Ultrasonic surgical scalpel, device, equipment and system and machining method of scalpel head of ultrasonic surgical scalpel

By forming a material layer with varying component content gradient on the ultrasonic cutting head, the problem of easy falling off of traditional coatings is solved, adhesion and wear resistance are improved, and the reliability and surgical efficiency of the cutting head are enhanced.

CN118948383APending Publication Date: 2024-11-15WUHAN DRAGONBIO ORTHOPEDIC PROD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310522736.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-06
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The surface coating of traditional ultrasonic cutting heads is prone to fall off under high-frequency vibration conditions, resulting in poor adhesion and affecting product reliability and surgical efficiency.

Method used

A first material layer with a gradient of component content is formed on the cutting head substrate, the first component is used to enhance binding force, and the second component is used to reduce surface energy, ensuring the hydrophobicity and anti-adhesion effect of the surface layer.

Benefits of technology

It improves the adhesion and wear resistance of the coating, reduces impedance, and enhances the reliability and surgical efficiency of the cutting head.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118948383A_ABST
    Figure CN118948383A_ABST
Patent Text Reader

Abstract

The invention discloses an ultrasonic surgical scalpel, device, equipment and system and a machining method of a scalpel head of the ultrasonic surgical scalpel. The ultrasonic surgical scalpel comprises the scalpel head and a waveguide rod. The tool bit comprises a base body and a first material layer formed on the base body, the first material layer is provided with a first side attached to the base body and a second side deviating from the base body from inside to outside, the first material layer comprises a surface layer, and the surface of the surface layer is used for making contact with a tissue object. Wherein the first material layer comprises a first component and a second component, the first component is used for improving the binding force of the first material layer and the base body, the second component is used for reducing the surface energy of the first material layer, in the surface layer, the content of the first component is gradually reduced from inside to outside, and the content of the second component is gradually increased from inside to outside. Through gradient change setting of the contents of the first component and the second component of the first material layer, the problem of poor adhesion is solved, and the surface of the first material layer has the characteristics of low friction coefficient, low surface energy, tissue adhesion resistance and the like while the adhesion is maintained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of medical devices, and in particular to a method for processing a blade of an ultrasonic surgical scalpel, device, equipment, system, and a blade head thereof. Background Art

[0002] Ultrasonic scalpel is a tool for ultrasonic treatment. It has the advantages of high cutting accuracy, less bleeding and less thermal damage, and is widely used in surgical operations. The application principle of ultrasonic scalpel is to convert electrical energy into mechanical vibration through the transducer, and transmit the vibration to the blade through the guide rod, so that the blade produces mechanical oscillation, which has the effect of cutting and coagulating animal or human tissue.

[0003] In traditional technology, there are several treatment options for the ultrasonic knife head:

[0004] In the first solution, the surface of the blade is mechanically polished or sandblasted without coating. During clinical use, this solution causes severe tissue adhesion on the blade, leading to secondary bleeding after coagulation, which seriously affects the doctor's surgical efficiency.

[0005] The second solution is to process two or more layers of coating on the surface of the blade. Since the non-metallic element coating with a low friction coefficient cannot be effectively attached to the metal substrate of the ultrasonic knife itself through spraying, even if it is attached, it cannot cope with the use scenarios under the high-frequency vibration conditions of the ultrasonic knife, and it is difficult to avoid the problem of rapid falling off.

[0006] In traditional processes, the wear resistance of the coating is often sacrificed to ensure the anti-adhesion effect of the coating. In order to improve the wear resistance of the coating, the coating thickness needs to be increased, which leads to a decrease in the adhesion of the coating and the coating is prone to large-scale shedding. Thicker coatings will also increase the impedance of the ultrasonic knife, causing the transducer to heat up and reduce product reliability. Summary of the invention

[0007] In view of this, the present application proposes a method for processing an ultrasonic surgical scalpel, device, equipment, system and its blade head.

[0008] A first aspect of the present application provides an ultrasonic surgical scalpel, comprising a cutter head that directly acts on a tissue object and a waveguide rod for transmitting vibration to the cutter head, wherein the cutter head comprises:

[0009] A substrate having a proximal end and a distal end, wherein the proximal end of the substrate is connected to the waveguide rod, and the substrate is used to receive the ultrasonic vibration transmitted from the waveguide rod, so that the cutter head can operate and process the tissue object based on the received ultrasonic vibration;

[0010] A first material layer is formed on the substrate, wherein the first material layer has a first side that is in contact with the substrate and a second side that is away from the substrate from the inside to the outside, and the first material layer includes a surface layer, and a surface of the surface layer is used to contact the tissue object;

[0011] Among them, the first material layer has a first component and a second component, the first component is used to improve the bonding strength between the first material layer and the substrate, and the second component is used to reduce the surface energy of the first material layer. In the surface layer, the content of the first component gradually decreases from the inside to the outside, and the content of the second component gradually increases from the inside to the outside.

[0012] A second aspect of the present application provides an ultrasonic surgical scalpel, comprising a cutter head that directly acts on a tissue object and a waveguide rod for transmitting vibration to the cutter head, wherein the cutter head comprises:

[0013] A substrate having a proximal end and a distal end, wherein the proximal end of the substrate is connected to the waveguide rod, and the substrate is used to receive the ultrasonic vibration transmitted from the waveguide rod, so that the cutter head can operate and process the tissue object based on the received ultrasonic vibration;

[0014] A first material layer formed on the substrate, wherein the first material layer has a first side in contact with the substrate and a second side facing away from the substrate from the inside to the outside;

[0015] Wherein, the first material layer comprises a first component and a second component, the first component is used to enhance the bonding force between the first material layer and the substrate, and the second component is used to reduce the surface energy of the first material layer;

[0016] Near the first side, the content of the first component is greater than the content of the second component, near the second side, the content of the second component is greater than the content of the first component, and\or, the content of the first component at the first side is greater than the content of the first component at the second side, and\or, the content of the second component at the second side is greater than the content of the second component at the first side.

[0017] The third aspect of the present application provides a method for processing a blade head of an ultrasonic surgical scalpel, comprising:

[0018] Pre-treatment: performing surface pre-treatment on the base of the tool head to increase at least one parameter of the base's surface roughness, surface energy, and bonding area with the material to be processed;

[0019] Selecting a material to be processed to process the substrate to form a first material layer on the substrate, wherein the first material layer has a first side in contact with the substrate and a second side away from the substrate from the inside to the outside, and the material to be processed includes a first material and a second material, wherein the first material contains a first component for improving the bonding force between the first material layer and the substrate, and the second material contains a second component for reducing the surface energy of the first material layer;

[0020] In the process of forming the first material layer, the concentration of the first material and / or the concentration of the second material is adjusted so that the content of the first component is greater than the content of the second component at the first side of the first material layer, and the content of the second component is greater than the content of the first component at the second side of the first material layer, and / or so that in the first material layer, the content of the first component at the first side is greater than the content of the first component at the second side, and / or so that in the first material layer, the content of the second component at the second side is greater than the content of the second component at the first side.

[0021] A fourth aspect of the present application provides an ultrasonic surgical device, comprising:

[0022] A hand piece for holding;

[0023] A clamping assembly, including a clamping member;

[0024] In the ultrasonic surgical scalpel mentioned above, the blade head is mounted on the clamping assembly through the waveguide rod, and the clamping assembly is used to control one of the clamping members to cooperate with the blade head to clamp or release the tissue object.

[0025] A fifth aspect of the present application provides an ultrasonic surgical device, characterized in that it includes:

[0026] The ultrasonic surgical device as described above;

[0027] The ultrasonic transducer is connected to the handpiece, and is used for receiving external electrical signals and converting the electrical signals into mechanical vibrations in the ultrasonic frequency band, and transmitting the mechanical vibrations to the ultrasonic surgical scalpel.

[0028] A sixth aspect of the present application provides an ultrasonic surgical system, comprising:

[0029] Host;

[0030] The ultrasonic surgical device is connected to the host, and is used to receive the electrical signal sent by the host and generate ultrasonic vibration to operate and process the tissue object.

[0031] From the above technical scheme, it can be seen that the ultrasonic surgical scalpel proposed in the first aspect of the present application forms a first material layer with a component content having a regional gradient change on the base of the blade head. In the surface layer, the content of the first component gradually decreases from the inside to the outside, that is, the content of the first component on the side close to the base in the surface layer is greater than that on the side away from the base, which can improve the bonding force between the first material layer and the base, thereby improving the adhesion of the first material layer as a whole. In the surface layer, the content of the second component gradually increases from the inside to the outside, so that the second component content on the second side of the first material layer in contact with the tissue object is relatively high, so as to reduce the surface energy of the first material layer, thereby making the surface of the first material layer relatively hydrophobic and having a good anti-tissue adhesion effect. The ultrasonic surgical scalpel of the present application, through the gradient change setting of the first component and the second component content of the first material layer, not only solves the problem of poor adhesion, but also has the characteristics of low friction coefficient, low surface energy, anti-tissue adhesion, etc. on the surface of the first material layer while maintaining adhesion. Compared with the existing coating or plating, it has stronger adhesion and better wear resistance, meeting the requirements of multiple use of the product. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained like these drawings without paying any creative work.

[0033] Figure 1 is a schematic diagram of the structure of the ultrasonic surgical scalpel proposed in an embodiment of the present application;

[0034] Figure 2 yes Figure 1 A partial enlarged schematic diagram of the middle cutter head;

[0035] Figure 3 is a cross-sectional schematic diagram of a cutter head proposed in an embodiment of the present application;

[0036] Figure 4 is a partial schematic diagram of the cutting surface of the coating of the ultrasonic surgical scalpel proposed in an embodiment of the present application;

[0037] Figure 5 is a schematic diagram of the structure of an ultrasonic surgical device proposed in an embodiment of the present application;

[0038] Figure 6 is a schematic diagram of the structure of an ultrasonic surgical device proposed in an embodiment of the present application;

[0039] Figure 7 It is a schematic diagram of the structure of the ultrasonic surgical system proposed in the embodiment of the present application.

[0040] Description of the accompanying drawings:

[0041] 10. Ultrasonic surgical scalpel;

[0042] 11, blade head; 11a, blood coagulation cutting surface; 11b, auxiliary surface; 11c, back cutting surface; 111, base; 112, first material layer; 1121, first side; 1122, second side; 113, second material layer;

[0043] 12. Waveguide rod;

[0044] 100. Ultrasonic surgical device;

[0045] 20. Hand piece; 21. Handle; 22. Trigger; 30. Clamping assembly; 31. Clamping piece;

[0046] 1000. Ultrasonic surgical equipment; 200. Ultrasonic transducer;

[0047] 10000. Ultrasonic surgical system; 2000. Host. DETAILED DESCRIPTION

[0048] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.

[0049] It should also be understood that the terms used in this application specification are only for the purpose of describing specific embodiments and are not intended to limit the application. As used in this application specification and the appended claims, unless the context clearly indicates otherwise, the singular forms "a", "an" and "the" are intended to include plural forms.

[0050] It should be further understood that the term “and / or” used in the specification and appended claims refers to any combination and all possible combinations of one or more of the associated listed items, and includes these combinations.

[0051] See also Figure 1-Figure 3As shown, an embodiment of the present application provides an ultrasonic surgical scalpel 10, including a blade head 11 that directly acts on a tissue object and a waveguide rod 12 for transmitting vibration to the blade head 11. The blade head 11 includes a substrate 111 and a first material layer 112. The substrate 111 can be made of metal material. The substrate 111 has a proximal end and a distal end. The proximal end of the substrate 111 is connected to the waveguide rod 12 and can be bent away from the waveguide rod 12 in the longitudinal direction and extend to the distal end. The substrate 111 is used to receive the ultrasonic vibration transmitted from the waveguide rod 12, so that the blade head 11 can operate and process the tissue object based on the received ultrasonic vibration.

[0052] The first material layer 112 is formed on the base 111. The first material layer 112 has a first side 1121 that is in contact with the base 111 and a second side 1122 that is away from the base 111 from the inside to the outside. The first material layer 112 includes a surface layer, and the surface of the surface layer is used to contact the tissue object. Exemplarily, the surface layer can be the entire first material layer 112, or it can be a region of the first material layer 112 close to the second side 1122.

[0053] Among them, the first material layer 112 has a first component and a second component. The first component is used to enhance the bonding force between the first material layer 112 and the substrate 111, and the second component is used to reduce the surface energy of the first material layer 112. In the surface layer, the content of the first component gradually decreases from the inside to the outside, and the content of the second component gradually increases from the inside to the outside.

[0054] The ultrasonic surgical scalpel 10 proposed in the embodiment of the present application has a first material layer 112 with a component content having a regional gradient change formed on the base 111 of the blade head 11. In the surface layer, the content of the first component gradually decreases from the inside to the outside, that is, in the surface layer, the content of the first component on the side close to the base 111 is greater than the side away from the base 111, which can improve the bonding force between the first material layer 112 and the base 111, thereby improving the overall adhesion of the first material layer 112. In the surface layer, the content of the second component gradually increases from the inside to the outside, so that the second side 1122 of the first material layer 112 in contact with the tissue object has a higher content of the second component, so as to reduce the surface energy of the first material layer 112, so that the hydrophobicity of the surface of the first material layer 112 is relatively high, and the anti-tissue adhesion effect is good. The ultrasonic surgical scalpel of the present application not only solves the problem of poor adhesion by setting the gradient change of the content of the first component and the second component of the first material layer 112, but also has the characteristics of low friction coefficient, low surface energy, and anti-tissue adhesion on the surface of the first material layer 112 while maintaining adhesion. Compared with existing coatings or platings, it has stronger adhesion and better wear resistance, and meets the requirements for multiple uses of the product.

[0055] In some embodiments, the content of the first component is greater than the content of the second component on the side of the surface layer close to the substrate 111. In this embodiment, this configuration can enhance the bonding force between the first material layer 112 and the substrate 111.

[0056] In some embodiments, the content of the second component is greater than the content of the first component on the side of the surface layer away from the substrate 111. In this embodiment, this arrangement can reduce the surface energy of the first material layer 112, so that the surface of the first material layer 112 has the characteristics of low friction coefficient, low surface energy, and anti-tissue adhesion.

[0057] In some embodiments, the content of the first component gradually decreases from the first side 1121 to the second side 1122. In this embodiment, the first component is used for primer, and a material containing silicon can be used to make the first material layer 112 and the substrate 111 have better bonding strength.

[0058] In some embodiments, the content of the second component gradually increases from the first side 1121 to the second side 1122. In this embodiment, the second component may be a material containing fluorine to make the surface of the first material layer 112 more hydrophobic and reduce the surface energy of the first material layer 112.

[0059] Exemplarily, the content of the first component can be set to gradually decrease from close to the first side 1121 to close to the second side 1122, showing a gradient change, so that the content of the first component close to the first side 1121 is higher to ensure the bonding force between the first material layer 112 and the substrate 111. At the same time, the content of the second component correspondingly increases from close to the first side 1121 to close to the second side 1122 to reduce the surface energy of the first material layer 112, so that the hydrophobicity of the surface of the first material layer 112 is relatively high, and the anti-tissue adhesion effect is good.

[0060] In some embodiments, the content of the first component is greater than 50% near the first side 1121. In this embodiment, the content of the first component specifically refers to the mass fraction of the first component. The content of the first component is greater than 50% near the first side 1121, which can ensure the bonding force between the first material layer 112 and the substrate 111 and improve the overall adhesion of the first material layer 112.

[0061] In some embodiments, the content of the second component is greater than 40% near the second side 1122. In this embodiment, the content of the second component specifically refers to the mass fraction of the second component. Near the second side 1122, the content of the second component is greater than 40%, which can ensure that the surface of the first material layer 112 has a lower surface energy, so that the hydrophobicity of the surface of the first material layer 112 is relatively high, and the anti-tissue adhesion effect is good.

[0062] In some embodiments, the first material layer 112 further includes a bonding layer and an intermediate layer, wherein the bonding layer is close to the first side 1121 of the first material layer 112 , the surface layer is close to the second side 1122 of the first material layer 112 , and the intermediate layer is located between the bonding layer and the surface layer.

[0063] In the bonding layer, the content of the first component is greater than that of the second component. In this embodiment, the content of the first component in the bonding layer is relatively high, which can improve the bonding force between the first material layer 112 and the substrate 111, thereby improving the overall adhesion of the first material layer 112.

[0064] Among them, in the surface layer, the content of the second component is greater than that of the first component. In this embodiment, after the first component is used to prime the bonding layer to ensure the bonding force, the content of the second component can be controlled to gradually increase from the inside to the outside, so that the content of the second component in the surface layer is relatively large, which can reduce the surface energy of the first material layer 112, thereby making the surface of the first material layer 112 relatively hydrophobic and having a good anti-tissue adhesion effect.

[0065] Exemplarily, in the embodiment of the present application, the first material layer 112 is divided into a bonding layer, an intermediate layer and a surface layer, and the area division is performed only in the thickness direction of the single-layer first material layer 112. The area close to the first side 1121 is the bonding layer, the area close to the second side 1122 is the surface layer, and the area between the first side 1121 and the second side 1122 is the intermediate layer.

[0066] Of course, in other embodiments, the above division method may not be adopted, and the first material layer 112 may be divided into a surface layer as a whole, or the first material layer 112 may be divided only into a bonding layer close to the first side 1121 and a surface layer close to the second side 1122.

[0067] In some embodiments, the intermediate layer includes a first sub-region and a second sub-region from the inside to the outside. In the first sub-region, the content of the first component gradually increases from the inside to the outside, and in the second sub-region, the content of the first component gradually decreases from the inside to the outside. In the first sub-region, the content of the second component gradually decreases from the inside to the outside, and in the second sub-region, the content of the second component gradually increases from the inside to the outside.

[0068] Alternatively, in the first sub-region, the content of the first component gradually decreases from the inside to the outside, and in the second sub-region, the content of the first component gradually increases from the inside to the outside. In the first sub-region, the content of the second component gradually increases from the inside to the outside, and in the second sub-region, the content of the second component gradually decreases from the inside to the outside.

[0069] In some other embodiments, the intermediate layer includes a first sub-region, a second sub-region and a third sub-region from the inside to the outside. In the first sub-region, the content of the first component gradually increases from the inside to the outside, in the second sub-region, the content of the first component gradually decreases from the inside to the outside, and in the third sub-region, the content of the first component gradually increases from the inside to the outside. In the first sub-region, the content of the second component gradually decreases from the inside to the outside, in the second sub-region, the content of the second component gradually increases from the inside to the outside, and in the third sub-region, the content of the second component gradually decreases from the inside to the outside.

[0070] Alternatively, in the first sub-region, the content of the first component gradually decreases from the inside to the outside, in the second sub-region, the content of the first component gradually increases from the inside to the outside, and in the third sub-region, the content of the first component gradually decreases from the inside to the outside. In the first sub-region, the content of the second component gradually increases from the inside to the outside, in the second sub-region, the content of the second component gradually decreases from the inside to the outside, and in the third sub-region, the content of the second component gradually increases from the inside to the outside.

[0071] It can be understood that the middle layer can be divided into one sub-region, two sub-regions, three sub-regions or even more. The above-mentioned sub-regions are merely different areas within the middle layer. The content of components in different areas is different, and can gradually increase or decrease. The first component and the second component in the middle layer can change uniformly or in a gradient. It is only necessary to satisfy that the content of the first component on the side close to the substrate 111 is greater than the content on the side away from the substrate 111, and the content of the second component on the side away from the substrate 111 is greater than the content on the side close to the substrate 111.

[0072] In some embodiments, the first component may be a chemical element, including (but not limited to) at least one of silicon, aluminum, titanium, tungsten, molybdenum, chromium, iron, nickel, cobalt, and magnesium. In this embodiment, the above components have good bonding strength with the substrate 111, which can ensure the adhesion of the first material layer 112.

[0073] In some embodiments, the second component may be a single chemical element or a finished compound, a pure substance or a mixture, including (but not limited to) at least one of fluorine, carbon, silicon, Teflon, and organic silicon. In this embodiment, the use of the above components can reduce the surface energy of the first material layer 112, so that the hydrophobicity of the surface of the first material layer 112 is relatively high, and the anti-tissue adhesion effect is good.

[0074] In some embodiments, the thickness a of the first material layer 112 has a value range of 5 nanometers ≤ a ≤ 0.3 millimeters. In this embodiment, the area of ​​the substrate 111 where the first material layer 112 is formed is the coagulation cutting surface 11a, which is also the front of the blade head 11 and is used to contact the tissue object. The above value range can ensure that the coagulation cutting surface 11a meets the wear resistance requirements and can control the impedance of the coagulation cutting surface 11a in a smaller range, which is conducive to ensuring the reliability of the blade head 11.

[0075] In some embodiments, the thickness a of the first material layer 112 is in the range of 5 microns ≤ a ≤ 8 microns. In the above smaller range, the coagulation cutting surface 11a of the blade head 11 can achieve a better balance between the requirements of wear resistance and impedance control, thereby producing a better final effect and being more conducive to ensuring the reliability of the blade head 11.

[0076] In some embodiments, Figure 2 and Figure 3 As shown, the surface of the substrate 111 has a first area and a second area, and the first material layer 112 is formed in the first area for contacting the tissue object. The cutting head also includes a second material layer 113 formed in the second area, and the thickness of the second material layer 113 is less than the thickness of the first material layer 112. The area on the substrate 111 where the second material layer 113 is formed is the auxiliary surface 11b, and the auxiliary surface 11b is located on the side of the coagulation cutting surface 11a, that is, the side of the cutting head 11. In this embodiment, different coating thicknesses are applied to different areas on the cutting head 11. Since the coagulation cutting surface 11a needs to be wear-resistant, while the auxiliary surfaces 11b on both sides do not need to be wear-resistant, the thickness of the second material layer 113 can be thinner than the first material layer 112 to reduce the impedance of the cutting head 11.

[0077] In some embodiments, the thickness b of the second material layer 113 is in the range of 1 nm ≤ b ≤ 0.3 mm. In this embodiment, considering that the wear resistance requirement of the auxiliary surface 11 b is lower than that of the coagulation cutting surface 11 a, the above value range can ensure that the auxiliary surface 11 b meets the wear resistance requirement and control the impedance of the auxiliary surface 11 b within a smaller range, which is conducive to ensuring the reliability of the blade 11.

[0078] In some embodiments, the thickness b of the second material layer 113 is in the range of 1 micron ≤ b ≤ 2 microns. In this embodiment, as the thickness of the second material layer 113 decreases, the impedance of the cutter head 11 can be further reduced. In the above smaller range, the auxiliary surface 11b of the cutter head 11 can achieve a better balance between meeting the wear resistance requirements and impedance control, thereby producing a better final effect and being more conducive to ensuring the reliability of the cutter head 11.

[0079] In some embodiments, Figure 3 As shown, the blade head 11 further includes a back cutting surface 11c, and the coagulation cutting surface 11a and the back cutting surface 11c are symmetrically or approximately symmetrically arranged on both sides of the central axis of the blade head 11 along the longitudinal direction.

[0080] In some embodiments, the element content of each region of the second material layer 113 may be the same or different. For example, the element content of each region of the second material layer 113 may be set with reference to the gradient change of the first material layer 112 in the above embodiment, or may be a common plating or coating with no change in element content.

[0081] In other embodiments, the first material layer 112 is provided on the coagulation cutting surface 11a of the blade head 11, and the second material layer 113 may not be provided on the auxiliary surface 11b, so that the impedance of the blade head 11 can be minimized while satisfying the functional performance of the product.

[0082] In some embodiments, the material layer is a coating or a plating. In the present embodiment, the first material layer 112 can be processed by the following techniques, such as coating, dipping, spraying, brushing, drying, melting, laser curing, UV curing, anodizing, electroplating, chemical deposition, physical vapor deposition (PVD), chemical vapor deposition (CVD), thermal spraying, thick film high-speed oxygen flame plasma and other suitable material application techniques. The present application embodiment preferably selects spraying, physical vapor deposition (PVD), and chemical vapor deposition (CVD) techniques. The coating can be completed by one or more constructions.

[0083] In some embodiments, the first material layer 112 is a coating formed by processing the material to be plated on the substrate 111 by a vacuum coating process. In this embodiment, the vacuum coating process can be ionized under vacuum and then positive and negative ions are combined to form chemical bonds with strong binding force, centrifuged into atomic particles, and impacted on the substrate 111 through an electric field, and the accumulation is very dense, so the binding force is relatively strong.

[0084] Exemplarily, vacuum coating processes include physical vapor deposition (PVD) and chemical vapor deposition (CVD). The main methods of physical vapor deposition are: vacuum evaporation, sputtering coating, arc plasma coating, ion plating and molecular beam epitaxy, while chemical vapor deposition technology is a process that uses gaseous substances to produce chemical reactions and transport reactions on solids to produce solid deposits.

[0085] In other embodiments, the material layer is a coating formed by spraying the spray material on the substrate 111 by a spraying process. In this embodiment, the spraying process includes thermal spraying and cold spraying. Thermal spraying refers to heating and melting the coating material, atomizing it into extremely fine particles with a high-speed airflow, and spraying it onto the surface of the workpiece at a very high speed to form a coating. Cold spraying refers to spraying the coating powder onto the substrate by a supersonic gas-solid two-phase airflow at room temperature or a lower temperature to form a dense coating.

[0086] In some embodiments, the first material layer 112 is a coating layer processed on the coagulation cutting surface 11a by a vacuum coating process, and the vacuum coating process includes:

[0087] The coating area of ​​the substrate 111 is subjected to surface pretreatment to increase at least one of the parameters of the surface roughness, surface energy and bonding area of ​​the coating area with the material to be plated, so that the coating area can be more easily bonded with the material to be plated.

[0088] A material to be plated is selected to perform a coating process on the substrate 111 to form a first material layer 112 on the substrate 111, wherein the material to be plated includes a first material and a second material, wherein the first material contains a first component and the second material contains a second component;

[0089] During the process of forming the first material layer 112, the concentration of the first material and / or the concentration of the second material is adjusted so that in the surface layer of the formed first material layer 112, the content of the first component gradually decreases from the inside to the outside, and the content of the second component gradually increases from the inside to the outside.

[0090] Optionally, the first material is a target material, the second material is a gas source, a sputtering gas and a target material are selected, the gas source is introduced, and the gas source flow rate is controlled to gradually increase, so that the first material layer 112 is formed in the surface layer, the content of the first component gradually decreases from the inside to the outside, and the content of the second component gradually increases from the inside to the outside. Of course, in other embodiments, the first material and the second material can both use a gas source.

[0091] In this embodiment, a coating with a gradient content of a component is formed on the substrate 111 by the above method. The sputtering gas can be an inert gas such as argon. The first material can be a target material containing metal elements such as silicon or a silicon-containing gas source. The second material can be a fluorine-containing gas source. The introduction time of the gas source and the flow rate of the gas source can be controlled. For example, in the process of silicon element primer formation to form a bonding layer, the time for introducing the fluorine-containing gas source is adjusted to a later time, and then the flow rate of the fluorine-containing gas source is controlled to gradually increase, so that the content of the first component in the bonding layer is high, so as to ensure the bonding force between the first material layer 112 and the substrate 111. At the same time, the content of the second component is gradually increased from the inside to the outside to reduce the surface energy of the first material layer 112, so that the hydrophobicity of the surface of the first material layer 112 is relatively high, and the anti-tissue adhesion effect is good.

[0092] In other embodiments, the first material layer 112 is a coating layer processed on the coagulation cutting surface 11a by a spraying process, and the spraying process includes:

[0093] Pretreatment: Surface pretreatment is performed on the coating area of ​​the blade head 11 of the ultrasonic surgical scalpel 10 to increase at least one parameter of the surface roughness, surface energy and bonding area of ​​the coating area with the material to be sprayed, so that the coating area is easier to bond with the material to be sprayed.

[0094] Spraying, spraying the spray material onto the coating area to form a coating.

[0095] In this embodiment, the first material layer 112 can also be prepared by a spraying process, wherein the material composition ratios sprayed in different time periods are controlled to be different so that the component contents of each region of the formed first material layer 112 are different. For example, the first component content in the sprayed material of the sprayed bonding layer is controlled to be greater than the second component content, and the first component content in the sprayed materials from the sprayed bonding layer, the intermediate layer to the surface layer gradually decreases, and the second component content gradually increases, so that the second component content in the sprayed material of the surface layer is greater than the first component content, so as to ensure the bonding force between the first material layer 112 and the substrate 111 while reducing the surface energy of the first material layer 112, so that the hydrophobicity of the surface of the first material layer 112 is relatively high, and the anti-tissue adhesion effect is good.

[0096] In some embodiments, the first material layer 112 and the second material layer 113 can be made of the same or different materials. For example, in order to reduce processing costs, a plating layer or coating of the same material can be provided on both the coagulation cutting surface 11a and the auxiliary surface 11b. During processing, the element contents of each region of the first material layer 112 on the coagulation cutting surface 11a are controlled to be different, and the element contents of each region of the second material layer 113 on the auxiliary surface 11b can be the same or different. At the same time, the thickness of the second material layer 113 is controlled to be less than the thickness of the first material layer 112. As the thickness of the second material layer 113 decreases, the impedance of the cutter head 11 can be further reduced, and the reliability of the product can be further improved.

[0097] Since the wear resistance requirements of the coagulation cutting surface 11a and the auxiliary surface 11b are different, and the wear resistance requirement of the auxiliary surface 11b is lower than that of the coagulation cutting surface 11a, there is no need to make too many requirements for the second material layer 113 on the auxiliary surface 11b, and different material plating layers or coatings can be respectively provided on the coagulation cutting surface 11a and the auxiliary surface 11b to form the first material layer 112 and the second material layer 113. In this way, the diversity of the selection of the second material layer 113 is increased. The most suitable materials can be selected for the coagulation cutting surface 11a and the auxiliary surface 11b according to actual needs.

[0098] See also Figure 1-Figure 3 As shown, the embodiment of the present application also provides an ultrasonic surgical scalpel 10, including a blade head 11 that directly acts on a tissue object and a waveguide rod 12 for transmitting vibration to the blade head 11. The blade head 11 includes a substrate 111 and a first material layer 112. The substrate 111 can be made of metal material. The substrate 111 has a proximal end and a distal end. The proximal end of the substrate 111 is connected to the waveguide rod 12 and can be bent away from the waveguide rod 12 in the longitudinal direction and extend to the distal end. The substrate 111 is used to receive the ultrasonic vibration transmitted from the waveguide rod 12, so that the blade head 11 can operate and process the tissue object based on the received ultrasonic vibration.

[0099] A first material layer 112 is formed on the substrate 111 , and the first material layer 112 has a first side 1121 in contact with the substrate 111 and a second side 1122 facing away from the substrate 111 from the inside to the outside;

[0100] The first material layer 112 includes a first component and a second component, the first component is used to enhance the bonding force between the first material layer 112 and the substrate 111, and the second component is used to reduce the surface energy of the first material layer 112;

[0101] Near the first side 1121, the content of the first component is greater than the content of the second component, near the second side 1122, the content of the second component is greater than the content of the first component, and\or, the content of the first component at the first side 1121 is greater than the content of the first component at the second side 1122, and\or, the content of the second component at the second side 1122 is greater than the content of the second component at the first side 1121.

[0102] It can be seen from the above technical solutions that the ultrasonic surgical scalpel 10 proposed in the present application forms a first material layer 112 with different component contents in different regions on the base 111 of the blade head 11, wherein the first component content at the first side 1121 where the first material layer 112 is combined with the base 111 is relatively high, which can ensure the bonding force between the first material layer 112 and the base 111, thereby improving the overall adhesion of the first material layer 112. The second component content at the second side 1122 where the first material layer 112 contacts the tissue object is relatively high to reduce the surface energy of the first material layer 112, so that the hydrophobicity of the surface of the first material layer 112 is relatively high, and the anti-tissue adhesion effect is good. The ultrasonic surgical scalpel 10 of the present application, through the setting of different component contents in different regions of the first material layer 112, not only solves the problem of poor adhesion, but also has the characteristics of low friction coefficient, low surface energy, anti-tissue adhesion, etc. on the surface of the first material layer 112 while maintaining adhesion. Compared with existing coatings or ordinary plating layers, it has stronger adhesion and better wear resistance, meeting the requirements of multiple use of the product.

[0103] In some embodiments, the component contents of different regions of the first material layer 112 may vary in a gradient, for example, the content of the first component mentioned in the above embodiment gradually decreases from close to the first side 1121 to close to the second side 1122, and the content of the second component gradually increases from close to the first side 1121 to close to the second side 1122. Of course, different regions of the first material layer 112 may not vary in a gradient, as long as the formed first material layer 112 can have low friction coefficient, low surface energy, anti-tissue adhesion and other characteristics while ensuring adhesion.

[0104] Optionally, different areas of the first material layer 112 can be divided into a bonding layer, an intermediate layer and a surface layer from inside to outside, the bonding layer is located on the first side 1121 of the first material layer 112, the surface layer is located on the second side 1122 of the first material layer 112, and the intermediate layer is located between the bonding layer and the surface layer.

[0105] In the bonding layer, the content of the first component is greater than that of the second component. In this embodiment, the content of the first component in the bonding layer is relatively high, which can improve the bonding force between the first material layer 112 and the substrate 111, thereby improving the overall adhesion of the first material layer 112.

[0106] Among them, in the surface layer, the content of the second component is greater than that of the first component. In this embodiment, after the first component is used to prime the bonding layer to ensure the bonding force, the content of the second component can be controlled to gradually increase from the inside to the outside, so that the content of the second component in the surface layer is relatively large, which can reduce the surface energy of the first material layer 112, thereby making the surface of the first material layer 112 relatively hydrophobic and having a good anti-tissue adhesion effect.

[0107] Exemplarily, in the embodiment of the present application, the first material layer 112 is divided into a bonding layer, an intermediate layer and a surface layer, and the area division is performed only in the thickness direction of the single-layer first material layer 112. The area close to the first side 1121 is the bonding layer, the area close to the second side 1122 is the surface layer, and the area between the first side 1121 and the second side 1122 is the intermediate layer.

[0108] Of course, in other embodiments, the above division method may not be adopted, and the first material layer 112 may be divided into a surface layer as a whole, or the first material layer 112 may be divided only into a bonding layer close to the first side 1121 and a surface layer close to the second side 1122.

[0109] In some embodiments, the content of the first component in the bonding layer is greater than 50%. In this embodiment, the content of the first component specifically refers to the mass fraction of the first component. In the bonding layer, the content of the first component is greater than 50%, which can ensure the bonding force between the first material layer 112 and the substrate 111 and improve the overall adhesion of the first material layer 112.

[0110] In some embodiments, the content of the second component in the surface layer is greater than 40%. In this embodiment, the content of the second component specifically refers to the mass fraction of the second component. In the surface layer, the content of the second component is greater than 40%, which can ensure that the surface of the first material layer 112 has a lower surface energy, so that the hydrophobicity of the surface of the first material layer 112 is relatively high, and the anti-tissue adhesion effect is good.

[0111] The embodiment of the present application also provides a method for processing a blade head 11 of an ultrasonic surgical scalpel 10, comprising:

[0112] Surface treatment: The base 111 of the cutter head 11 is subjected to surface treatment to improve the adhesion of the base 111 .

[0113] Pretreatment: performing surface pretreatment on the substrate 111 to increase at least one parameter of the surface roughness, surface energy and bonding area of ​​the substrate 111 with the material to be processed, so that the substrate 111 can be more easily bonded with the material to be processed.

[0114] Material layer processing: processing the material to be processed on the substrate 111 to form a material layer.

[0115] For example, the surface treatment may be performed on the substrate 111 by shot blasting, sand blasting, knurling, engraving, etching, laser engraving, plasma etching, corona spot etching, polishing, abrasive flow machining or other techniques.

[0116] In some embodiments, shot blasting or sand blasting techniques may be preferred.

[0117] Of course, in other embodiments, the processing method may also omit the surface treatment step.

[0118] In some embodiments, the pretreatment may be performed by a surface plasma treatment process. Exemplarily, the pretreatment may be performed by using an inorganic oxygen-containing gas or a hydrocarbon-containing gas or a mixture for surface plasma treatment. The inorganic oxygen-containing gas includes (but is not limited to) at least one of water, hydrogen peroxide, ozone, oxygen, carbon dioxide, nitrogen dioxide, and nitric oxide. The hydrocarbon-containing gas includes (but is not limited to) at least one of straight-chain hydrocarbons, epoxy hydrocarbons, aromatic hydrocarbons, alcohols, carboxylic acids, ethers, furans, and organic amines.

[0119] In some embodiments, the material layer may be a coating formed on the substrate 111 by a vacuum coating process. After the metal substrate 111 is ionized, the material layer combines with the ionized coating molecules to form chemical bonds, thereby enhancing the bonding force between the coating and the metal substrate 111 .

[0120] In other embodiments, the material layer may also be a coating formed on the substrate 111 by a spraying process.

[0121] Exemplarily, the construction range on the blade 11 can be limited to the coagulation cutting surface 11a of the blade 11, which can ensure the anti-adhesion function, or it can be limited to the coagulation cutting surface 11a and the auxiliary surface 11b of the blade 11, and no plating or coating is added to the remaining areas to avoid an increase in product impedance and affect product reliability. The thickness of the material layer on the auxiliary surface 11b is less than the thickness of the material layer on the coagulation cutting surface 11a to further reduce the product impedance.

[0122] Exemplarily, the material to be processed for processing the material layer can be selected from polymeric materials and polymer-containing materials or non-polymeric materials. Polymeric materials and polymer-containing materials, such as (but not limited to) tetrafluorocarbon, hexafluoroethane, hexafluoropropane, heptafluoropropane, octafluoropropane, perfluorobutane, perfluoropentane, decafluoropentane, perfluorohexane, tetrafluoroethylene (TFE) and hexafluoropropylene (HFP) copolymer (FEP), FEP / ceramic composite, polytetrafluoroethylene (PTFE), PTFE / ceramic composite, polypropylene, polyethylene, polycaprolactone; non-polymeric materials, such as (but not limited to) tungsten disulfide, molybdenum disulfide, graphite, aluminum oxide, tungsten oxide, titanium nitride, chromium nitride, chromium carbide, tungsten carbide, metallized ceramics, stainless steel, molybdenum; silica gel, inorganic polysilazane, organic polysilazane, modified inorganic polysilazane and modified organic polysilazane. The coating can be formed by one or more combinations of the above.

[0123] The embodiments of the present application preferably select polytetrafluoroethylene (PTFE), PTFE / ceramic composites, chromium nitride coatings, and organic polysilazane.

[0124] Exemplarily, the elements contained in the material layer include: non-metallic coating elements such as C, F, Si, H, S, and metal elements such as Al, Ti, W, Mo, Cr, and Fe. The material layer may contain any of the above elements, as well as compounds, polymers, organics, and inorganics composed of the above elements. In the embodiment of the present application, F, Si, C, H, and Ti are preferably selected to form silicon carbide, organosilicon, diamond-like carbon, fluorine-containing inorganics or organics.

[0125] As an embodiment, a method for processing a blade head of an ultrasonic surgical scalpel 10 includes:

[0126] Pre-treatment: performing surface pre-treatment on the base 111 of the tool head to increase at least one parameter of the surface roughness, surface energy and bonding area of ​​the base 111 with the material to be processed, so that the surface of the base 111 is more easily bonded with the material to be processed.

[0127] A material to be processed is selected to process the substrate 111 to form a first material layer 112 on the substrate 111. The first material layer 112 has a first side 1121 in contact with the substrate 111 and a second side 1122 away from the substrate 111 from the inside to the outside. The material to be processed includes a first material and a second material. The first material contains a first component for improving the bonding force between the first material layer 112 and the substrate 111, and the second material contains a second component for reducing the surface energy of the first material layer 112.

[0128] In the process of forming the first material layer 112, the concentration of the first material and / or the concentration of the second material is adjusted so that the content of the first component is greater than the content of the second component at the first side 1121 of the formed first material layer 112, and the content of the second component is greater than the content of the first component at the second side 1122 of the formed first material layer 112, and / or so that in the formed first material layer 112, the content of the first component at the first side 1121 is greater than the content of the first component at the second side 1122, and / or so that in the formed first material layer 112, the content of the second component at the second side 1122 is greater than the content of the second component at the first side 1121.

[0129] In this embodiment, the first material layer 112 with different component contents in different regions is formed by the above method, so that the first component content at the first side 1121 where the first material layer 112 is combined with the substrate 111 is relatively high, which can ensure the bonding force between the first material layer 112 and the substrate 111, thereby improving the overall adhesion of the first material layer 112. In addition, the second component content at the second side 1122 where the first material layer 112 contacts the tissue object is relatively high, so as to reduce the surface energy of the first material layer 112, thereby making the hydrophobicity of the surface of the first material layer 112 relatively high, and having a good anti-tissue adhesion effect.

[0130] In some embodiments, the first material includes a target material containing a first component, and the second material includes a gas source containing a second component. In this embodiment, the target material can be a target material containing metal elements such as silicon, and the gas source can be a fluorine-containing gas source. The introduction time and flow rate of the gas source can be controlled to make different regions of the first material layer 112 have different component contents.

[0131] Illustratively, in the process of forming the first material layer 112, the flow rate of the gas source is controlled to change uniformly or gradiently so that the content of the first component is greater than the content of the second component at the first side 1121 of the first material layer 112, and the content of the second component is greater than the content of the first component at the second side 1122 of the first material layer 112.

[0132] Illustratively, during the process of forming the first material layer 112 , the flow rate of the gas source is controlled to change uniformly or gradually so that in the formed first material layer 112 , the content of the first component at the first side 1121 is greater than the content of the first component at the second side 1122 .

[0133] Illustratively, during the process of forming the first material layer 112 , the flow rate of the gas source is controlled to change uniformly or gradually so that in the formed first material layer 112 , the content of the second component at the second side 1122 is greater than the content of the second component at the first side 1121 .

[0134] Of course, the first material may also use a gas source containing the second component (silicon or other elements capable of improving bonding strength) to control the flow rate of the gas source containing the first component so that different regions of the first material layer 112 have different component contents.

[0135] Exemplarily, a gas source containing a first component is gradually introduced from zero to form a film on the substrate 111. After the film is formed, the flow rate of the gas source containing the first component is controlled to be gradually reduced so that the first component content of the first side 1121 of the first material layer 112 is the highest, and the first component content gradually decreases from the first side 1121 to the second side 1122. The introduction time of the gas source containing the second component (fluorine or other elements capable of reducing surface energy) can be controlled to be later than the introduction time of the gas source containing the first component, and the introduction flow rate of the gas source containing the second component is controlled to be gradually increased so that the second component content of the second side 1122 of the first material layer 112 is the highest, and the second component content gradually increases from the first side 1121 to the second side 1122. In this way, the formed first material layer 112 can have the characteristics of low friction coefficient, low surface energy, anti-tissue adhesion, etc. while ensuring adhesion.

[0136] In some embodiments, the process of forming the first material layer 112 includes an initial time period, an intermediate time period, and an end time period. In this embodiment, the concentration of the first material and / or the second material in different time periods can be controlled to achieve different component contents in different regions of the first material layer 112.

[0137] Exemplarily, the concentration of the first material in the initial time period is controlled to be greater than the concentration of the second material, so that the content of the first component is greater than the content of the second component at the first side 1121 of the formed first material layer 112. That is, in the bonding layer close to the first side 1121, the content of the first component is greater than the content of the second component.

[0138] Exemplarily, the concentration of the second material at the end time period is controlled to be greater than the concentration of the first material, so that the content of the second component is greater than the content of the first component at the second side 1122 of the formed first material layer 112. That is, in the surface layer close to the second side 1122, the content of the second component is greater than the content of the first component.

[0139] Exemplarily, the concentration of the first material in the initial time period is controlled to be greater than the concentration of the first material in the end time period, so that in the formed first material layer 112 , the content of the first component at the first side 1121 is greater than the content of the first component at the second side 1122 .

[0140] Exemplarily, the concentration of the second material in the initial time period is controlled to be lower than the concentration of the second material in the end time period, so that in the formed first material layer 112 , the content of the second component at the second side 1122 is greater than the content of the second component at the first side 1121 .

[0141] In some embodiments, the first material layer 112 forms a bonding layer on the first side 1121 in the initial time period, forms an intermediate layer in the middle time period, and forms a surface layer on the second side 1122 in the end time period.

[0142] Exemplarily, during the initial period of time, the concentration of the first material is controlled to gradually increase, so that the content of the first component in the bonding layer gradually increases.

[0143] Exemplarily, during the end time period, the concentration of the first material is controlled to gradually decrease and / or the concentration of the second material is controlled to gradually increase, so that in the surface layer, the content of the first component gradually decreases from the inside to the outside, and the content of the second component gradually increases from the inside to the outside.

[0144] In some embodiments, the pre-treatment uses plasma etching, which can make the etching highly directional, so as to facilitate the surface pre-treatment of the coating area.

[0145] In some embodiments, in the processing method of the first material layer 112 , surface treatment may be performed before pre-treatment, and the surface treatment includes performing surface treatment on the coating area to improve the adhesion of the coating area.

[0146] Illustratively, a method for processing a blade head of an ultrasonic surgical scalpel 10 of the present application includes (but is not limited to) the following specific embodiments.

[0147] Example 1

[0148] The present application can adopt the method of vacuum coating-vapor deposition to obtain a gradient coating, and the specific example operation process is as follows:

[0149] Before the experiment: first use acetone to remove oil stains on the surface of the sample, then use an ultrasonic cleaning device filled with deionized water to shake and wash to remove dust and other impurities on the surface of the sample. After washing, immediately put it in a drying oven to dry to avoid leaving water marks. After processing, immediately put it in a vacuum chamber.

[0150] Pre-treatment uses plasma etching to further process the surface of the substrate 111 of the tool head. The bombardment time lasts for several minutes or even dozens of minutes to remove impurities, oil molecules, oxides, etc. adsorbed on the surface of the substrate 111, improve the surface state of the sample, and enhance the bonding strength of the coating.

[0151] The specific operation is as follows: put the sample on the rack, close the vacuum chamber, turn on the mechanical pump, and when the vacuum degree reaches 1-10Pa, turn on the molecular pump until the vacuum is drawn to 9*10 -2 After the pressure drops below Pa, the gas source is introduced. Turn on the plasma power supply, set the power, time and other parameters, so that the ions move toward the sample surface under the action of negative bias, and the ions collide with the surface to remove surface impurities. Turn off the gas source, turn off the magnetic field source, etc.

[0152] After cleaning the sample surface, continue to vacuum to 9*10 -2 Pa, select high-purity silicon target as silicon source, argon as sputtering gas, turn on magnetic source, plasma source, bias power supply, target bias. Start coating, vacuum chamber temperature at 300℃-500℃, working pressure at 0.06-1.2Pa, while introducing gas source CH4 / CHF3, gas source concentration ratio 1:3-1:10, power 150W-300W, pulse high voltage 100Hz-300Hz, pulse width 15μs-30μs, duration 2h-4h.

[0153] After the work is completed, first turn off the bias power supply, plasma source, magnetic field power supply, etc. in the working order, wait for 20min-45min or longer, wait until the sample cools down naturally along with the vacuum chamber, then open the vacuum chamber to deflate and take out the sample.

[0154] The prepared coating is a carbon-fluorine-hydrogen-silicon compound, or a mixture of a carbon-fluorine compound, a hydrocarbon compound, a silicon-fluorine compound and the like in free combination.

[0155] In the embodiment of the present application, in order to achieve different element contents in different areas of the coating, the initial gas source flow rate ratio can be controlled first. Different flow rates correspond to different fluorine-carbon ratios. The change in flow rate ratio directly affects the coating structure and performance. For example, for hydrophobic performance, the fluorine-carbon ratio in the gas source increases, the concentration of F groups in the plasma increases, the probability of replacing H increases, the hydrophobic group -CF2 / CF3 increases, and the coating contact angle is improved.

[0156] In the embodiment of the present application, the gas source flow ratio can be gradually changed according to different time periods, CHF3 can be introduced into CH4, the initial time and the end time of CHF3 introduction can be controlled, and the element content in different areas of the coating can be controlled, thereby controlling the adhesion and / or surface energy of the coating.

[0157] In the embodiment of the present application, the gas source may include (but not limited to) methane, ethane, propane, acetylene, tetrafluoromethane, hexafluoroethane, hexafluoropropane, heptafluoropropane, octafluoropropane, perfluorobutane, perfluoropentane, decafluoropentane, perfluorohexane, and copolymers of tetrafluoroethylene and hexafluoropropylene. The target material may include (but not limited to) metal targets such as titanium target, chromium target, aluminum target, copper target, nickel target, tungsten target, and ceramic targets such as magnesium oxide target, iron oxide target, silicon oxide target, titanium nitride target, silicon carbide target, silicon dioxide target, and alloy targets such as iron-cobalt target, aluminum-silicon target, and titanium-zinc target. It is used to dope any one or more of the elements such as F, N, Si, Cr, P, Al, Ni, Fe, W, Co, and Mg in the coating to optimize the performance of the tool head coating.

[0158] In other embodiments, a radio frequency glow discharge method, a plasma stream ion implantation method or other vapor deposition method, a radio frequency magnetron sputtering method or the like may be used to obtain a gradient coating.

[0159] The gradient coating obtained in Example 1 is as follows Figure 4 As shown, specifically, it is a first material layer 112 on the coagulation cutting surface 11a, wherein points 1, 2 and 3 in three different areas are taken in the first material layer 112, point 1 is located in the binding layer, point 2 is located in the middle layer, and point 3 is located in the surface layer. The element contents at the positions of point 1, point 2 and point 3 are detected as shown in Table 1.

[0160] Table 1

[0161] Point 1 Point 2 Point 3 element Wt% Wt% Wt% C 16.13 25.3 30.2 O 3.27 5.55 4.62 Si 62.3 32.5 20.3 F 18.3 36.65 44.88 Total amount: 100.00 100.00 100.00

[0162] From the test data in Table 1, it can be seen that the silicon content of the coating gradually decreases from point 1, point 2 to point 3, that is, the silicon content gradually decreases from the bonding layer, the middle layer to the surface layer. The fluorine content gradually increases from point 1, point 2 to point 3, that is, the fluorine content gradually increases from the bonding layer, the middle layer to the surface layer.

[0163] The content of each element, water drop angle and adhesion of the surface of the coating prepared in Example 1 were tested as shown in Table 2.

[0164] Table 2

[0165]

[0166] It can be seen from the test data in Table 2 that the adhesion of the coating of the ultrasonic surgical scalpel in the embodiment of the present application is 60N, which can meet the bonding strength requirements between the coating and the substrate. The water drop angle on the coating surface is 100°, which can meet the requirements of anti-adhesion performance. Among them, the higher the water drop angle, the better the hydrophobicity, the lower the surface energy, and the better the anti-adhesion performance. Therefore, the ultrasonic surgical scalpel of the present application not only solves the problem of poor adhesion, but also has the characteristics of low friction coefficient, low surface energy, and anti-tissue adhesion while maintaining adhesion. Compared with ordinary coatings, it has stronger adhesion and better wear resistance, which meets the requirements of multiple use of the product.

[0167] Example 2

[0168] The present application can also use a thermal spraying process to obtain a gradient coating, using thermal energy to melt the spraying material, and then atomizing it with the help of a high-speed airflow. Driven by the high-speed airflow, the particles hit the surface of the substrate 111 and condense to form a functional coating. The specific example operation process is as follows:

[0169] Sample preparation, in order to improve the adhesion of the coating, first clean and remove dirt and grease on the surface of the workpiece, use organic solvents or others, and heat to a certain temperature.

[0170] Pre-treatment: The surface is roughened by sandblasting.

[0171] Spraying process: a double spray gun system is used, one spray gun sprays a binder that can be well bonded to the substrate 111, and the other spray gun sprays a low surface energy coating, such as Teflon, silicone, etc. The spray gun process parameters are controlled to achieve sequential spraying to ensure that the coating is well bonded and has a low surface energy.

[0172] The element content of each area of ​​the formed coating can be different by controlling the different ratios of the material elements sprayed in different time periods.

[0173] Drying and sintering: The coating is dried in a furnace to evaporate most of the solvent. Depending on the coating selection, the sintering process can be increased to make the coating and the substrate 111 more firmly bonded.

[0174] Among them, the content of each element, water drop angle and adhesion of the coating surface prepared in Example 2 were tested as shown in Table 3.

[0175] Table 3

[0176]

[0177] From the test data in Table 3, it can be seen that the adhesion of the coating in Example 2 is 50N, which can meet the bonding strength requirement between the coating and the substrate, and the water drop angle on the coating surface is 95°, which can meet the anti-adhesion performance requirement.

[0178] It can be seen from the data in Table 2 and Table 3 that the ultrasonic surgical scalpel of the present application not only solves the problem of poor adhesion, but also has the characteristics of low friction coefficient, low surface energy, and anti-tissue adhesion while maintaining adhesion. Compared with ordinary coatings, it has stronger adhesion and better wear resistance, and meets the requirements for multiple use of the product.

[0179] Example 3

[0180] The present application can also adopt the cold spray process to obtain the gradient coating, which is a solid-state forming method based on the principles of aerodynamics and high-speed collision dynamics. In the cold spray process, high-pressure gas (nitrogen, helium, compressed air, etc.) is used as an accelerating medium, and in a specially designed contraction-expansion Laval nozzle, it drives the metal or metal and ceramic mixed powder particles to move at a very high speed in the solid state, collides with the substrate 111 to be coated, and causes the particles / substrate 111 to undergo strong plastic deformation, and deposits to form a coating after meeting specific deformation conditions.

[0181] The element content of each area of ​​the formed coating can be different by controlling the different ratios of the material elements sprayed in different time periods.

[0182] Among them, the spraying material can be selected from polymeric materials and polymer-containing materials or non-polymeric materials. Polymeric materials and polymer-containing materials include (but are not limited to) FEP / ceramic composites, polytetrafluoroethylene (PTFE), PTFE / ceramic composites, polypropylene, polyethylene, polycaprolactone; non-polymeric materials include (but are not limited to) tungsten disulfide, molybdenum disulfide, graphite, aluminum oxide, tungsten oxide, titanium nitride, chromium nitride, chromium carbide, tungsten carbide, metallized ceramics, stainless steel, molybdenum; silica gel, inorganic polysilazane, organic polysilazane, modified inorganic polysilazane and modified organic polysilazane. The coating can be formed by one or more combinations of the above. Polytetrafluoroethylene (PTFE), PTFE / ceramic composites, chromium nitride coatings, and organic polysilazane are preferably selected.

[0183] Comparative Example 1

[0184] The existing common coating was selected as comparative example 1, and the content of each element, water drop angle and adhesion of the surface of the common coating were tested as shown in Table 4

[0185] Table 4

[0186]

[0187] From the test data in Table 4, it can be seen that the water drop angle of Comparative Example 1 is 90°. Although it can meet the hydrophobic performance requirements, the adhesion force is only 30N, which is difficult to meet the bonding strength requirements between the coating and the substrate.

[0188] By comparing the test data in Table 2 and Table 4, it can be seen that the adhesion of the coating of Example 1 is greater than that of the coating of Comparative Example 1, and the water drop angle of the coating surface of Example 1 is greater than that of the coating surface of Comparative Example 1, that is, the hydrophobicity of the coating surface of Example 1 is greater than that of the coating surface of Comparative Example 1. The lower the surface energy, the better the hydrophobicity and the better the anti-adhesion performance. Therefore, the ultrasonic surgical scalpel of the present application not only solves the problem of poor adhesion, but also has the characteristics of low friction coefficient, low surface energy, and anti-tissue adhesion while maintaining adhesion. Compared with ordinary coatings, it has stronger adhesion and better wear resistance, which meets the requirements of multiple uses of the product.

[0189] See also Figure 5 As shown, the embodiment of the present application also provides an ultrasonic surgical device 100, including a handpiece 20, a clamping assembly 30 and the above-mentioned ultrasonic surgical scalpel 10. The handpiece 20 is used for holding, the clamping assembly 30 includes a clamping member 31, and the blade head 11 is installed on the clamping assembly 30 through a waveguide rod 12. The clamping assembly 30 can control a clamping member 31 to cooperate with the blade head 11 to clamp or loosen the tissue object. In this embodiment, the handpiece 20 includes a handle 21 and a trigger 22 movably connected to the handle 21. The clamping assembly 30 includes a clamping member 31 and a transmission chain connected to the clamping member 31. When operating the ultrasonic surgical device 100, the operator can hold the handle 21 and extend the blade head 11 into the lesion site in the human body through the slender waveguide rod 12. Then, by operating the trigger 22 to trigger the excitation transmission chain or the closing transmission chain, a clamping member 31 is controlled to cooperate with the blade head 11 to clamp or release the tissue object, thereby facilitating the cutting, coagulation and other operations of human tissue through the blade head 11.

[0190] The structure and function of the ultrasonic surgical scalpel 10 in the ultrasonic surgical device 100 proposed in the embodiment of the present application are the same as those in the above embodiment. For details, please refer to the description of the above embodiment, and this embodiment will not be repeated.

[0191] See also Figure 6 As shown, the embodiment of the present application provides an ultrasonic surgical device 1000, including an ultrasonic surgical device 100 and an ultrasonic transducer 200, wherein the ultrasonic transducer 200 is connected to a handpiece 20, and is used to receive an external electrical signal and convert the electrical signal into a mechanical vibration in an ultrasonic frequency band, so as to transmit the mechanical vibration to an ultrasonic surgical scalpel 10. In this embodiment, the ultrasonic transducer 200 can convert the electrical signal into a mechanical vibration, and transmit the generated mechanical vibration to the waveguide rod 12 and the blade head 11 of the ultrasonic surgical scalpel 10.

[0192] The structure and function of the ultrasonic surgical scalpel 10 in the ultrasonic surgical device 1000 proposed in the embodiment of the present application are the same as those in the above embodiment. For details, please refer to the description of the above embodiment, and this embodiment will not be repeated.

[0193] See also Figure 7 As shown, the embodiment of the present application also provides an ultrasonic surgical system 10000, including a host 2000 and the above-mentioned ultrasonic surgical device 1000, the ultrasonic surgical device 1000 is connected to the host 2000, and is used to receive the electrical signal sent by the host 2000 to generate ultrasonic vibration to operate the tissue object. In this embodiment, the host 2000 can also be used to receive signal feedback from the surgical object and perform relevant analysis.

[0194] The structure and function of the ultrasonic surgical scalpel 10 in the ultrasonic surgical system 10000 proposed in the embodiment of the present application are the same as those in the above embodiment. For details, please refer to the description of the above embodiment, and this embodiment will not be repeated.

[0195] Those skilled in the art may combine and associate different embodiments or examples and features of different embodiments or examples described in this specification without mutual contradiction.

[0196] The above is only a specific implementation of the present application, but the protection scope of the present application is not limited thereto. Any technician familiar with the technical field can easily think of various equivalent modifications or replacements within the technical scope disclosed in the present application, and these modifications or replacements should be included in the protection scope of the present application. Therefore, the protection scope of the present application shall be based on the protection scope of the claims.

Claims

1. An ultrasonic surgical scalpel, characterized in that: The invention comprises a cutting head directly acting on a tissue object and a waveguide rod for transmitting vibration to the cutting head, wherein the cutting head comprises: A substrate having a proximal end and a distal end, wherein the proximal end of the substrate is connected to the waveguide rod, and the substrate is used to receive the ultrasonic vibration transmitted from the waveguide rod, so that the cutter head can operate and process the tissue object based on the received ultrasonic vibration; A first material layer is formed on the substrate, wherein the first material layer has a first side that is in contact with the substrate and a second side that is away from the substrate from the inside to the outside, and the first material layer includes a surface layer, and a surface of the surface layer is used to contact the tissue object; Among them, the first material layer has a first component and a second component, the first component is used to improve the bonding strength between the first material layer and the substrate, and the second component is used to reduce the surface energy of the first material layer. In the surface layer, the content of the first component gradually decreases from the inside to the outside, and the content of the second component gradually increases from the inside to the outside.

2. The ultrasonic surgical scalpel according to claim 1, characterized in that: On a side of the surface layer close to the substrate, the content of the first component is greater than the content of the second component; and / or, On a side of the surface layer away from the substrate, the content of the second component is greater than the content of the first component.

3. The ultrasonic surgical scalpel according to claim 1, characterized in that: The content of the first component gradually decreases from close to the first side to close to the second side; and / or, The content of the second component gradually increases from close to the first side to close to the second side.

4. The ultrasonic surgical scalpel according to claim 1, characterized in that: The content of the first component is greater than 50% near the first side; and / or the content of the second component is greater than 40% near the second side.

5. The ultrasonic surgical scalpel according to claim 1, characterized in that: The first material layer further comprises a bonding layer and an intermediate layer, the bonding layer is close to the first side of the first material layer, the surface layer is close to the second side of the first material layer, and the intermediate layer is located between the bonding layer and the surface layer; Wherein, in the bonding layer, the content of the first component is greater than the content of the second component; and / or, in the surface layer, the content of the second component is greater than the content of the first component.

6. The ultrasonic surgical scalpel according to claim 5, characterized in that: The intermediate layer includes a first sub-region and a second sub-region from the inside to the outside; In the first sub-region, the content of the first component gradually increases from the inside to the outside, and in the second sub-region, the content of the first component gradually decreases from the inside to the outside, and / or, in the first sub-region, the content of the second component gradually decreases from the inside to the outside, and in the second sub-region, the content of the second component gradually increases from the inside to the outside; or, In the first sub-zone, the content of the first component gradually decreases from the inside to the outside, and in the second sub-zone, the content of the first component gradually increases from the inside to the outside, and / or, in the first sub-zone, the content of the second component gradually increases from the inside to the outside, and in the second sub-zone, the content of the second component gradually decreases from the inside to the outside.

7. The ultrasonic surgical scalpel according to claim 5, characterized in that: The intermediate layer includes a first sub-region, a second sub-region and a third sub-region from the inside to the outside; In the first sub-region, the content of the first component gradually increases from the inside to the outside, in the second sub-region, the content of the first component gradually decreases from the inside to the outside, and in the third sub-region, the content of the first component gradually increases from the inside to the outside, and / or, in the first sub-region, the content of the second component gradually decreases from the inside to the outside, in the second sub-region, the content of the second component gradually increases from the inside to the outside, and in the third sub-region, the content of the second component gradually decreases from the inside to the outside; or, In the first sub-zone, the content of the first component gradually decreases from the inside to the outside, in the second sub-zone, the content of the first component gradually increases from the inside to the outside, and in the third sub-zone, the content of the first component gradually decreases from the inside to the outside, and / or, in the first sub-zone, the content of the second component gradually increases from the inside to the outside, in the second sub-zone, the content of the second component gradually decreases from the inside to the outside, and in the third sub-zone, the content of the second component gradually increases from the inside to the outside.

8. The ultrasonic surgical scalpel according to claim 1, characterized in that: The first component includes at least one of silicon, aluminum, titanium, tungsten, molybdenum, chromium, iron, nickel, cobalt, and magnesium.

9. The ultrasonic surgical scalpel according to claim 1, characterized in that: The second component includes at least one of fluorine, carbon, silicon, Teflon, and silicone.

10. The ultrasonic surgical scalpel according to claim 1, characterized in that: The thickness a of the first material layer ranges from 5 micrometers to 8 micrometers.

11. The ultrasonic surgical scalpel according to claim 1, characterized in that: The substrate surface has a first area and a second area, and the first material layer is formed in the first area for contacting the tissue object; The tool head further includes a second material layer formed in the second region, and a thickness of the second material layer is smaller than a thickness of the first material layer.

12. The ultrasonic surgical scalpel according to claim 10, characterized in that: The thickness b of the second material layer ranges from 1 micron to 2 microns.

13. The ultrasonic surgical scalpel according to claim 1, characterized in that: The first material layer is a coating or a plating layer.

14. The ultrasonic surgical scalpel according to claim 13, characterized in that: The first material layer is a coating layer processed on the substrate by a vacuum coating process; or The first material layer is a coating formed on the substrate by a spraying process.

15. The ultrasonic surgical scalpel according to claim 14, characterized in that: The first material layer is a coating formed by processing the material to be plated on the substrate by a vacuum coating process, wherein the vacuum coating process comprises: Performing surface pretreatment on the coating region of the substrate to increase at least one parameter of the coating region's surface roughness, surface energy, and bonding area with the material to be coated; Selecting a material to be plated to perform a coating process on the substrate to form the first material layer on the substrate, the material to be plated includes a first material and a second material, the first material contains the first component, and the second material contains the second component; During the process of forming the first material layer, the concentration of the first material and / or the concentration of the second material is adjusted so that in the surface layer of the formed first material layer, the content of the first component gradually decreases from the inside to the outside, and the content of the second component gradually increases from the inside to the outside.

16. An ultrasonic surgical scalpel, characterized in that: The invention comprises a cutting head directly acting on a tissue object and a waveguide rod for transmitting vibration to the cutting head, wherein the cutting head comprises: A substrate having a proximal end and a distal end, wherein the proximal end of the substrate is connected to the waveguide rod, and the substrate is used to receive the ultrasonic vibration transmitted from the waveguide rod, so that the cutter head can operate and process the tissue object based on the received ultrasonic vibration; A first material layer formed on the substrate, wherein the first material layer has a first side in contact with the substrate and a second side facing away from the substrate from the inside to the outside; Wherein, the first material layer comprises a first component and a second component, the first component is used to enhance the bonding force between the first material layer and the substrate, and the second component is used to reduce the surface energy of the first material layer; Near the first side, the content of the first component is greater than the content of the second component, near the second side, the content of the second component is greater than the content of the first component, and\or, the content of the first component at the first side is greater than the content of the first component at the second side, and\or, the content of the second component at the second side is greater than the content of the second component at the first side.

17. The ultrasonic surgical scalpel according to claim 16, characterized in that: The content of the first component gradually decreases from close to the first side to close to the second side; and / or, The content of the second component gradually increases from close to the first side to close to the second side.

18. The ultrasonic surgical scalpel according to claim 16, characterized in that: The first material layer comprises a bonding layer, an intermediate layer and a surface layer from inside to outside, the bonding layer is located on a first side of the first material layer, the surface layer is located on a second side of the first material layer, and the intermediate layer is located between the bonding layer and the surface layer; Wherein, in the bonding layer, the content of the first component is greater than the content of the second component; and / or, in the surface layer, the content of the second component is greater than the content of the first component.

19. The ultrasonic surgical scalpel according to claim 18, characterized in that: In the bonding layer, the content of the first component is greater than 50%; and / or, in the surface layer, the content of the second component is greater than 40%.

20. A method for processing a blade of an ultrasonic surgical scalpel, characterized in that: include: Pre-treatment: performing surface pre-treatment on the base of the tool head to increase at least one parameter of the base's surface roughness, surface energy, and bonding area with the material to be processed; Selecting a material to be processed to process the substrate to form a first material layer on the substrate, wherein the first material layer has a first side in contact with the substrate and a second side away from the substrate from the inside to the outside, and the material to be processed includes a first material and a second material, wherein the first material contains a first component for improving the bonding force between the first material layer and the substrate, and the second material contains a second component for reducing the surface energy of the first material layer; In the process of forming the first material layer, the concentration of the first material and / or the concentration of the second material is adjusted so that the content of the first component is greater than the content of the second component at the first side of the first material layer, and the content of the second component is greater than the content of the first component at the second side of the first material layer, and / or so that in the first material layer, the content of the first component at the first side is greater than the content of the first component at the second side, and / or so that in the first material layer, the content of the second component at the second side is greater than the content of the second component at the first side.

21. The processing method according to claim 20, characterized in that: The process of forming the first material layer includes an initial time period, an intermediate time period and an end time period; Controlling the concentration of the first material in the initial time period to be greater than the concentration of the second material, so that at the first side of the formed first material layer, the content of the first component is greater than the content of the second component; and / or, Controlling the concentration of the second material in the end time period to be greater than the concentration of the first material, so that at the second side of the formed first material layer, the content of the second component is greater than the content of the first component; Controlling the concentration of the first material in the initial time period to be greater than the concentration of the first material in the end time period, so that in the formed first material layer, the content of the first component at the first side is greater than the content of the first component at the second side; and / or, The concentration of the second material in the initial time period is controlled to be lower than the concentration of the second material in the end time period, so that in the formed first material layer, the content of the second component at the second side is greater than the content of the second component at the first side.

22. The processing method according to claim 21, characterized in that: The first material layer forms a bonding layer located on the first side in the initial time period, the first material layer forms an intermediate layer in the intermediate time period, and the first material layer forms a surface layer located on the second side in the final time period; During the initial time period, the concentration of the first material is controlled to gradually increase and / or the concentration of the second material is controlled to gradually decrease, so that the content of the first component in the bonding layer gradually increases; and / or, During the end time period, the concentration of the first material is controlled to gradually decrease and / or the concentration of the second material is controlled to gradually increase, so that in the surface layer, the content of the first component gradually decreases from the inside to the outside, and the content of the second component gradually increases from the inside to the outside.

23. The processing method according to claim 20, characterized in that: The first material includes a target material containing the first component, and the second material includes a gas source containing the second component; In the process of forming the first material layer, the flow rate of the gas source is controlled to change uniformly or gradually so that the content of the first component at the first side of the first material layer is greater than the content of the second component, and the content of the second component at the second side of the first material layer is greater than the content of the first component, and / or so that in the first material layer, the content of the first component at the first side is greater than the content of the first component at the second side, and / or so that in the first material layer, the content of the second component at the second side is greater than the content of the second component at the first side.

24. The processing method according to claim 20, characterized in that: The pre-treatment adopts plasma etching.

25. An ultrasonic surgical device, characterized in that: include: A hand piece for holding; A clamping assembly, including a clamping member; According to the ultrasonic surgical scalpel as described in any one of claims 1 to 19, the blade head is mounted on the clamping assembly through the waveguide rod, and the clamping assembly is used to control one of the clamping members to cooperate with the blade head to clamp or release the tissue object.

26. An ultrasonic surgical device, characterized in that: include: The ultrasonic surgical device of claim 25; The ultrasonic transducer is connected to the handpiece, and is used for receiving external electrical signals and converting the electrical signals into mechanical vibrations in the ultrasonic frequency band, and transmitting the mechanical vibrations to the ultrasonic surgical scalpel.

27. An ultrasonic surgical system, characterized in that: include: Host; The ultrasonic surgical device as described in claim 26 is connected to the host, and is used to receive the electrical signal sent by the host and generate ultrasonic vibration to operate and process the tissue object.