., can be cited. Only one of them can be used, or two or more of them can be used in combination. In addition, when it is desired to add some functions in addition to temperature sensitivity, as long as it can be copolymerized with a (meth)acrylic acid monomer having a linear alkyl group with 14 or more carbon atoms and has the function, the monomer can be freely copolymerized.
[0168] The ratio of the mass of the structural unit derived from the monofunctional monomer to the mass of the side chain crystalline polymer A is preferably 0.1 mass % or more, more preferably 1 mass % or more. The ratio is preferably 20 mass % or less, more preferably 10 mass % or less.
[0169] The multifunctional monomer can crosslink the multiple molecular chains contained in the side chain crystalline polymer A. From the perspective of the dispersion state of the temperature-sensitive crosslinked microparticles during use or the suppression of deformation and the repeatability of the function, the side chain crystalline polymer A preferably contains a constituent unit derived from the multifunctional monomer. That is, it is preferred that the temperature-sensitive crosslinked microparticles or the side chain crystalline polymer A are crosslinked. The multifunctional monomer has two or more, preferably 2 to 4, double bonds that can be free radically polymerized in the molecule. As a multifunctional monomer, for example, bifunctional (meth) acrylates, trifunctional (meth) acrylates, and tetrafunctional (meth) acrylates can be cited. As specific examples, 1,6-hexanediol di(meth) acrylate, 1,9-nonanediol di(meth) acrylate, trimethylolpropane tri(meth) acrylate, pentaerythritol tetra(meth) acrylate, polyethylene glycol 200 di(meth) acrylate, ethoxylated bisphenol A di(meth) acrylate, etc. can be cited. They can be used alone or in combination of two or more. The polyfunctional monomer may be at least one selected from bifunctional (meth)acrylates, trifunctional (meth)acrylates, and tetrafunctional (meth)acrylates.
[0170] The ratio of the mass of the structural unit derived from the polyfunctional monomer to the mass of the side chain crystalline polymer A is preferably 0.1 mass % or more, more preferably 1 mass % or more. The ratio is preferably 20 mass % or less, more preferably 10 mass % or less.
[0171] The refractive index adjusting monomer may be a monomer having a refractive index of 1.300 to 1.600. Examples of the refractive index adjusting monomer include 2-(o-phenylphenoxy)ethyl acrylate (refractive index: 1.577), 2-(3-phenoxyphenyl)methyl acrylate (refractive index: 1.566), 1-naphthyl acrylate (refractive index: 1.595), acrylamide (refractive index: 1.515), hydroxyacrylamide (refractive index: 1.515), EO-modified bisphenol A diacrylate (refractive index: 1.537), acrylamide (refractive index: 1.515), 2,2,2-trifluoroethyl acrylate (refractive index: 1.348), and methacrylic acid-modified polydimethylsiloxane (refractive index: 1.408). These monomers may be used alone or in combination of two or more.
[0172] The ratio of the mass of the constituent units derived from the refractive index adjusting monomer to the mass of the side chain crystalline polymer A is preferably 0.1 mass % or more, more preferably 1 mass % or more. In addition, the above ratio is preferably 30 mass % or less, more preferably 20 mass % or less, and further preferably 10 mass % or less.
[0173] From the aspect of having a good dispersibility in the adhesive, the temperature-sensitive crosslinked microparticles preferably do not contain a constituent unit derived from a reactive emulsifier. A reactive emulsifier refers to an emulsifier having a polymerizable unsaturated bond such as a vinyl group in the molecule. A reactive emulsifier is a polymerizable monomer having an emulsifying function and having a hydrophilic group and a polymerizable group having an unsaturated bond such as a vinyl group in its molecule.
[0174] In the adhesive composition, the content of the temperature-sensitive crosslinked microparticles is 1 part by mass or more and 100 parts by mass or less relative to 100 parts by mass of the adhesive. The above content is preferably 5 parts by mass or more, more preferably 20 parts by mass or more. In addition, the above content is preferably 70 parts by mass or less, more preferably 40 parts by mass or less.
[0175] The method for producing the thermosensitive crosslinked fine particles is not particularly limited, and the fine particles can be obtained by a conventionally known polymerization method such as miniemulsion polymerization and suspension polymerization.
[0176] (Thermosensitive non-crosslinked polymer)
[0177] The temperature-sensitive non-crosslinked polymer has a melting point. The temperature-sensitive non-crosslinked polymer crystallizes at a temperature below the melting point, and undergoes a phase change and exhibits fluidity at a temperature above the melting point. As a result, the adhesive force of the adhesive composition containing the adhesive and the temperature-sensitive non-crosslinked polymer decreases as the temperature rises, and the amount of decrease in adhesive force per 1°C, i.e., the adhesive force decrease rate, is greater near the melting point of the temperature-sensitive non-crosslinked polymer in the adhesive composition than in a temperature range other than near the melting point.
[0178] The peel strength of the adhesive composition with respect to stainless steel (SUS) at 23° C. is preferably 1.0 N / 25 mm or more. The upper limit of the peel strength is not particularly limited.
[0179] The adhesive composition preferably has a peel strength with respect to stainless steel (SUS) of 0.1 N / 25 mm or less at 60° C. The lower limit of the peel strength is not particularly limited.
[0180] The melting point of the temperature-sensitive non-crosslinked polymer is preferably 20° C. or higher, more preferably 30° C. or higher, and further preferably 40° C. or higher. The melting point is preferably 100° C. or lower, more preferably 80° C. or lower, and further preferably 60° C. or lower.
[0181] The melting point of the temperature-sensitive non-crosslinked polymer is preferably higher than the melting point of the temperature-sensitive crosslinked fine particles by 5° C. or more. This allows not only the turbidity to be changed autonomously according to the temperature, but also the adhesive layer to be peeled off and re-arranged by raising the temperature of the adhesive layer even when air bubbles are trapped or wrinkles occur during the arrangement of the adhesive layer.
[0182] In another embodiment, the melting point of the temperature-sensitive non-crosslinked polymer is preferably less than 5° C. different from the melting point of the temperature-sensitive crosslinked fine particles. This allows the white turbidity to change autonomously according to the temperature, and allows visual recognition of changes in adhesive strength even without a contact thermometer.
[0183] The melting point of the temperature-sensitive non-crosslinked polymer can be adjusted by, for example, changing the composition of the monomer components constituting the side chain crystalline polymer B included in the temperature-sensitive non-crosslinked polymer. To give a specific example, the melting point can be adjusted by changing the length of the side chain in the side chain crystalline polymer B. When the length of the side chain is long, there is a tendency for the melting point of the temperature-sensitive crosslinked fine particles to be high.
[0184] The temperature-sensitive non-crosslinked polymer preferably includes a side chain crystalline polymer B. The side chain crystalline polymer B preferably includes a constituent unit derived from a (meth) acrylic monomer having a straight-chain alkyl group with a carbon number of 14 or more. In the constituent unit derived from a (meth) acrylic monomer having a straight-chain alkyl group with a carbon number of 14 or more, the straight-chain alkyl group with a carbon number of 14 or more functions as a side chain crystalline site in the side chain crystalline polymer B. That is, the side chain crystalline polymer B is, for example, a comb-shaped polymer having a straight-chain alkyl group with a carbon number of 14 or more in the side chain. The side chain is integrated into an orderly arrangement by intermolecular forces, etc., so that the side chain crystalline polymer B is crystallized. In addition, the above-mentioned (meth) acrylic monomer refers to an acrylic monomer or a methacrylic monomer. The upper limit of the carbon number of the straight-chain alkyl group is preferably 50 or less, more preferably 30 or less.
[0185] Examples of the (meth)acrylic acid monomer having a linear alkyl group having 14 or more carbon atoms include hexadecyl (meth)acrylate, octadecyl (meth)acrylate, eicosyl (meth)acrylate, and behenyl (meth)acrylate. These monomers may be used alone or in combination of two or more.
[0186] The ratio of the mass of the constituent units derived from the (meth)acrylic monomer having a linear alkyl group having 14 or more carbon atoms to the mass of the side chain crystalline polymer B is preferably 70% by mass or more. The above ratio may be 100% by mass, but is preferably 90% by mass or less, and more preferably 80% by mass or less.
[0187] The side chain crystalline polymer B may also contain a constituent unit derived from other monomers copolymerizable with a (meth)acrylic monomer having a linear alkyl group having 14 or more carbon atoms. Examples of other monomers include compatible monomers, etc. That is, the side chain crystalline polymer B may also contain a constituent unit derived from a compatible monomer.
[0188] As compatible monomers, for example, (meth)acrylates having an alkyl group with a carbon number of 1 to 12, such as ethylhexyl (meth)acrylate, methyl (meth)acrylate, ethyl (meth)acrylate, and butyl (meth)acrylate, (meth)acrylates having an ethylene glycol group, such as 2-ethylhexyl-diethylene glycol (meth)acrylate, methoxyethyl (meth)acrylate, methoxypolyethylene glycol mono(meth)acrylate, and ethoxy-diethylene glycol (meth)acrylate, (meth)acrylates having a hydroxyalkyl group, such as hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, and hydroxyhexyl (meth)acrylate, ethylenically unsaturated monomers having a carboxyl group, such as acrylic acid, methacrylic acid, crotonic acid, itaconic acid, maleic acid, and fumaric acid, styrene, vinyl acetate, etc. These may be used alone or in combination of two or more. Among them, (meth)acrylates having an alkyl group with a carbon number of 1 to 12 and ethylenically unsaturated monomers having a carboxyl group are preferred.
[0189] The ratio of the mass of the structural unit derived from the compatible monomer to the mass of the side chain crystalline polymer B is preferably 0.1 mass % or more, more preferably 1 mass % or more. The ratio is preferably 90 mass % or less, more preferably 80 mass % or less.
[0190] The side chain crystalline polymer B may include the same structural unit as that included in the polymer constituting the adhesive. This improves the dispersibility of the non-crosslinked polymer in the adhesive composition and tends to reduce the adhesive force when heated.
[0191] The weight average molecular weight of the temperature-sensitive non-crosslinked polymer is preferably 1000 or more, more preferably 5000 or more. The weight average molecular weight is preferably 100,000 or less, more preferably 10,000 or less. When it is 100,000 or less, there is a tendency to suppress the influence of the temperature-sensitive non-crosslinked polymer on the haze value when added. When it is 10,000 or less, there is a tendency to easily reduce the adhesive force when heated.
[0192] The weight average molecular weight of the temperature-sensitive non-crosslinked polymer can be adjusted by, for example, using a chain transfer agent during polymerization. As the chain transfer agent, for example, mercaptan compounds such as dodecyl mercaptan, mercaptopropionic acid, mercaptosuccinic acid, ethylhexyl mercaptoacetate, mercaptoethanol, and cyclohexanethiol can be cited. These can be used alone or in combination of two or more.
[0193] In the adhesive composition, the content of the temperature-sensitive non-crosslinked polymer is 1 part by mass or more and 20 parts by mass or less relative to 100 parts by mass of the adhesive. The above content is preferably 3 parts by mass or more. The above content is preferably 10 parts by mass or less.
[0194] The method for producing the temperature-sensitive non-crosslinked polymer is not particularly limited, and the temperature-sensitive non-crosslinked polymer can be obtained by a conventionally known polymerization method such as solution polymerization and UV polymerization.
[0195] (Adhesive)
[0196] The adhesive is not particularly limited, and conventionally known adhesives such as acrylic adhesives, natural rubber adhesives, synthetic rubber adhesives, silicone adhesives, and urethane adhesives can be used. Among them, acrylic adhesives are preferred.
[0197] The polymer constituting the adhesive preferably comprises the constituent units derived from the adhesive monomers that contribute to adhesion, the constituent units derived from the functional group monomers for crosslinking. The polymer constituting the adhesive may also comprise the constituent units derived from other monomers that can copolymerize with these monomers. As other monomers, for example, refractive index adjustment monomers etc. may be enumerated. That is, the polymer constituting the adhesive may also comprise the constituent units derived from the refractive index adjustment monomers.
[0198] Examples of the adhesive monomer include (meth)acrylates having an alkyl group with 1 to 12 carbon atoms, such as ethylhexyl (meth)acrylate, methyl (meth)acrylate, ethyl (meth)acrylate, and butyl (meth)acrylate; (meth)acrylates having an ethylene glycol group, such as 2-ethylhexyl-diethylene glycol (meth)acrylate, methoxyethyl (meth)acrylate, methoxypolyethylene glycol mono(meth)acrylate, and ethoxy-diethylene glycol (meth)acrylate; ethylenically unsaturated monomers such as styrene and vinyl acetate; and the like. These monomers may be used alone or in combination of two or more. Among them, (meth)acrylates having an alkyl group with 1 to 12 carbon atoms are preferred.
[0199] The ratio of the mass of the constituent units derived from the binder monomer to the mass of the polymer constituting the binder is preferably 50% by mass or more, more preferably 70% by mass or more, and preferably 99.9% by mass or less, more preferably 90% by mass or less.
[0200] Examples of the functional group monomer include (meth)acrylates having a hydroxyalkyl group such as hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, and hydroxyhexyl (meth)acrylate; ethylenically unsaturated monomers having a carboxyl group such as acrylic acid, methacrylic acid, crotonic acid, itaconic acid, maleic acid, and fumaric acid; etc. Only one type may be used, or two or more types may be used in combination.
[0201] The mass of the constituent unit derived from the functional group monomer is preferably more than 0.1 mass % relative to the ratio of the mass of the polymer constituting the adhesive, and more preferably more than 1 mass %. In addition, the above ratio is preferably below 30 mass %, more preferably below 20 mass %, and further preferably below 10 mass %. When it is more than 0.1 mass %, there is a good trend of shape retention. When it is less than 30 mass %, there is a trend that viscosity will not excessively become high and coating property is good.
[0202] The refractive index adjusting monomer may be a monomer having a refractive index of 1.300 to 1.600. Examples of the refractive index adjusting monomer include 2-(o-phenylphenoxy)ethyl acrylate (refractive index: 1.577), 2-(3-phenoxyphenyl)methyl acrylate (refractive index: 1.566), 1-naphthyl acrylate (refractive index: 1.595), acrylamide (refractive index: 1.515), hydroxyacrylamide (refractive index: 1.515), EO-modified bisphenol A diacrylate (refractive index: 1.537), acrylamide (refractive index: 1.515), 2,2,2-trifluoroethyl acrylate (refractive index: 1.348), and methacrylic acid-modified polydimethylsiloxane (refractive index: 1.408). These monomers may be used alone or in combination of two or more.
[0203] The ratio of the mass of the constituent units derived from the refractive index adjusting monomer to the mass of the polymer constituting the binder is preferably 0.1 mass % or more, more preferably 1 mass % or more, and further preferably 10 mass % or more. The above ratio is preferably 30 mass % or less.
[0204] The weight average molecular weight of the adhesive is preferably 200,000 or more, more preferably 300,000 or more. The above weight average molecular weight is preferably 2,000,000 or less, more preferably 1,000,000 or less, and further preferably 600,000 or less. When it is 200,000 or more, there is a trend of good shape retention. When it is 2,000,000 or less, there is a trend of good coating property without excessively increasing viscosity.
[0205] The glass transition temperature (Tg) of the adhesive is preferably 25° C. or lower because the adhesive tends to exhibit high adhesive strength.
[0206] The refractive index difference between the binder and the thermosensitive crosslinked fine particles at 23°C is preferably less than 0.015, more preferably less than 0.010. The refractive index difference at 60°C is preferably 0.015 or more. The upper limit of the refractive index difference at 60°C is not particularly limited, and is, for example, 0.1.
[0207] The ratio of the mass of the adhesive to the mass of the solid content of the adhesive composition is not particularly limited, and is, for example, 50% by mass or more and 95% by mass or less. In addition, in this specification, the solid content of the adhesive composition refers to all components after removing solvents such as aqueous solvents or organic solvents from the adhesive composition.
[0208] The method for producing the adhesive is not particularly limited, and the adhesive can be obtained by a conventionally known polymerization method such as solution polymerization and UV polymerization.
[0209] The adhesive composition may also contain a crosslinking agent for crosslinking the adhesive. That is, the adhesive may be crosslinked. Examples of the crosslinking agent include aziridine-based crosslinking agents, metal chelate-based crosslinking agents, epoxy-based crosslinking agents, and isocyanate-based crosslinking agents.
[0210] In the adhesive composition, the content of the crosslinking agent is not particularly limited, for example, relative to 100 parts by mass of the adhesive, it is 0.1 parts by mass or more and 10 parts by mass or less. When it is 0.1 parts by mass or more, there is a tendency that the shape retention is not easy to become low. In addition, when it is 10 parts by mass or less, there is a tendency that it is easy to exert high adhesive force.
[0211] The adhesive composition may contain other additives such as organic solvents, inhibitors for inhibiting the progress of crosslinking, tackifying resins (tackifiers), ultraviolet (UV) absorbers, light stabilizers (HALS), antioxidants, infrared absorbers, dyes, pigments, etc.
[0212] <<Adhesive Sheet>>
[0213] The pressure-sensitive adhesive sheet includes a pressure-sensitive adhesive layer comprising a pressure-sensitive adhesive composition.
[0214] As described above, the temperature-sensitive light-adjusting liquid stack of Patent Document 1 requires a dedicated structure for maintaining the shape of the temperature-sensitive light-adjusting liquid. Therefore, when installing it in an already installed window or roof, a large-scale project such as replacing the window together is required, which makes it difficult to introduce.
[0215] In contrast, a pressure-sensitive adhesive sheet has the following advantages: it does not require a dedicated structure for maintaining its shape, can be easily installed by simply sticking it to an already installed window or roof, and can easily be given a function of autonomously changing the white turbidity according to the temperature.
[0216] The thickness of the adhesive layer is not particularly limited, but is preferably 5 μm or more and 1 mm or less, and more preferably 10 μm or more and 100 μm or less. In addition, the thicker the adhesive layer, the more likely it is that a dimming function will be exhibited by adding a small amount of temperature-sensitive cross-linked particles. The thinner the thickness, the more likely it is that a large amount of temperature-sensitive cross-linked particles need to be added in order to exhibit the dimming function.
[0217] The difference between the haze value of the adhesive layer at 23° C. and the haze value at 60° C. is preferably 10% or more. In particular, the haze value of the adhesive layer at 60° C. is more preferably 10% or more higher than the haze value at 23° C. This tends to make it easier to visually recognize the change in white turbidity due to temperature.
[0218] The haze value of the adhesive layer at 23°C is preferably 10% or less. The lower limit of the haze value at 23°C is not particularly limited. In addition, the haze value of the adhesive layer at 60°C is preferably 12% or more, more preferably 20% or more, and further preferably 30% or more. The upper limit of the haze value at 60°C is not particularly limited, for example, 70% or less, 50% or less.
[0219] The difference between the solar transmittance at 23° C. and the solar transmittance at 60° C. of the adhesive layer is preferably 10% or more. The solar transmittance at 60° C. of the adhesive layer is preferably 10% or more lower than the solar transmittance at 23° C.
[0220] The solar transmittance of the adhesive layer at 23°C is preferably 50% or more, more preferably 70% or more, and further preferably 80% or more. The upper limit of the solar transmittance at 23°C is not particularly limited, and is, for example, 99% or less, 95% or less. In addition, the solar transmittance of the adhesive layer at 60°C is preferably 80% or less, more preferably 70% or less, and further preferably 60% or less. The lower limit of the solar transmittance at 60°C is not particularly limited.
[0221] The adhesive sheet may also include a substrate sheet. The substrate constituting the substrate sheet is not particularly limited as long as it is a light-transmitting substrate. As the substrate, for example, corona-treated PET, untreated PET, highly transparent PET, annealed PET, UV-cut PET, heat-insulating PET, anti-fog PET, hard-coated PET, sandblasted PET, and other PETs; transparent PI, etc. can be used.
[0222] The adhesive layer may be formed on only one side of the substrate sheet or on both sides. Alternatively, an adhesive layer may be formed on one side of the substrate sheet and an adhesive layer not meeting the above description may be formed on the other side.
[0223] Similar to the substrate sheet, a release sheet may be laminated on the surface of the adhesive layer.
[0224] The adhesive sheet can be produced using the above-mentioned adhesive composition by a common method. For example, a coating solution prepared by adding a solvent or a crosslinking agent to the adhesive composition as needed is applied to a substrate sheet by a coater, and then dried by heating to form an adhesive layer.
[0225] As the coater, for example, a knife coater, a roll coater, a calendar coater, a comma coater, etc. can be mentioned. In addition, depending on the coating thickness or the viscosity of the coating liquid, a gravure coater, a rod coater, etc. can also be mentioned.
[0226] Example
[0227] Hereinafter, the present invention will be described in more detail with reference to Examples, but the scope of the present invention is not limited to these Examples.
[0228] Hereinafter, various chemicals used in the examples will be collectively described.
[0229] SA: BLEMMER SA (octadecyl acrylate) manufactured by NOF Corporation
[0230] CA: BLEMMER CA (hexadecyl acrylate) manufactured by NOF Corporation
[0231] VA: BLEMMER VA (behenyl acrylate) manufactured by NOF Corporation
[0232] A-HD-N: A-HD-N (1,6-hexanediol diacrylate) manufactured by Shin-Nakamura Chemical Industry Co., Ltd.
[0233] EHA: 2-Ethylhexyl acrylate manufactured by Toagosei Co., Ltd.
[0234] C1A: Methyl acrylate manufactured by Nippon Shokubai Co., Ltd.
[0235] AA: Acrylic acid manufactured by Nippon Shokubai Co., Ltd.
[0236] A-LEN-10: A-LEN-10 manufactured by Shin-Nakamura Chemical Industry Co., Ltd. (2-(o-phenylphenoxy)ethyl acrylate)
[0237] HEA: 2-Hydroxyethyl acrylate manufactured by Nippon Shokubai Co., Ltd.
[0238] NF-13: HITENOL NF-13 manufactured by Daiichi Kogyo Seiyaku Co., Ltd.
[0239] PEROYL L: PEROYL L (dilauroyl peroxide) manufactured by NOF Corporation
[0240] PERBUTYL ND: PERBUTYL ND (tert-butyl peroxyneodecanoate) manufactured by NOF Corporation
[0241] PERHEXYL PV: PERHEXYL PV (tert-hexyl peroxypivalate) manufactured by NOF Corporation
[0242] L45: CORONET L-45 manufactured by Tosoh Corporation (isocyanate crosslinking agent)
[0243] [Manufacturing of Thermosensitive Cross-linked Microparticles]
[0244] The side chain crystalline monomer, the multifunctional monomer and the initiator are added to the reaction container in the proportion shown in Table 1. The mixture in the reaction container is stirred with a scraper to make it uniformly mixed. Then, an aqueous medium and an emulsifier in the proportion shown in Table 1 are added to the reaction container to obtain a mixed solution. Water is used as an aqueous medium. The aqueous medium is added in a manner that the ratio of the mass of the side chain crystalline monomer to the total mass of the side chain crystalline monomer and the mass of the aqueous medium in the mixed solution is 40% by mass. Furthermore, the mixed solution is stirred at 7500 rpm for 5 minutes using a homogenizer manufactured by IKA (main body: T 25digitalULTRA-TURRAX, shaft generator: S25N-25F) to make the monomer component granular. Finally, nitrogen is introduced into the mixed solution for bubbling, and after removing the air (oxygen) in the mixed solution, it is heated and stirred at 67°C for 2 hours and at 80°C for 2 hours to polymerize the monomer component. Then, the aqueous medium was removed from the produced fine particles by suction filtration and vacuum drying, thereby obtaining thermosensitive crosslinked fine particles 1 .
[0245] Thermosensitive crosslinked fine particles 2 were obtained in the same manner as the method for producing the thermosensitive crosslinked fine particles 1, except that the mixed solution was stirred at 14,000 rpm for 5 minutes using a homogenizer.
[0246] Thermosensitive crosslinked fine particles 3 were obtained in the same manner as in the method for producing the thermosensitive crosslinked fine particles 1, except that the mixed solution was stirred at 5,600 rpm for 3 minutes using a homogenizer.
[0247] Thermosensitive crosslinked fine particles 4 were obtained in the same manner as in the method for producing the thermosensitive crosslinked fine particles 1, except that the mixed solution was stirred at 4200 rpm for 5 minutes using a homogenizer.
[0248] (Average particle size and D90 particle size of the temperature-sensitive cross-linked microparticles)
[0249] The particle size distribution of the thermosensitive crosslinked microparticles was measured using a laser diffraction particle size distribution meter "Mastersizer 3000" manufactured by Malvern. In the particle size distribution, the particle size corresponding to 50% of the cumulative volume frequency calculated from the smaller particle size of the thermosensitive crosslinked microparticles was defined as the "average particle size", and the particle size corresponding to 90% of the cumulative volume frequency was defined as the "D90 particle size". The results are shown in Table 1.
[0250] (Melting point of the temperature-sensitive cross-linked microparticles)
[0251] The melting point of the thermosensitive crosslinked fine particles was measured from the temperature of the endothermic peak top when measuring in the range of -30 to 100° C. at a scanning rate of 10° C. / min using a DSC (differential scanning calorimeter) manufactured by Seiko Instruments.
[0252] [Table 1]
[0253]
[0254] [Manufacture of adhesive]
[0255] (BR1)
[0256] The monomers were added to the reaction container in the proportions shown in Table 2. A solvent (ethyl acetate / toluene = 70 / 30 (mass ratio)) was added to the reaction container to dilute the monomers in such a manner that the monomer concentration became 33% by mass. Next, nitrogen was introduced into the monomer dilution for bubbling while the monomer dilution was stirred and heated. At the time point when the liquid temperature reached 55°C, an initiator was added to the monomer dilution in the proportions shown in Table 2. Furthermore, after heating and stirring the liquid in the reaction container at 55°C for 4 hours, the temperature of the oil bath was increased to 80°C. At the time point when the liquid temperature exceeded 70°C, an accelerator was added to the reaction solution in the proportions shown in Table 2. Finally, the mixture was heated and stirred at 80°C for 2 hours to obtain an adhesive (BR1).
[0257] (BR2)
[0258] Adhesive (BR2) was obtained in the same manner as Adhesive (BR1) except that the monomers were charged into the reaction container at the ratio shown in Table 2 and a solvent (ethyl acetate / methyl ethyl ketone=90 / 10 (mass ratio)) was added to dilute the monomers so that the monomer concentration became 38 mass %.
[0259] (Weight average molecular weight of binder)
[0260] The results are shown in Table 2.
[0261] (Glass transition temperature of adhesive)
[0262] Using a dynamic viscoelasticity measuring device "HAAKEMARS III" manufactured by Thermo Scientific, tanδ (loss tangent) was measured at 20 Hz, 5°C / min, and in a temperature rise process from -100 to 100°C. The glass transition temperature (Tg) was determined from the obtained tanδ peak temperature. The results are shown in Table 2.
[0263] [Table 2]
[0264]
[0265] [Manufacturing of Thermosensitive Non-crosslinked Polymers]
[0266] The monomer and the chain transfer agent were added to the reaction vessel in the ratio shown in Table 3. The solvent (toluene) was added to the reaction vessel to dilute the monomer in such a manner that the monomer concentration became 50% by mass. Then, nitrogen was introduced into the monomer dilution for bubbling while the monomer dilution was stirred and heated. At the time point when the liquid temperature reached 80°C, an initiator was added to the monomer dilution in the ratio shown in Table 3. Furthermore, the mixture was heated and stirred at 80°C for 3 hours to obtain a temperature-sensitive non-crosslinked polymer.
[0267] (Weight average molecular weight of the temperature-sensitive non-crosslinked polymer)
[0268] The weight average molecular weight was measured by the same method as that of the binder. The results are shown in Table 3.
[0269] (Melting point of temperature-sensitive non-crosslinked polymer)
[0270] The melting point of the thermosensitive crosslinked fine particles was measured by the same method as that of the thermosensitive crosslinked fine particles.
[0271] [Table 3]
[0272]
[0273] [Manufacturing of adhesive sheet]
[0274] Thermosensitive cross-linked microparticles were added to the obtained adhesive in the proportions shown in Tables 4 to 6. A solvent (ethyl acetate) was added to the mixture of the adhesive and the thermosensitive cross-linked microparticles to adjust the solid content concentration of the mixture to 30% by mass. A thermosensitive non-cross-linked polymer was added to the adjusted mixture in the proportions shown in Tables 4 to 6 to obtain an adhesive composition. A cross-linking agent was added to the adhesive composition in the proportions shown in Tables 4 to 6. The adhesive composition was applied to the corona-treated surface of a PET film (thickness 100 μm) using a rod coater. Thereafter, the PET film was heated and dried at 110° C. in a hot air circulation oven for 3 minutes to obtain an adhesive sheet (Examples 1 to 8) having an adhesive layer (thickness 40 μm) including a cross-linked adhesive composition.
[0275] (Refractive index of temperature-sensitive cross-linked microparticles and binder)
[0276] The refractive index of the obtained temperature-sensitive crosslinked fine particles and the binder at 23° C. and 60° C. was measured using an automatic refractometer “Abbemat 350” manufactured by Anton Paar. The results are shown in Tables 4 to 6.
[0277] (Haze value of adhesive layer)
[0278] The haze values of the adhesive layer of the obtained adhesive sheet at 23°C, 40°C and 60°C were measured using a spectrophotometer "CM3600" (light source C) manufactured by Konica Minolta (Co., Ltd.) in accordance with ASTM D1003. The adhesive sheet was bonded to the ITO glass surface and measured using ITO glass as a reference. The results are shown in Tables 4 to 6.
[0279] (Peel Strength)
[0280] For the obtained adhesive sheet, the 180° peel strength relative to stainless steel (SUS) at 23°C and 60°C was measured in accordance with JIS Z0237. Specifically, the adhesive sheet was bonded to SUS and left to stand for 20 minutes, and then 180° peeling was performed at a speed of 300 mm / min using a load cell. Plate-shaped SUS304 was used for SUS. The bonding of the adhesive sheet to SUS was performed by reciprocating a 2kg roller 5 times on the adhesive sheet. The results are shown in Tables 4 to 6.
[0281] In addition, the peel strength of the PSA sheet was also measured at temperatures between 23°C and 60°C, and the change in the adhesive strength reduction rate, which is the amount of adhesive strength reduction per 1°C of the PSA sheet, was confirmed. As a result, it was confirmed that the adhesive strength reduction rate near 49°C, which is the melting point of the temperature-sensitive non-crosslinked polymer, was greater than the adhesive strength reduction rate in temperature regions other than the melting point of the temperature-sensitive non-crosslinked polymer.
[0282] (Solar transmittance)
[0283] For the obtained adhesive sheet, the solar transmittance at 23°C, 40°C and 60°C was measured using a spectrophotometer "V770DS" manufactured by JASCO Corporation in accordance with 6.5 of JIS A5759:2016. However, in order to heat to 40°C and 60°C for measurement, an ITO glass ("GMT-100-12" manufactured by GEOMATEC) with a thickness of 1.1 mm was used as the object to which the adhesive sheet was attached. Specifically, a test piece was prepared by attaching the adhesive sheet to a single surface of the ITO glass. At 23°C, 40°C and 60°C (the surface temperature of the ITO glass measured by a contact thermometer), the glass surface of the test piece was directed toward the light source, and the spectral transmittance of each wavelength of 300 to 2500 nm was measured using a spectrophotometer. As specified in JIS A5759:2016, the solar transmittance was calculated based on the relative spectral distribution of sunlight. The results are shown in Tables 5 and 6.
[0284] (Thermal insulation)
[0285] For the obtained adhesive sheet, Figure 5 to Figure 7 The thermal insulation was evaluated as shown. Specifically, an adhesive sheet 1 was attached to a glass plate 2 to prepare a test piece. The test piece was placed as the top surface on a wooden frame 4 with a width of 120 mm, a depth of 200 mm, and a height of 100 mm in a manner that the adhesive sheet surface was facing upward. A thermometer (thermocouple) 3 was set at a position 10 mm below the glass surface. As a windshield, the side and bottom of the wooden frame 4 were covered with a polyethylene sheet. The wooden frame 4 on which the test piece was placed was set on a metal frame 5 at a height of 1000 mm from the ground 6. The temperature rise value of the thermocouple 3 during sunlight exposure (sun exposure time: about 360 minutes, average temperature: 32°C) was recorded. The temperature rise value was recorded in the same way as the test piece of the glass plate to which the adhesive sheet was not attached as a blank. The difference in temperature rise value with the blank was calculated. The results are shown in Tables 5 and 6.
[0286] [Table 4]
[0287]
[0288] As is clear from Table 4, according to Examples 1 and 2, the adhesive layers of Examples 1 and 2 having the aforementioned prescribed configuration can autonomously change the white turbidity according to the temperature. In addition, it can be seen that the adhesive force decreases by increasing the temperature. Therefore, it can be seen from Examples 1 and 2 that the window material or the light-transmitting roof material having the above-mentioned adhesive layer can autonomously change the white turbidity according to the temperature, and the adhesive layer can be peeled off and reconfigured, so the manufacturing is easy.
[0289] [Table 5]
[0290]
[0291] [Table 6]
[0292]
[0293] Description of Reference Numerals
[0294] 10First Window Material
[0295] 11 light-transmitting substrate layer
[0296] 12 adhesive layer
[0297] 12a Thermosensitive cross-linked microparticles
[0298] 13 substrate sheet
[0299] 20 Second window material
[0300] 21a, 21b light-transmitting base material layer
[0301] 22 adhesive layer
[0302] 22a Thermosensitive cross-linked microparticles
[0303] 30Translucent roofing materials
[0304] 31 light-transmitting substrate layer
[0305] 32 adhesive layers
[0306] 32a Thermosensitive cross-linked microparticles
[0307] 33 substrate sheets.
Claims
1. A window material, characterized in that: It comprises at least one light-transmitting substrate layer and at least one adhesive layer, The adhesive layer includes an adhesive composition containing 1 to 20 parts by mass of a temperature-sensitive non-crosslinked polymer and 1 to 100 parts by mass of temperature-sensitive crosslinked fine particles relative to 100 parts by mass of an adhesive. The refractive index of the thermosensitive cross-linked microparticles decreases as the temperature increases, and The amount of refractive index reduction per 1°C, that is, the refractive index reduction rate of the temperature-sensitive crosslinked fine particles is greater near the melting point of the temperature-sensitive crosslinked fine particles than in a temperature range other than near the melting point of the temperature-sensitive crosslinked fine particles. The adhesive force of the adhesive composition decreases with increasing temperature, and The amount of adhesive strength reduction per 1° C., that is, the adhesive strength reduction rate of the adhesive composition is greater near the melting point of the temperature-sensitive non-crosslinked polymer than in a temperature range other than near the melting point of the temperature-sensitive non-crosslinked polymer.
2. The window material according to claim 1, wherein The difference between the haze value of the adhesive layer at 23° C. and the haze value of the adhesive layer at 60° C. is 10% or more, The adhesive force of the adhesive composition is 1 N / 25 mm or more at 23° C. and 0.1 N / mm or less at 60° C.
3. The window material according to claim 1 or 2, wherein: The melting point of the temperature-sensitive non-cross-linked polymer is higher than the melting point of the temperature-sensitive cross-linked fine particles by 5° C. or more.
4. The window material according to any one of claims 1 to 3, wherein: The thermosensitive non-crosslinked polymer comprises a side chain crystalline polymer A, The side chain crystalline polymer A contains 70 to 100% by mass of a constituent unit derived from a (meth)acrylic acid monomer having a linear alkyl group having 14 or more carbon atoms, The thermosensitive cross-linked microparticles include a side chain crystalline polymer B, The side chain crystalline polymer B contains 70 to 100% by mass of a structural unit derived from a (meth)acrylic monomer having a linear alkyl group having 14 or more carbon atoms.
5. A light-transmitting roof material, characterized in that: It comprises at least one light-transmitting substrate layer and at least one adhesive layer, The adhesive layer includes an adhesive composition containing 1 to 20 parts by mass of a temperature-sensitive non-crosslinked polymer and 1 to 100 parts by mass of temperature-sensitive crosslinked fine particles relative to 100 parts by mass of an adhesive. The refractive index of the thermosensitive cross-linked microparticles decreases as the temperature increases, and The amount of refractive index reduction per 1°C, that is, the refractive index reduction rate of the temperature-sensitive crosslinked fine particles is greater near the melting point of the temperature-sensitive crosslinked fine particles than in a temperature range other than near the melting point of the temperature-sensitive crosslinked fine particles. The adhesive force of the adhesive composition decreases with increasing temperature, and The amount of adhesive strength reduction per 1° C., that is, the adhesive strength reduction rate of the adhesive composition is greater near the melting point of the temperature-sensitive non-crosslinked polymer than in a temperature range other than near the melting point of the temperature-sensitive non-crosslinked polymer.
6. The light-transmitting roofing material according to claim 5, wherein: The difference between the haze value of the adhesive layer at 23° C. and the haze value of the adhesive layer at 60° C. is 10% or more, The adhesive force of the adhesive composition is 1 N / 25 mm or more at 23° C. and 0.1 N / mm or less at 60° C.
7. The light-transmitting roofing material according to claim 5 or 6, wherein: The melting point of the temperature-sensitive non-cross-linked polymer is higher than the melting point of the temperature-sensitive cross-linked fine particles by 5° C. or more.
8. The light-transmitting roofing material according to any one of claims 5 to 7, wherein: The thermosensitive non-crosslinked polymer comprises a side chain crystalline polymer A, The side chain crystalline polymer A contains 70 to 100% by mass of a constituent unit derived from a (meth)acrylic acid monomer having a linear alkyl group having 14 or more carbon atoms, The thermosensitive cross-linked microparticles include a side chain crystalline polymer B, The side chain crystalline polymer B contains 70 to 100% by mass of a structural unit derived from a (meth)acrylic monomer having a linear alkyl group having 14 or more carbon atoms.
9. A building, characterized in that: A window material according to any one of claims 1 to 4 and / or a light-transmitting roof material according to any one of claims 5 to 8.
10. A vehicle, a vessel or an aircraft, characterized in that: A window material according to any one of claims 1 to 4 and / or a light-transmitting roof material according to any one of claims 5 to 8.
11. An adhesive composition comprising 1 to 20 parts by mass of a temperature-sensitive non-crosslinked polymer and 1 to 100 parts by mass of temperature-sensitive crosslinked fine particles relative to 100 parts by mass of an adhesive, characterized in that: The refractive index of the thermosensitive cross-linked microparticles decreases as the temperature increases, and The amount of refractive index reduction per 1°C, that is, the refractive index reduction rate of the temperature-sensitive crosslinked fine particles is greater near the melting point of the temperature-sensitive crosslinked fine particles than in a temperature range other than near the melting point of the temperature-sensitive crosslinked fine particles. The adhesive force of the adhesive composition decreases with increasing temperature, and The amount of adhesive strength reduction per 1° C., that is, the adhesive strength reduction rate of the adhesive composition is greater near the melting point of the temperature-sensitive non-crosslinked polymer than in a temperature range other than near the melting point of the temperature-sensitive non-crosslinked polymer.
12. The adhesive composition according to claim 11, wherein The adhesive force is 1 N / 25 mm or more at 23°C and 0.1 N / mm or less at 60°C.
13. The adhesive composition according to claim 11 or 12, wherein The melting point of the temperature-sensitive non-cross-linked polymer is higher than the melting point of the temperature-sensitive cross-linked fine particles by 5° C. or more.
14. The adhesive composition according to claim 11 or 12, wherein The difference between the melting point of the temperature-sensitive non-cross-linked polymer and the melting point of the temperature-sensitive cross-linked microparticles is less than 5°C.
15. The adhesive composition according to any one of claims 11 to 14, wherein The thermosensitive non-crosslinked polymer comprises a side chain crystalline polymer A, The side chain crystalline polymer A contains 70 to 100% by mass of a constituent unit derived from a (meth)acrylic acid monomer having a linear alkyl group having 14 or more carbon atoms, The thermosensitive cross-linked microparticles include a side chain crystalline polymer B, The side chain crystalline polymer B contains 70 to 100% by mass of a structural unit derived from a (meth)acrylic monomer having a linear alkyl group having 14 or more carbon atoms.
16. An adhesive sheet, characterized in that: A pressure-sensitive adhesive layer comprising the pressure-sensitive adhesive composition according to any one of claims 11 to 15 is provided.
17. The adhesive sheet according to claim 16, wherein A difference between a haze value of the adhesive layer at 23° C. and a haze value of the adhesive layer at 60° C. is 10% or more.