Multifunctional gel dressing for promoting wound repair and preparation method

By preparing a multifunctional gel dressing containing collagen, polysaccharide polymers, and moisturizers, the limitations of existing gel dressings in terms of applicability and healing effect have been solved. This results in rapid pain relief, reduced infection, and promotion of wound repair, making it suitable for various wound types.

CN118949106AInactive Publication Date: 2024-11-15BEIJING GUOXIETANG TECH DEV CO LTD +1

Patent Information

Application Number
CN202411443607.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-16
Publication Date
2024-11-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing gel dressings are insufficient in terms of applicability and healing effect, cannot effectively promote wound repair, and have complex components or limited application.

Method used

Using collagen, polysaccharide polymers, moisturizers, and excipients as the main components, a multifunctional gel dressing is prepared through a specific preparation method, including steps such as collagen dissolution, mixing, stirring, centrifugation and degassing, and sterilization, to form a care and repair material suitable for various non-chronic wounds.

Benefits of technology

This gel dressing provides rapid pain relief, reduces wound infection, promotes wound healing, reduces pigmentation and scar formation, and provides moisturizing effects. It is suitable for large-scale production and is non-toxic.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention provides a multifunctional gel dressing for promoting wound repair and a preparation method of the multifunctional gel dressing. The multifunctional gel dressing comprises the following raw materials: collagen and polysaccharide macromolecules. The gel dressing disclosed by the invention has the functions of resisting bacteria, repairing and reducing scar formation and pigmentation; the biocompatibility is high, wound infection can be reduced, wound pain can be quickly relieved, and a good repairing effect on various non-chronic wound masks is achieved; and the composition can also be used for resisting bacteria, moisturizing and repairing female vulva and vagina, and promoting vagina health. The method is controllable, low in cost, non-toxic and suitable for large-scale production. The material can be used as a biomedical material, and especially has a wide application prospect in the fields of wound repair and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of medical technology, and in particular to a multifunctional gel dressing for promoting wound repair and a preparation method thereof. Background Art

[0002] Dressings are an essential element of wound care, with the primary purposes of a) providing a temporary protective physical barrier, b) absorbing wound drainage, and c) providing the moisture necessary to optimize re-epithelialization. Modern wound dressings offer additional benefits, such as antimicrobial properties and pain relief, particularly gel dressings.

[0003] Gel dressings are applied to the wound surface by coating or spraying, and have been widely used in the care of superficial wounds such as minor wounds, abrasions, cuts and the surrounding skin, and are suitable for controlling infection of human surface wounds and promoting wound healing. The expected effects include but are not limited to cleaning, sterilization, isolation, protection, medication and / or nutrition, etc. However, existing gel wound dressings have the disadvantages of limited application range and unsatisfactory healing effect.

[0004] CN116688212A authorizes a type III recombinant collagen dressing with repair and anti-aging effects, its preparation method and application, including the following raw materials: recombinant type III humanized collagen, D-(+)-trehalose dihydrate, carbomer, xanthan gum, butylene glycol, glycerol, triethanolamine, which has a positive effect on skin repair and anti-aging. CN116019965A discloses a collagen film dressing and its preparation method, including raw materials: type III recombinant humanized collagen, modified chitosan, oil phase carrier, polyol, preservative, modified soy protein isolate, aloe fermentation liquid, modified hyaluronic acid, Chinese medicine extract, water, which has good biological functions and helps promote human wound healing and tissue repair, but its species are relatively complex and its wound repair ability has not been verified. CN117815372A discloses a wound repair composition, including recombinant collagen, hyaluronic acid or its salt, and carboxymethyl chitosan. The components in the composition have the effect of synergistically promoting collagen synthesis and improving wound healing rate, and it is mainly used for chronic wounds. CN112675353A discloses a recombinant collagen dressing and a preparation method thereof. Recombinant collagen, sodium hyaluronate, and chitosan are added to water, and finally freeze-dried to obtain a recombinant collagen dressing. The preparation method is simple, and the prepared recombinant collagen dressing has high biological activity, strong moisture retention, high tensile strength, strong softness and plasticity, and is suitable for industrial production, but because it is in a solid state, the scope of application is limited. Summary of the invention

[0005] In order to overcome the deficiencies of the prior art, the present invention provides a multifunctional gel dressing and a preparation method for promoting wound repair. The gel dressing of the present invention has the functions of quickly relieving wound pain, reducing wound infection, promoting wound healing and skin repair, and can also be used to reduce wound pigmentation and scar formation, while moisturizing the wound, and can be used for various non-chronic wounds; its preparation method is controllable, low-cost, non-toxic, and suitable for large-scale production. It is used for the care and repair of non-chronic wounds (such as superficial wounds, postoperative suture wounds, mechanical trauma, small wounds, abrasions, sunburns, cut wounds, puncture sites of puncture instruments, first-degree or shallow second-degree burn wounds, laser / photon / acid peeling / micro-plastic surgery / grinding wounds, and wounds caused by sensitive skin, dermatitis, acne, etc.), providing a microenvironment for wound healing.

[0006] To achieve the above-mentioned purpose, the present invention provides a multifunctional gel dressing for promoting wound repair and a preparation method thereof, the components of which include collagen, polysaccharide polymer, moisturizer, excipient, and purified water. The following is a specific preparation method: (1) Prepare collagen, polysaccharide polymer, moisturizer, excipient and purified water for later use; (2) Dissolving collagen in purified water to prepare a collagen solution for later use; (3) adding polysaccharide polymers to the collagen solution in sequence and dissolving them completely to obtain a mixture 1, which is allowed to stand for later use; (4) mixing the moisturizing agent and the excipient uniformly to obtain a mixture 2; (5) adding mixture 1 to mixture 2, stirring evenly, and centrifuging to degas, thereby obtaining a dressing base solution; (6) adding the dressing base liquid into a carrier to prepare a gel dressing; (7) Moist heat sterilization at 121°C for 6-10 min.

[0007] As a further improvement of the present invention, the contents of the components are as follows: collagen 0.01-5wt%, polysaccharide polymer 0.05-5wt%, moisturizer 1-5wt%, excipient 0.1-0.5wt%, and the balance is purified water.

[0008] As a further improvement of the present invention, the collagen can withstand irradiation sterilization and is one or both of recombinant type III humanized collagen and hydrophilic collagen. The preferred recombinant type III humanized collagen has a weight content of 0.05-5wt%; the preferred hydrophilic collagen is a hydrophilic collagen prepared by amidation modification of collagen extracted from animal tissue, and has a weight content of 0.01-2wt%.

[0009] As a further improvement of the present invention, the hydrophilic collagen can be obtained by freeze-drying the water-soluble collagen stock solution B in patent CN 116808279 B.

[0010] Alternatively, the specific preparation method of the hydrophilic collagen may include: ① Pre-treatment: The animal source tissue bovine Achilles tendon is washed, the surface fat is removed and then sliced; ② Virus inactivation: Soak the sliced ​​tissue in 0.5M sodium hydroxide solution. After 2 hours, rinse the tissue slices repeatedly with purified water and continue to mince the slices until they are shredded. ③ Extraction: Weigh the minced tissue and put it into a reactor, then add pepsin (the amount added is 1 / 20 of the tissue weight) and acetic acid (the amount added is 2.5% of the tissue weight), and react at a speed of 160 rpm for 48 hours to obtain a crude collagen solution; ④ Salting out purification: Add sodium chloride solution to the crude collagen solution to make its final concentration in the collagen solution 42g / L. At this time, the collagen precipitates in the form of flocs, and the supernatant is discarded after centrifugation; add 0.3% acetic acid aqueous solution to the flocs to dissolve the collagen, put it into a dialysis bag, seal it and put it into purified water, and dialyze it for 24h to obtain the purified collagen stock solution A; ⑤ Hydrophilic modification: Take an appropriate amount of collagen stock solution A, dilute it with 0.3% acetic acid to a collagen solution with a concentration of 10 mg / mL, adjust the pH to 12, add the modifier succinic anhydride, the mass ratio of succinic anhydride to collagen is 1:1, and stir for 3 hours to obtain a modified collagen crude solution; ⑥ Precipitation of modified collagen: Add 5M sodium hydroxide solution to the crude solution of modified collagen to make its pH value 4.5, and precipitate water-soluble collagen solid: ⑦ Washing and re-dissolving: Wash the water-soluble collagen solid repeatedly with 5% sodium chloride solution for 3 times, centrifuge and discard the supernatant, then dissolve it with 0.3% acetic acid to obtain the water-soluble collagen stock solution; ⑧ Freeze-drying: Freeze-drying to obtain hydrophilic collagen solid.

[0011] As a further improvement of the present invention, the polysaccharide polymer is a polysaccharide combination of at least three of carboxymethyl chitosan, carboxymethyl chitin, trehalose, and sodium hyaluronate, and the preferred weight content is 0.05-2wt% of carboxymethyl chitosan, 0.05-2wt% of carboxymethyl chitin, 0.05-2wt% of sodium hyaluronate, and 0.05-1wt% of trehalose.

[0012] As a further improvement of the present invention, the moisturizing agent is one or both of glycerol and propylene glycol.

[0013] As a further improvement of the present invention, the excipient is one or both of xanthan gum and carbomer.

[0014] As a further improvement of the present invention, in (4) and (5), the stirring is mechanical stirring at 100-200 rpm for 20-30 min at room temperature.

[0015] As a further improvement of the present invention, in (5), the centrifugation is performed at 4000-4500 rpm for 8-15 min at room temperature for degassing.

[0016] The recombinant and hydrophilic collagen, carboxymethyl chitosan, carboxymethyl chitosan, sodium hyaluronate, and trehalose in the gel dressing of the present invention work synergistically to ensure the ability of the dressing to promote wound repair. Collagen shows good biocompatibility due to its composition and biological characteristics. Its natural porous reticular structure can quickly adsorb blood and promote platelet aggregation when in contact with the wound, while absorbing tissue permeate, creating a good wound microenvironment and promoting wound healing, and is therefore commonly used in wound dressing ingredients. Carboxymethyl chitosan can be degraded by organisms, and its degradation products are raw materials for biological synthesis of the body, so it has good biological activity and biosafety, especially good biological activity for regeneration and repair of the body. Carboxymethyl chitosan is an important water-soluble chitosan derivative with good biocompatibility and biodegradability, which can promote wound healing, inhibit scarring, and has analgesic and antibacterial effects, and can also improve the mechanical stability of the dressing. Trehalose is a polymer stabilizer that can remove OH free radicals generated by α and β rays, making cell DNA less likely to mutate, and can further improve the gel's ability to adapt to the environment, resist radiation, moisturize, improve mechanics, reduce fine lines, brighten skin tone, and improve smoothness. Sodium hyaluronate can promote the proliferation and differentiation of epidermal cells, and can also remove free radicals. It has the function of repairing skin damage and is often used to replenish moisture, resist wrinkles, and resist aging to achieve the effect of improving skin luster. The addition of sodium hyaluronate can also improve the gel properties of the dressing, thereby enhancing the stability of the gel.

[0017] Compared with the prior art, the present invention has the following beneficial effects: the gel dressing of the present invention has the functions of antibacterial repair, reducing scar formation and pigmentation; it has high biocompatibility, can reduce wound infection, quickly relieve wound pain, and has good repair effects on various non-chronic wounds; it can also be used for antibacterial, moisturizing, and repairing of female vulva and vagina, and promote vaginal health. The production process of the method is controllable, low-cost, non-toxic, and suitable for large-scale production. It can be used as a biomedical material, especially in the fields of wound repair and has broad application prospects. DETAILED DESCRIPTION

[0018] The present application is further described below by way of examples, but the present application is not limited to the scope of the examples. The experimental methods without specific conditions in the following examples are selected according to conventional methods and conditions, or according to the product instructions.

[0019] Example 1 All ingredients are calculated based on 100g (1) Take 0.05 g of recombinant humanized type III collagen, 0.1 g of carboxymethyl chitosan, 0.1 g of trehalose, 0.5 g of sodium hyaluronate, 5 g of glycerol, 0.5 g of xanthan gum and 93.75 g of purified water for later use; (2) Dissolve 0.05 g of recombinant humanized type III collagen in 60 g of purified water to prepare a recombinant humanized type III collagen solution for later use; (3) Add 0.1 g of carboxymethyl chitosan, 0.1 g of trehalose, and 0.5 g of sodium hyaluronate to the recombinant type III humanized collagen solution, homogenize to obtain a mixture 1, and let it stand for later use; (4) 5 g of glycerol and 0.5 g of xanthan gum were dissolved in the remaining purified water (33.75 g), and the mixture was mechanically stirred at 200 rpm for 30 min to obtain a mixture II; (5) adding mixture 1 to mixture 2, mechanically stirring at 150 rpm for 20 min, and centrifuging at 4000 rpm for 10 min to degas, to obtain a dressing base solution; (6) adding the dressing base liquid into the non-woven fabric to prepare a gel dressing; (7) Moist heat sterilization at 121°C for 8 min.

[0020] Example 2 All ingredients are calculated based on 100g (1) Take 0.5 g of recombinant humanized type III collagen, 2 g of carboxymethyl chitosan, 1 g of trehalose, 1 g of sodium hyaluronate, 2.5 g of glycerol, 2.5 g of propylene glycol, 0.5 g of xanthan gum and 90 g of purified water for later use; (2) Dissolve 0.5 g of recombinant humanized type III collagen in 60 g of purified water to prepare a recombinant humanized type III collagen solution for later use; (3) Add 2 g of carboxymethyl chitosan, 1 g of trehalose, and 1 g of sodium hyaluronate to the recombinant type III humanized collagen solution in sequence, homogenize to obtain a mixture 1, and let stand for later use; (4) 2.5 g of glycerol, 2.5 g of propylene glycol, and 0.5 g of xanthan gum were dissolved in the remaining purified water (30 g), and the mixture was mechanically stirred at 100 rpm for 30 min to obtain a mixture II; (5) adding mixture 1 to mixture 2, mechanically stirring at 150 rpm for 20 min, and centrifuging at 4000 rpm for 10 min to degas, to obtain a dressing base solution; (6) adding the dressing base liquid into the non-woven fabric to prepare a gel dressing; (7) Moist heat sterilization at 121°C for 10 min.

[0021] Example 3 All ingredients are calculated based on 100g (1) Take 5 g of hydrophilic collagen, 0.5 g of carboxymethyl chitosan, 1 g of trehalose, 1 g of sodium hyaluronate, 5 g of propylene glycol, 0.5 g of xanthan gum and 87 g of purified water for later use; (2) Dissolve 5 g of hydrophilic collagen in 60 g of purified water to prepare a hydrophilic collagen solution for later use; (3) 0.5 g of carboxymethyl chitosan, 1 g of trehalose, and 1 g of sodium hyaluronate were sequentially added to the hydrophilic collagen solution, homogenized to obtain a mixture 1, and allowed to stand for later use; (4) 5 g of propylene glycol and 0.5 g of xanthan gum were dissolved in the remaining purified water (27 g), and the mixture was mechanically stirred at 200 rpm for 30 min to obtain a mixture II; (5) adding mixture 1 to mixture 2, mechanically stirring at 150 rpm for 20 min, and centrifuging at 4500 rpm for 8 min to degas, to obtain a dressing base solution; (6) adding the dressing base liquid into the non-woven fabric to prepare a gel dressing; (7) Moist heat sterilization at 121°C for 8 min.

[0022] Example 4 All ingredients are calculated based on 100g (1) Take 1 g of hydrophilic collagen, 1 g of carboxymethyl chitosan, 1 g of trehalose, 1 g of sodium hyaluronate, 5 g of glycerol, 0.5 g of carbomer and 90.5 g of purified water for later use; (2) Dissolve 1 g of hydrophilic collagen in 60 g of purified water to prepare a hydrophilic collagen solution for later use; (3) 1 g of carboxymethyl chitosan, 1 g of trehalose, and 1 g of sodium hyaluronate are sequentially added to the hydrophilic collagen solution, homogenized to obtain a mixture 1, and allowed to stand for later use; (4) 5 g of glycerol and 0.5 g of carbomer were dissolved in the remaining purified water (30.5 g), and the mixture was mechanically stirred at 200 rpm for 30 min to obtain a mixture II; (5) adding mixture 1 to mixture 2, mechanically stirring at 150 rpm for 20 min, and centrifuging at 4000 rpm for 10 min to degas, to obtain a dressing base solution; (6) adding the dressing base liquid into the non-woven fabric to prepare a gel dressing; (7) Moist heat sterilization at 121°C for 6 min.

[0023] Example 5 All ingredients are calculated based on 100g (1) Take 5 g of hydrophilic collagen, 2 g of carboxymethyl chitosan, 1 g of trehalose, 1 g of sodium hyaluronate, 5 g of glycerol, 0.5 g of xanthan gum and 85.5 g of purified water for later use; (2) Dissolve 5 g of hydrophilic collagen in 60 g of purified water to prepare a hydrophilic collagen solution for later use; (3) 2 g of carboxymethyl chitosan, 2 g of trehalose, and 1 g of sodium hyaluronate were sequentially added to the recombinant type III humanized collagen solution, homogenized to obtain a mixture 1, and allowed to stand for later use; (4) 5 g of glycerol and 0.5 g of xanthan gum were dissolved in the remaining purified water (25.5 g), and the mixture was mechanically stirred at 200 rpm for 30 min to obtain a mixture II; (5) adding mixture 1 to mixture 2, mechanically stirring at 150 rpm for 20 min, and centrifuging at 4000 rpm for 10 min to degas, to obtain a dressing base solution; (6) adding the dressing base liquid into the non-woven fabric to prepare a gel dressing; (7) Moist heat sterilization at 121°C for 9 min.

[0024] Example 6 All ingredients are calculated based on 100g (1) Take 5 g of recombinant humanized type III collagen, 2 g of carboxymethyl chitosan, 2 g of carboxymethyl chitin, 0.5 g of trehalose, 0.5 g of sodium hyaluronate, 1 g of glycerol, 0.5 g of xanthan gum and 88.5 g of purified water and set aside; (2) Dissolve 5 g of recombinant humanized type III collagen in 60 g of purified water to prepare a recombinant humanized type III collagen solution for later use; (3) Add 2 g of carboxymethyl chitosan, 2 g of carboxymethyl chitin, 0.5 g of trehalose, and 0.5 g of sodium hyaluronate to the recombinant type III humanized collagen solution and dissolve them completely to obtain a mixture 1, which is allowed to stand for later use; (4) 1 g of glycerol and 0.5 g of xanthan gum were dissolved in the remaining purified water (28.5 g), and the mixture was mechanically stirred at 200 rpm for 30 min to obtain a mixture II; (5) adding mixture 1 to mixture 2, mechanically stirring at 150 rpm for 20 min, and centrifuging at 4000 rpm for 10 min to degas, to obtain a dressing base solution; (6) adding the dressing base liquid into the non-woven fabric to prepare a gel dressing; (7) Moist heat sterilization at 121°C for 8 min.

[0025] Example 7 (1) Take 3 g of recombinant humanized type III collagen, 0.5 g of carboxymethyl chitosan, 0.5 g of carboxymethyl chitin, 0.1 g of trehalose, 0.1 g of sodium hyaluronate, 1 g of propylene glycol, 0.5 g of carbomer and 94.3 g of purified water and set aside; (2) Dissolve 3 g of recombinant humanized type III collagen in 60 g of purified water to prepare a recombinant humanized type III collagen solution for later use; (3) Add 0.5 g of carboxymethyl chitosan, 0.5 g of carboxymethyl chitin, 0.1 g of trehalose, and 0.1 g of sodium hyaluronate to the recombinant type III humanized collagen solution and dissolve them completely to obtain a mixture 1, which is allowed to stand for later use; (4) 1 g of propylene glycol and 0.5 g of carbomer were dissolved in the remaining purified water (34.3 g), and the mixture was mechanically stirred at 200 rpm for 30 min to obtain a mixture II; (5) adding mixture 1 to mixture 2, mechanically stirring at 150 rpm for 20 min, and centrifuging at 4000 rpm for 10 min to degas, to obtain a dressing base solution; (6) adding the dressing base liquid into the non-woven fabric to prepare a gel dressing; (7) Moist heat sterilization at 121°C for 8 min.

[0026] Example 8 (1) Take 2 g of hydrophilic collagen, 2 g of carboxymethyl chitosan, 0.5 g of carboxymethyl chitosan, 0.5 g of trehalose, 1 g of sodium hyaluronate, 1 g of glycerol, 0.5 g of propylene glycol, 0.5 g of carbomer and 92 g of purified water and set aside; (2) Dissolve 2 g of hydrophilic collagen in 60 g of purified water to prepare a hydrophilic collagen solution for later use; (3) Add 2 g of carboxymethyl chitosan, 0.5 g of carboxymethyl chitin, 0.5 g of trehalose, and 1 g of sodium hyaluronate to the hydrophilic collagen solution and dissolve them completely to obtain a mixture 1, which is allowed to stand for later use; (4) 1 g of glycerol, 0.5 g of propylene glycol, and 0.5 g of carbomer were dissolved in the remaining purified water (32 g), and the mixture was mechanically stirred at 200 rpm for 30 min to obtain a mixture II; (5) adding mixture 1 to mixture 2, mechanically stirring at 150 rpm for 20 min, and centrifuging at 4000 rpm for 10 min to degas, to obtain a dressing base solution; (6) adding the dressing base liquid into the non-woven fabric to prepare a gel dressing; (7) Moist heat sterilization at 121°C for 8 min.

[0027] Example 9 (1) Take 0.1 g of hydrophilic collagen, 0.05 g of carboxymethyl chitosan, 0.05 g of carboxymethyl chitin, 0.1 g of trehalose, 0.15 g of sodium hyaluronate, 1 g of glycerol, 0.1 g of xanthan gum and 98.45 g of purified water and set aside; (2) Dissolve 0.1 g of hydrophilic collagen in 60 g of purified water to prepare a hydrophilic collagen solution for later use; (3) Add 0.05 g of carboxymethyl chitosan, 0.05 g of carboxymethyl chitin, 0.1 g of trehalose, and 0.15 g of sodium hyaluronate to the hydrophilic collagen solution and dissolve them completely to obtain a mixture 1, which is allowed to stand for later use; (4) 1 g of glycerol and 0.1 g of xanthan gum were dissolved in the remaining purified water (38.45 g), and the mixture was mechanically stirred at 200 rpm for 30 min to obtain a mixture II; (5) adding mixture 1 to mixture 2, mechanically stirring at 150 rpm for 20 min, and centrifuging at 4000 rpm for 10 min to degas, to obtain a dressing base solution; (6) adding the dressing base liquid into the non-woven fabric to prepare a gel dressing; (7) Moist heat sterilization at 121°C for 9 min.

[0028] Example 10 All ingredients are calculated based on 100g (1) Take 0.05 g of recombinant humanized type III collagen, 0.01 g of hydrophilic collagen, 0.05 g of carboxymethyl chitosan, 0.15 g of carboxymethyl chitosan, 0.2 g of trehalose, 1 g of sodium hyaluronate, 5 g of glycerol, 1 g of xanthan gum and 92.54 g of purified water for later use; (2) Dissolve 0.05 g of recombinant humanized type III collagen and 0.01 g of hydrophilic collagen in 60 g of purified water to prepare a collagen solution for later use; (3) 0.05 g of carboxymethyl chitosan, 0.15 g of carboxymethyl chitosan, 0.2 g of trehalose, and 1 g of sodium hyaluronate were added to the collagen solution in sequence and dissolved completely to obtain a mixture 1, which was allowed to stand for later use; (4) 5 g of glycerol and 1 g of xanthan gum were dissolved in the remaining purified water (32.54 g), and the mixture was mechanically stirred at 200 rpm for 5 min to obtain a mixture II; (5) adding mixture 1 to mixture 2, mechanically stirring at 200 rpm for 30 min, and centrifuging at 4500 rpm for 10 min to degas, to obtain a dressing base solution; (6) adding the dressing base liquid into the non-woven fabric to prepare a gel dressing; (7) Moist heat sterilization at 121°C for 7 min.

[0029] Embodiment 11 All ingredients are calculated based on 100g (1) Take 0.1 g of recombinant humanized type III collagen, 0.02 g of hydrophilic collagen, 0.05 g of carboxymethyl chitosan, 0.1 g of carboxymethyl chitin, 0.05 g of trehalose, 0.15 g of sodium hyaluronate, 1 g of glycerol, 0.1 g of xanthan gum and 98.43 g of purified water for later use; (2) Dissolve 0.1 g of recombinant humanized type III collagen and 0.02 g of hydrophilic collagen in 60 g of purified water to prepare a collagen solution for later use; (3) 0.05 g of carboxymethyl chitosan, 0.1 g of carboxymethyl chitin, 0.05 g of trehalose, and 0.15 g of sodium hyaluronate were added to the collagen solution in sequence and dissolved completely to obtain a mixture 1, which was allowed to stand for later use; (4) 1 g of glycerol and 0.1 g of xanthan gum were dissolved in the remaining purified water (38.43 g), and the mixture was mechanically stirred at 200 rpm for 5 min to obtain a mixture II; (5) adding mixture 1 to mixture 2, mechanically stirring at 200 rpm for 30 min, and centrifuging at 4000 rpm for 15 min to degas, to obtain a dressing base solution; (6) adding the dressing base liquid into the non-woven fabric to prepare a gel dressing; (7) Moist heat sterilization at 121°C for 8 min.

[0030] Test Example 1: In vitro cytotoxicity test According to the method described in GB / T16886.5-2017 "Biological Evaluation of Medical Devices Part 5: In Vitro Cytotoxicity Test", the sample solution prepared in the above example was evaluated for in vitro cytotoxicity, and the viability of living cells was calculated by absorbance. If the viability dropped to <70% of the blank, it was potentially cytotoxic.

[0031] The results are shown in Table 1: Table 1. Cytotoxicity results

[0032] In Table 1, the negative control is high-density polyethylene, and the positive control is 5 mg / mL phenol solution. The results of the positive control and the negative control indicate the feasibility of this in vitro cytotoxicity experiment. The cell survival rate results of Examples 1-11 demonstrate that the cytotoxicity of the gel dressing prepared by the present invention is level 1, and has good cell safety.

[0033] Test Example 2: Skin irritation test According to the method described in GB / T16886.10-2017 "Biological Evaluation of Medical Devices Part 10: Irritation and Skin Sensitization Test", the samples prepared in the above examples were evaluated for skin irritation, and the primary irritation index was calculated after scoring the irritation reactions of the test samples and blank controls.

[0034] The results are shown in Table 2: Table 2. Skin irritation test results

[0035] The experimental results showed that there was no erythema and edema on the skin of the test site in each test group, the primary irritation index was less than 0.5, and the irritation reaction type was extremely mild.

[0036] Test Example 3: Pyrogen Test According to GB / T 16886.11-2021 "Biological Evaluation of Medical Devices Part 11: Systemic Toxicity Test", the test method was carried out in accordance with the 2020 edition of the Pharmacopoeia of the People's Republic of China, Part IV, General Rules 1142 Pyrogen Test Method, to verify whether the samples prepared in the above examples would cause pyrogenic reactions after intravenous injection into rabbits. Measurement criteria: Within 72 hours, the body temperature of the three rabbits increased by less than 0.6°C, and the total increase was less than 1.3°C, indicating that the experimental material contained no pyrogenic substances.

[0037] The results are shown in Table 3: Table 3. Heat source test results

[0038] The results in Table 3 show that the changes in the body temperature of the rabbits are all within the acceptable range of the Pharmacopoeia of the People's Republic of China, proving that the product developed by the present invention has no pyrogenicity.

[0039] Test Example 4: Comparison of the effects of liquid dressings Volunteers with 8 types of non-chronic wound injuries were selected, including postoperative suture wounds, abrasions, sunburns, puncture sites of puncture instruments, first-degree burn wounds, superficial second-degree burn wounds, laser / photon / acid peels / micro-plastic surgery / abrasion wounds, and dermatitis, with 10 volunteers in each group, half male and half female, aged 18 to 60 years old. The dressing prepared in Example 11 was used as the test product and applied to the 8 groups of subjects respectively.

[0040] Usage: Apply the dressing evenly to the damaged part of the skin, once in the morning and once in the evening, for 14 days. Professional testers will rate the volunteers.

[0041] The scoring criteria are as follows: Pigmentation score: According to the degree of pigmentation of the wound surface, it is divided into low (0-3 points), medium (4-6 points), and high (7-10 points). From 0 to 10 points, the degree of pigmentation of the wound surface gradually deepens.

[0042] Scarring score: The scarring of the wound surface is divided into low (0-3 points), medium (4-6 points), and high (7-10 points). From 0 to 10 points, the scarring degree of the wound surface gradually deepens.

[0043] Redness and swelling score: According to the redness and swelling of the wound surface, it is divided into low (0-3 points), medium (4-6 points), and high (7-10 points). From 0 to 10 points, the redness and swelling of the wound surface gradually increases.

[0044] Pain score: According to the pain of the wound surface, it is divided into low (0-3 points), medium (4-6 points), and high (7-10 points). From 0 to 10 points, the pain of the wound surface gradually increases.

[0045] According to the experience of wound healing, the lower the redness, swelling, pain, pigmentation and scarring at the wound healing site, the more ideal the wound healing is, and the better the effect of the tested sample is.

[0046] Therefore, the efficacy indicators are defined as follows: Significant effect: low scarring (0-3 points) + low pigmentation (0-3 points) + low redness and swelling (0-3 points) + low pain (0-3 points); Valid: Meet any of the following conditions: Low scarring (0-3 points) + moderate pigmentation (4-6 points) + low redness (0-3 points) + low pain (0-3 points); Moderate scarring (4-6 points) + low pigmentation (0-3 points) + low redness (0-3 points) + low pain (0-3 points); Moderate scarring (4-6 points) + moderate pigmentation (4-6 points) + low redness (0-3 points) + low pain (0-3 points); Invalid: Other cases are considered invalid.

[0047] Effectiveness = (number of people with significant effects + number of effective people) / 10 × 100% The results are shown in Table 4: Table 4. Statistical results of the effects of the subjects after 14 days of use

[0048] From the above data, it can be seen that the feedback from the test subjects of the test example of the present invention shows that the wound repair efficiency of the gel dressing prepared in Example 11 is ≥80%.

[0049] Although the present invention has been disclosed as above by way of embodiments, it is not intended to limit the present invention. Any person with ordinary knowledge in the technical field may make some changes and modifications without departing from the spirit and scope of the present invention. Therefore, the protection scope of the present invention shall be determined by the scope of the patent application attached hereto.

Claims

1. A multifunctional gel dressing that promotes wound repair. It is characterized in that The invention comprises the following components: collagen, polysaccharide polymer, moisturizing agent, excipient and purified water.

2. The multifunctional gel dressing according to claim 1, It is characterized in that The content of each component is as follows: collagen 0.01-5wt%, polysaccharide polymer 0.05-5wt%, moisturizer 1-5wt%, excipient 0.1-0.5wt%, and the balance is purified water.

3. The multifunctional gel dressing according to claim 1, It is characterized in that The collagen is resistant to irradiation sterilization.

4. The multifunctional gel dressing according to claim 3, It is characterized in that The collagen is one or both of recombinant type III humanized collagen and hydrophilic collagen.

5. The multifunctional gel dressing according to claim 4, It is characterized in that The hydrophilic collagen is: a hydrophilic collagen prepared by amidation modification of collagen extracted from animal tissue; The preparation method of the hydrophilic collagen comprises the following steps: washing the bovine Achilles tendon of animal tissue, removing the surface grease, soaking in sodium hydroxide to inactivate the virus, extracting with pepsin, purifying by salting out, hydrophilic grafting modification with succinic anhydride, precipitating the modified collagen, washing and freeze drying to obtain the hydrophilic collagen.

6. The multifunctional gel dressing according to claim 1, It is characterized in that The polysaccharide polymer is a polysaccharide combination of at least three of carboxymethyl chitosan, carboxymethyl chitin, trehalose and sodium hyaluronate.

7. The multifunctional gel dressing according to claim 1, It is characterized in that The moisturizing agent is one or two of glycerol and propylene glycol.

8. The multifunctional gel dressing according to claim 1, It is characterized in that The excipients are: one or two of xanthan gum and carbomer.

9. The multifunctional gel dressing according to claim 4 or 6, It is characterized in that The contents of the collagen and polysaccharide polymer are as follows: 0.05-5wt% of recombinant humanized type III collagen, 0.01-2wt% of hydrophilic collagen, 0.05-2wt% of carboxymethyl chitosan, 0.05-2wt% of carboxymethyl chitin, 0.05-2wt% of sodium hyaluronate, and 0.05-1wt% of trehalose.

10. A method for preparing the multifunctional gel dressing according to any one of claims 1 to 9, It is characterized in that The following steps are involved: (1) Prepare collagen, polysaccharide polymer, moisturizer, excipient and purified water for later use; (2) Dissolving collagen in purified water to prepare a collagen solution for later use; (3) adding polysaccharide polymers to the collagen solution in sequence and dissolving them completely to obtain a mixture 1, which is allowed to stand for later use; (4) mixing the moisturizing agent and the excipient uniformly to obtain a mixture 2; (5) adding mixture 1 to mixture 2, stirring evenly, and centrifuging to degas, thereby obtaining a dressing base solution; (6) adding the dressing base liquid into a carrier to prepare a gel dressing; (7) Moist heat sterilization at 121°C for 6-10 min.

11. The method for preparing the multifunctional gel dressing according to claim 10, It is characterized in that The gel dressing may or may not contain a nonwoven or gauze carrier.

Citation Information

Patent Citations

  • Medical dressing containing recombinant humanized collagen, and preparation method

    CN113117137A

  • Recombinant collagen dressing and preparation method thereof

    CN115137868A

  • Recombinant III-type humanized triple-helix structure collagen dressing

    CN115475277A

  • Hydrophilic composite collagen sponge and preparation method thereof

    CN116808279A

  • Modified recombinant humanized collagen and application thereof in vaginal dressing

    CN117327171A

Cited By

  • Anti-adhesion repair dressing for endometrium protection after intrauterine operation

    CN122297767A