Defoaming agent for coating as well as preparation method and application of defoaming agent
By using a specific proportion of the first and second polyether polyols and polysiloxanes in the defoaming agent, combined with heating and pressurization treatment, the problem of foam in the emulsion is solved, and more effective defoaming is achieved It also has the effect of suppressing foam, avoiding the entrainment of emulsion foam and covering materials, and improving the desolution efficiency.
Patent Information
- Application Number
- CN202411380963.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-30
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-09-30
AI Technical Summary
The prior art produces a large amount of foam when removing the organic solvent acetone in the emulsion, and the emulsion produces foam faster after the desolution process is optimized. The existing defoaming agent cannot eliminate the foam in time, affecting product packaging.
Provided is a coating defoaming agent, containing 10 parts to 20 parts of the first polyether polyol and 15 parts to 25 parts of the second polyether polyol, combined with polysiloxane and other components, prepared by stirring and standing, for use in Heating and pressurizing the emulsion to achieve rapid defoaming effect.
This defoaming agent can effectively inhibit the large amount of foam generated by the emulsion during the desolation process, prolong the foam suppression time, avoid the emulsion foam entrainment and material explosion, improve the vacuum efficiency, and do not affect the fineness and stability of the emulsion.
Smart Images

Figure BDA0005069894750000131
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of defoamer preparation, and specifically relates to a defoamer for coatings and a preparation method and application thereof. Background Art
[0002] Foam is a heterogeneous dispersion system in which a large number of bubbles are isolated from each other by the liquid when an insoluble gas enters the liquid under the action of external force. When foam is generated, the contact surface area between the liquid and the gas increases rapidly, and the free energy of the system also increases rapidly. The increased free energy of the foam system is directly related to the surface tension. The lower the surface tension, the smaller the free energy required for the system to form foam, and the easier it is to generate foam. In industrial production, foam will reduce production capacity, waste raw materials, reduce quality, and other hazards, which will have an adverse effect on production. Therefore, it is necessary to use a defoaming agent to achieve rapid defoaming.
[0003] The defoamer used in water-based paint always penetrates into the foam system in the form of latex particles. When the system generates foam for some reason, the defoamer particles immediately destroy the elastic membrane of the bubble and inhibit the generation of bubbles. If the foam already exists, the added defoamer will immediately capture the hydrophobic chain end on the foam surface after contacting the foam, and quickly replace the membrane wall of the original foam. Due to the low surface tension, the membrane wall of the foam can be gradually thinned, and the stress generated by the entire bubble is unbalanced, which leads to the rupture of the bubble. Therefore, the defoamer of water-based paint needs to meet the following requirements: ① It is insoluble in the foam medium or has extremely low solubility, which does not affect the performance of the product; ② The surface tension is lower than the surface tension of the foam medium; ③ It is easy to diffuse in the foam system and can replace the foam membrane wall; ④ It has a certain chemical stability; ⑤ It has the ability to be dispersed in the aqueous emulsion as suitable particles as the defoaming core.
[0004] Common water-based defoamers are mainly divided into two categories: ① Mineral oil defoamers; mineral oil defoamers are usually composed of carriers, active agents, and developing agents. The carrier is a substance with low surface tension, commonly water or fatty alcohols; common active agents are wax, silicone oil, aliphatic amides, and hydrophobic silica; ② Silicone; its active ingredients are mainly hydrophobic siloxanes, generally including polydimethylsiloxane and modified polydimethylsiloxane, and the effect is better when used in combination with other carrier surfactants.
[0005] When removing the organic solvent acetone from the emulsion, a large amount of foam will be generated. If the bubbles cannot be suppressed or quickly eliminated, it will affect the product packaging. Solvent removal accounts for a high proportion of the production cycle of waterborne polyurethane emulsion. At the same time, due to the characteristics of the product, some brands are very easy to foam during desolventizing. With the continuous optimization of the desolventizing process, the emulsion produces foam faster and the amount of foam increases. If the emulsion is not defoamed in time, the emulsion mist will be entrained to the vacuum unit to cause material overflow. At the same time, the generation of foam will affect the packaging of the product, so higher requirements are placed on the performance of the defoamer. Summary of the invention
[0006] Therefore, the first technical problem to be solved by the present invention is that a large amount of foam will be generated when removing the organic solvent acetone from the emulsion in the prior art; the second technical problem to be solved by the present invention is that the desolventizing process in the prior art is continuously optimized, the emulsion generates foam faster and in greater quantities, and the existing defoamer cannot remove the foam in time. The present invention provides a defoamer for coatings and its preparation method and application, which can solve the above technical problems without causing the problem of material overflow and affecting product packaging.
[0007] To this end, the present invention provides the following technical solutions.
[0008] The first aspect of the present invention provides a defoamer for coatings, which comprises, by weight, 10 to 20 parts of a first polyether polyol and 15 to 25 parts of a second polyether polyol;
[0009] The first polyether polyol uses sorbitol and glycerol as initiators, has an average functionality of 5 to 6, and a number average molecular weight of 500 to 1000;
[0010] The second polyether polyol uses propylene glycol as an initiator, has an average functionality of 2, and a number average molecular weight of 4000-6000.
[0011] In an optional embodiment, the first polyether polyol is R2490 polyether polyol; and / or,
[0012] The second polyether polyol is C2040D polyether polyol.
[0013] In an optional embodiment, the mass ratio of the first polyether polyol to the second polyether polyol is 1:1.
[0014] In an optional embodiment, the defoaming agent further comprises 25 to 45 parts of polysiloxane;
[0015] Preferably, the polysiloxane is polydimethylsiloxane.
[0016] In an optional embodiment, the defoaming agent further comprises a solvent and / or an auxiliary agent;
[0017] Preferably, the solvent is water;
[0018] Preferably, the auxiliary agent includes at least one of an emulsifier, a thickener and a stabilizer;
[0019] Preferably, the emulsifier includes at least one of sodium dodecyl sulfate, sodium dodecylbenzene sulfonate and sodium p-styrene sulfonate;
[0020] Preferably, the thickener comprises at least one of methyl cellulose, carboxymethyl cellulose and sodium carboxymethyl cellulose;
[0021] Preferably, the stabilizer comprises an organic rare earth stabilizer;
[0022] Preferably, the organic rare earth stabilizer includes at least one of a citric acid rare earth stabilizer and a lauric acid rare earth stabilizer.
[0023] In an optional embodiment, the defoamer includes, by weight, 25 to 45 parts of polysiloxane, 10 to 20 parts of R2490 polyether polyol, 15 to 25 parts of C2040D polyether polyol, 2 to 5 parts of emulsifier, 1 to 1.2 parts of thickener, 1 to 2 parts of stabilizer, and 80 to 100 parts of water;
[0024] Preferably, based on weight, the composition includes 40 parts of polysiloxane, 20 parts of R2490 polyether polyol, 20 parts of C2040D polyether polyol, 5 parts of emulsifier, 1 part of thickener, 2 parts of stabilizer and 90 parts of water.
[0025] The organic rare earth stabilizer includes a rare earth citric acid stabilizer and a rare earth lauric acid stabilizer. Among them, the rare earth citric acid stabilizer is a common stabilizer in the art, such as RE (Cit) nH2O, RE = La\Pr\Nd\Sm\Eu. The rare earth lauric acid stabilizer is a common stabilizer in the art, such as (Cit) nH2O, RE = La\Pr\Nd\Sm\Eu. 11 H 23 COO)3RE,RE=La\Sm.
[0026] The second aspect of the present invention provides a method for preparing the above-mentioned defoaming agent, comprising mixing the raw materials, stirring and standing;
[0027] Preferably, the preparation method is carried out at a temperature of 60°C to 80°C.
[0028] The third aspect of the present invention provides a desolventizing process, using the above-mentioned defoaming agent, including: adding the defoaming agent to the emulsion, and simultaneously heating and pressurizing the system so that the system reaches a first pressure, after the system stabilizes to a second pressure, adjusting the pressurization speed to bring the system to a third pressure, and maintaining the third pressure unchanged until a qualified emulsion is obtained.
[0029] In an optional embodiment, the emulsion is an aqueous emulsion;
[0030] Preferably, the amount of the defoaming agent added is 200ppm to 300ppm.
[0031] In an optional embodiment, the desolventizing process satisfies at least one of A to E:
[0032] A. The first pressure is not less than -75KPa;
[0033] B. The second pressure is not less than -85KPa and less than -75KPa;
[0034] C. The third pressure is not less than -96 KPa and less than -85 KPa;
[0035] D. The heating temperature is 38°C to 45°C;
[0036] E. Pressurize the system to reach the first pressure at a rate of 3 to 5 KPa / min.
[0037] The technical solution of the present invention has the following advantages:
[0038] 1. The defoamer for coating provided by the present invention comprises 10 to 20 parts of a first polyether polyol and 15 to 25 parts of a second polyether polyol; the first polyether polyol uses sorbitol and glycerol as initiators, has an average functionality of 5 to 6, and a number average molecular weight of 500 to 1000; the second polyether polyol uses propylene glycol as an initiator, has an average functionality of 2, and a number average molecular weight of 4000 to 6000. The defoamer can be used in an emulsion to remove and inhibit a large amount of foam generated when removing acetone, with better defoaming effect and longer foam inhibition time; the defoamer can also be applied to the desolventizing process after technological upgrading, overcoming the defect that the existing defoamer cannot effectively inhibit the occurrence of a large number of bubbles in the desolventizing process, and avoiding the occurrence of undesirable situations such as emulsion mist entrainment causing material overflow and affecting the product due to untimely defoaming. This defoamer is suitable for defoaming water-based emulsions such as polyurethane, polyurethane-acrylate, epoxy resin and polyacrylate, and does not affect the performance of the emulsion. After testing, the defoamer does not affect the fineness and stability of the emulsion, and after film formation, it will not clump and fall off.
[0039] The defoamer of the present invention comprises a first polyether polyol and a second polyether polyol. The first polyether polyol is a modified sorbitol polyether, which has good defoaming performance and a relatively special block structure. Compared with general polyethers, it has higher functionality and better dimensional stability, and can improve the system stability and fluidity of the defoamer. The first polyether polyol also has good low-temperature fluidity, lubricity and thermal stability. The oxygen atoms in the ether bonds can be hydrogen-bonded with the hydrogen atoms in the solvent water, and the molecular chain becomes zigzag. The hydrophobic groups are placed inside the molecules, and the chains are easily combined with the solvent water, thereby improving the defoaming effect of the defoamer. The second polyether polyol has a higher molecular weight, can more effectively destroy the stability of the foam, and has a better defoaming effect. The second polyether polyol molecule is larger, quickly diffuses into the foam film, reduces the surface tension, and achieves the purpose of rapid defoaming. The first polyether polyol and the second polyether polyol are used in combination to make the defoamer quickly defoam and have a better defoaming effect. When the defoamer is applied to the desolvation of the aqueous emulsion, there will be no problems such as a large amount of foam, and the foam suppression time is longer. DETAILED DESCRIPTION
[0040] The following examples are provided for a better understanding of the present invention, but are not intended to limit the best mode of implementation, nor to limit the content and protection scope of the present invention. Any product identical or similar to the present invention obtained by anyone under the inspiration of the present invention or by combining the features of the present invention with other prior arts shall fall within the protection scope of the present invention.
[0041] If no specific experimental steps or conditions are specified in the examples, the conventional experimental steps or conditions described in the literature in the field can be used. If no manufacturer is specified for the reagents or instruments used, they are all conventional reagent products that can be obtained commercially.
[0042] With the continuous improvement of the desolventizing process, the emulsion generates foam faster and in greater quantities. Existing defoamers are difficult to apply to the upgraded desolventizing process. In addition, a large amount of foam will be generated when removing the organic solvent acetone from the emulsion. In order to solve the above problems, the present invention provides a defoamer for coatings and a preparation method and application thereof, which adopts the following technical solution.
[0043] In the first aspect, the present invention provides a defoaming agent for coatings, which comprises, by weight, 10 to 20 parts of a first polyether polyol and 15 to 25 parts of a second polyether polyol; the first polyether polyol uses sorbitol and glycerol as initiators, has an average functionality of 5 to 6, and a number average molecular weight of 500 to 1000; the second polyether polyol uses propylene glycol as an initiator, has an average functionality of 2, and a number average molecular weight of 4000 to 6000.
[0044] The defoaming agent can be used in the emulsion to remove and inhibit a large amount of foam generated when removing acetone, with better defoaming effect and longer foam inhibition time; the defoaming agent can also be applied to the desolventizing process after technological upgrading, overcoming the defect that the existing defoaming agent cannot effectively inhibit the occurrence of a large number of bubbles in the desolventizing process, and avoiding the undesirable situation such as the entrainment of emulsion mist and foam causing material overflow and affecting the product due to untimely defoaming.
[0045] In an optional embodiment, the first polyether polyol is R2490 polyether polyol; and / or, the second polyether polyol is C2040D polyether polyol.
[0046] C2040 polyether polyol has a higher molecular weight than the polyether used in existing defoamers. High molecular weight polyethers usually have better defoaming effects and can more effectively destroy the stability of foam. C2040 polyether polyol has larger molecules and can quickly diffuse into the foam film, reducing surface tension and thus quickly defoaming. The bio-based polyether R2490 produced by Wanhua Chemical is introduced into the system. This polyether is a modified sorbitol polyether, which not only has good defoaming properties, but also has special blocks, which have higher functionality and better dimensional stability than general polyethers. Compared with other polyethers, it has the characteristics of improving the stability and fluidity of the defoamer system.
[0047] In an optional embodiment, the mass ratio of the first polyether polyol to the second polyether polyol is 1:1.
[0048] In an optional embodiment, the defoaming agent further comprises 25 to 45 parts of polysiloxane;
[0049] Preferably, the polysiloxane is polydimethylsiloxane. Polydimethylsiloxane has a high boiling point, poor solubility, very low surface tension, excellent defoaming ability, and can improve the defoaming effect of the defoaming agent. It should also be noted that the molecular weight of polydimethylsiloxane is 500-10000. Polydimethylsiloxane with a molecular weight of 500-10000 has a certain viscosity and can form a stable dispersion system in a liquid, providing a lasting defoaming effect, but still has a certain fluidity, quickly disperses into the system, and improves the defoaming rate. The molecular weight of polydimethylsiloxane is preferably 1000-5000 (e.g., 1500, 2000, 2500, 3000, 3500, etc.).
[0050] In an optional embodiment, the defoaming agent further comprises a solvent and / or an auxiliary agent;
[0051] Preferably, the solvent is water;
[0052] Preferably, the auxiliary agent includes at least one of an emulsifier, a thickener and a stabilizer;
[0053] Preferably, the emulsifier is at least one of sodium dodecyl sulfate, sodium dodecylbenzene sulfonate and sodium p-styrene sulfonate;
[0054] Preferably, the thickener is at least one of methyl cellulose, carboxymethyl cellulose and sodium carboxymethyl cellulose;
[0055] Preferably, the stabilizer is an organic rare earth stabilizer.
[0056] In a second aspect, the present invention provides a method for preparing the above-mentioned defoaming agent, comprising mixing the raw materials, stirring, and standing;
[0057] Preferably, the preparation method is carried out at a temperature of 60°C to 80°C.
[0058] In an optional embodiment, the stirring speed is 1300-1500 rpm, the stirring time is 60 min to 90 min, and the standing time is 60-80 min.
[0059] In a third aspect, the present invention provides a desolventizing process, using the above-mentioned defoaming agent, comprising:
[0060] The defoaming agent is added to the emulsion, and the system is heated and pressurized at the same time to make the system reach a first pressure, at which the system temperature is 38° C. to 45° C., and the pressurization rate is 3 to 5 KPa / min; after the system reaches the first pressure, acetone is quickly removed, and the system pressure is further reduced without applying external pressure. After the system is stabilized to the second pressure, the system pressure is adjusted at a pressurization speed of adjusting the valve opening by 10% every 5 minutes until the system reaches a third pressure, and the third pressure is kept unchanged until an emulsion with a qualified acetone content is obtained.
[0061] The present invention provides a defoamer for use in the emulsion desolventizing process, which can effectively inhibit the emulsion from generating a large amount of foam at -75KPa to -93KPa, and the foam suppression time is longer, avoiding the problem of material overflow due to vacuuming, and significantly reducing the number of half-barrel packaging caused by foaming during packaging. Heating and pressurizing are carried out simultaneously, avoiding the defect of the prior art that long-term heating is required to remove acetone, saving about 10% to 15% of the desolventizing time, and improving the vacuuming efficiency. It is understandable that the emulsion will generate a large amount of foam at -93KPa, and after adding the defoamer of the present invention, a large amount of foam will not be generated at this pressure, but it does not affect the third pressure, which is at least -96KPa.
[0062] The brands of raw materials used in the following examples are: R2490 polyether polyol and C2040D polyether polyol are from Wanhua Chemical, the manufacturer of rare earth citric acid and rare earth laurate is China North Rare Earth (Group) High-Tech Co., Ltd., the manufacturer of polydimethylsiloxane (molecular weight of about 2000) is Beijing Inokai Technology Co., Ltd., and other raw materials and equipment not specially specified are conventional raw materials.
[0063] Example 1
[0064] This embodiment provides a defoaming agent, which includes, by weight, 10 parts of R2490 polyether polyol, 20 parts of C2040D polyether polyol, 40 parts of polydimethylsiloxane, 3 parts of emulsifier sodium lauryl sulfate, 1 part of thickener methyl cellulose, 2 parts of stabilizer rare earth citrate RE (Cit) nH2O, RE = La\Pr\Nd\Sm\Eu and 85 parts of deionized water.
[0065] This embodiment also provides a method for preparing the above defoaming agent, comprising the following steps:
[0066] (1) Weigh 10 g of R2490 polyether polyol, 20 g of C2040D polyether polyol, 40 g of polydimethylsiloxane, 3 g of sodium lauryl sulfate, 1 g of thickener methylcellulose, 2 g of stabilizer rare earth citrate and 85 g of deionized water respectively and set aside; polydimethylsiloxane, R2490 and C2040D are stirred and mixed to form a first mixture; emulsifier sodium lauryl sulfate, thickener methylcellulose, stabilizer rare earth citrate and water are stirred and mixed to form a second mixture.
[0067] (2) After the first mixture and the second mixture are mixed, the mixture is stirred at a speed of 1500 rpm for 70 minutes and allowed to stand for 60 minutes to obtain a defoaming agent.
[0068] Wherein, step (1) and step (2) are both carried out in an environment of 80°C.
[0069] Example 2
[0070] This embodiment provides a defoaming agent, which includes, by weight, 20 parts of R2490 polyether polyol, 15 parts of C2040D polyether polyol, 40 parts of polydimethylsiloxane, 2 parts of emulsifier sodium lauryl sulfate, 1.2 parts of thickener carboxymethyl cellulose, 2 parts of stabilizer rare earth citrate and 80 parts of deionized water.
[0071] This embodiment also provides a method for preparing the above defoaming agent, comprising the following steps:
[0072] (1) Weigh 20 g of R2490 polyether polyol, 15 g of C2040D polyether polyol, 40 g of polydimethylsiloxane, 2 g of sodium lauryl sulfate, 1.2 g of thickener carboxymethyl cellulose, 2 g of stabilizer rare earth citrate and 80 g of deionized water respectively and set aside; polydimethylsiloxane, R2490 and C2040D are stirred and mixed to form a first mixture; water, emulsifier sodium lauryl sulfate, thickener carboxymethyl cellulose and stabilizer rare earth citrate are stirred and mixed to form a second mixture.
[0073] (2) After the first mixture and the second mixture are mixed, the mixture is stirred at a speed of 1500 rpm for 70 minutes and allowed to stand for 60 minutes to obtain a defoaming agent.
[0074] Wherein, step (1) and step (2) are both carried out in an environment of 60°C.
[0075] Example 3
[0076] This embodiment provides a defoaming agent, which includes, by weight, 10 parts of R2490 polyether polyol, 15 parts of C2040D polyether polyol, 45 parts of polydimethylsiloxane, 5 parts of emulsifier sodium lauryl sulfate, 1 part of thickener carboxymethyl cellulose, 1 part of stabilizer rare earth citrate and 85 parts of deionized water.
[0077] This embodiment also provides a method for preparing the above defoaming agent, comprising the following steps:
[0078] (1) Weigh 10 g of R2490 polyether polyol, 15 g of C2040D polyether polyol, 45 g of polydimethylsiloxane, 5 g of sodium lauryl sulfate, 1 g of thickener carboxymethyl cellulose, 1 g of stabilizer rare earth citrate and 85 g of deionized water respectively and set aside; polydimethylsiloxane, R2490 and C2040D are stirred and mixed to form a first mixture; water, emulsifier sodium lauryl sulfate, thickener carboxymethyl cellulose and stabilizer are stirred and mixed to form a second mixture.
[0079] (2) After the first mixture and the second mixture are mixed, the mixture is stirred at a speed of 1500 rpm for 70 minutes and allowed to stand for 60 minutes to obtain a defoaming agent.
[0080] Wherein, step (1) and step (2) are both carried out in an environment of 80°C.
[0081] Example 4
[0082] The present embodiment provides a defoaming agent, which comprises, by weight, 15 parts of R2490 polyether polyol, 25 parts of C2040D polyether polyol, 30 parts of polydimethylsiloxane, 5 parts of emulsifier sodium lauryl sulfate, 1 part of thickener sodium carboxymethyl cellulose, 2 parts of stabilizer rare earth laurate (C 11 H23 COO)3RE, RE = La\Sm and 100 parts of deionized water.
[0083] This embodiment also provides a method for preparing the above defoaming agent, comprising the following steps:
[0084] (1) Weigh 15 g of R2490 polyether polyol, 25 g of C2040D polyether polyol, 30 g of polydimethylsiloxane, 5 g of sodium lauryl sulfate, 1 g of thickener sodium carboxymethyl cellulose, 2 g of stabilizer rare earth laurate and 100 g of deionized water respectively and set aside; polydimethylsiloxane, R2490 and C2040D are stirred and mixed to form a first mixture; water, emulsifier sodium lauryl sulfate, thickener sodium carboxymethyl cellulose and stabilizer rare earth laurate are stirred and mixed to form a second mixture.
[0085] (2) After the first mixture and the second mixture are mixed, the mixture is stirred at a speed of 1500 rpm for 80 minutes and allowed to stand for 60 minutes to obtain a defoaming agent.
[0086] Wherein, step (1) and step (2) are both carried out in an environment of 70°C.
[0087] Example 5
[0088] This embodiment provides a defoaming agent, which includes, by weight, 20 parts of R2490 polyether polyol, 20 parts of C2040D polyether polyol, 40 parts of polydimethylsiloxane, 5 parts of emulsifier sodium lauryl sulfate, 1 part of thickener methyl cellulose, 2 parts of stabilizer rare earth citrate and 90 parts of deionized water.
[0089] This embodiment also provides a method for preparing the above defoaming agent, comprising the following steps:
[0090] (1) Weigh 20 g of R2490 polyether polyol, 20 g of C2040D polyether polyol, 40 g of polydimethylsiloxane, 5 g of sodium lauryl sulfate, 1 g of thickener methyl cellulose, 2 g of stabilizer rare earth citrate and 90 g of deionized water respectively and set aside; polydimethylsiloxane, R2490 and C2040D are stirred and mixed to form a first mixture; water, emulsifier sodium lauryl sulfate, thickener methyl cellulose and stabilizer are stirred and mixed to form a second mixture.
[0091] (2) After the first mixture and the second mixture are mixed, the mixture is stirred at a speed of 1500 rpm for 70 minutes and allowed to stand for 60 minutes to obtain a defoaming agent.
[0092] Wherein, step (1) and step (2) are both carried out in an environment of 80°C.
[0093] Comparative Example 1
[0094] This comparative example provides a defoamer, which is basically the same as Example 3, except that C2004 (Wanhua Chemical) is used instead of C2040D. C2004 uses propylene glycol as an initiator, has an average functionality of 2, and a number average molecular weight of 3000-4500.
[0095] Comparative Example 2
[0096] This comparative example provides a defoamer, which is basically the same as Example 3, except that R2305 (Wanhua Chemical) is used instead of R2490. R2305 is a polyether polyol based on glycerol as an initiator, with an average functionality of 3-4 and a number average molecular weight of 500-1000.
[0097] Application Example 1
[0098] This application example provides a defoaming process. The defoaming agents are from various embodiments and comparative examples. The commercially available polyether silicone defoaming agent BYK-025 produced by BYK is used as the control group.
[0099] 30L of aqueous polyurethane emulsion was added to the desolventizing kettle, and a defoamer (from each embodiment, comparative example and control group) was added when the emulsion desolventizing foaming height reached 15cm. The amount of defoamer added was 200ppm, and the defoaming time and the foam suppression time were observed and recorded. The results are shown in Table 1. Among them, the time from adding the defoamer to eliminating the foam height of 10cm was recorded as the defoaming time; the time for bubbles to be generated again refers to the time from eliminating the foam with a height of 10cm to the time when the foam height reaches 15cm again, which is recorded as the foam suppression time.
[0100] Table 1 Defoaming test results
[0101] Example Time to eliminate 10cm high foam Anti-foam time Example 1 3.0 seconds 17 minutes 20 seconds Example 2 3.4 seconds 15 minutes 33 seconds Example 3 3.6 seconds 15 minutes 7 seconds Example 4 3.2 seconds 16 minutes 18 seconds Example 5 2.2 seconds 19 minutes 39 seconds Comparative Example 1 4.2 seconds 13 minutes 10 seconds Comparative Example 2 3.9 seconds 11 minutes 41 seconds Control group 3.9 seconds 10 minutes 58 seconds
[0102] From the above results, the defoamer provided by the present invention has a significant defoaming effect, a short defoaming time and a longer foam suppression time. From Example 3 and Comparative Examples 1-2, when the present invention eliminates the same amount of foam, the defoaming time is shorter and the foam suppression time is longer. The first polyether polyol uses sorbitol and glycerol as initiators, with an average functionality of 5 to 6 and a number average molecular weight of 500 to 1000; the second polyether polyol uses propylene glycol as an initiator, with an average functionality of 2 and a number average molecular weight of 4000 to 6000, indicating that the first polyether polyol and the second polyether polyol are used in combination, which can more effectively destroy the stability of the foam, improve the defoaming effect, and have a longer foam suppression time. Compared with the defoamers of the prior art, such as BYK-025, the defoamer of the present invention has a significant effect.
[0103] Verify whether the defoamer affects the emulsion performance as follows:
[0104] Test method for thermal stability of emulsion: Place the polyurethane in an oven at 60°C and record the demulsification time of the emulsion.
[0105] Fineness test method: Use a scraper fineness meter to test the fineness of the emulsion.
[0106] Table 2 Properties of the emulsion before and after adding defoamer
[0107]
[0108] Note: This invention only investigates the stability of waterborne polyurethane emulsion after adding defoamer, and does not investigate the stability of emulsion without defoamer. "-" in the table means that the data does not exist.
[0109] It can be seen from the above results that when the defoaming agent of the present invention is applied to the emulsion, it will not affect the properties of the emulsion, such as stability, fineness, etc.; after the emulsion forms a film, there will be no problems such as agglomeration and falling off.
[0110] Application Example 2
[0111] This application example provides a defoaming process. The defoaming agents are from various embodiments and comparative examples. The commercially available polyether silicone defoaming agent BYK-025 produced by BYK is used as the control group.
[0112] Add the aqueous polyurethane emulsion to the desolventizing kettle, add 200ppm defoamer to the aqueous polyurethane emulsion, and stir and mix for 10 minutes. The external circulation heat exchanger is connected in series with the kettle jacket to heat the system, so that the system temperature is controlled at 38-40°C. While heating, adjust the pressure of the desolventizing kettle to -75KPa with 5KPa, and close the valve when the pressure stabilizes at -75KPa. The acetone in the system is quickly removed. Since the removal of acetone will further reduce the pressure of the system, when the pressure stabilizes to -81KPa, open the valve 10% every 5 minutes until the system stabilizes at -96KPa, and further remove acetone until the aqueous polyurethane emulsion with qualified acetone content is obtained. Among them, the time when the foam height is 15cm is recorded, and the results are shown in Table 3.
[0113] Table 3 Defoaming test results
[0114] Example Time to generate 15cm high foam Example 1 32min Example 2 28min Example 3 26min Example 4 30min Example 5 37min Comparative Example 1 21min Comparative Example 2 19min Control group 15min
[0115] It can be seen from the above results that when the defoamer of the present invention is added to the aqueous polyurethane emulsion, the time for the foam to appear at a height of 15 cm is longer, indicating that the defoamer of the present invention has a good foam suppression effect.
[0116] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from these are still within the scope of protection of the invention.
Claims
1. A defoamer for coatings, characterized in that: In parts by weight, it comprises 10 to 20 parts of a first polyether polyol and 15 to 25 parts of a second polyether polyol; The first polyether polyol uses sorbitol and glycerol as initiators, has an average functionality of 5 to 6, and a number average molecular weight of 500 to 1000; The second polyether polyol uses propylene glycol as an initiator, has an average functionality of 2, and a number average molecular weight of 4000-6000.
2. The defoamer for coating according to claim 1, characterized in that The first polyether polyol is R2490 polyether polyol; and / or, The second polyether polyol is C2040D polyether polyol.
3. The defoamer for coating according to claim 2, characterized in that The mass ratio of the first polyether polyol to the second polyether polyol is 1:
1.
4. The defoaming agent for coating according to any one of claims 1 to 3, characterized in that Also includes 25 to 45 parts of polysiloxane; Preferably, the polysiloxane is polydimethylsiloxane.
5. The defoaming agent for coating according to any one of claims 1 to 4, characterized in that Also includes solvents and / or additives; Preferably, the solvent is water; Preferably, the auxiliary agent includes at least one of an emulsifier, a thickener and a stabilizer; Preferably, the emulsifier includes at least one of sodium dodecyl sulfate, sodium dodecylbenzene sulfonate and sodium p-styrene sulfonate; Preferably, the thickener comprises at least one of methyl cellulose, carboxymethyl cellulose and sodium carboxymethyl cellulose; Preferably, the stabilizer comprises an organic rare earth stabilizer; Preferably, the organic rare earth stabilizer includes at least one of a citric acid rare earth stabilizer and a lauric acid rare earth stabilizer.
6. The defoaming agent for coating according to claim 5, characterized in that In parts by weight, it includes 25 to 45 parts of polysiloxane, 10 to 20 parts of R2490 polyether polyol, 15 to 25 parts of C2040D polyether polyol, 2 to 5 parts of emulsifier, 1 to 1.2 parts of thickener, 1 to 2 parts of stabilizer, and 80 to 100 parts of water; Preferably, based on weight, the composition includes 40 parts of polysiloxane, 20 parts of R2490 polyether polyol, 20 parts of C2040D polyether polyol, 5 parts of emulsifier, 1 part of thickener, 2 parts of stabilizer and 90 parts of water.
7. The method for preparing the defoaming agent according to any one of claims 1 to 6, characterized in that: It includes stirring and standing the raw materials after mixing; Preferably, the preparation method is carried out at a temperature of 60°C to 80°C.
8. A desolventizing process, characterized in that: The method of using the defoaming agent according to any one of claims 1 to 6 comprises: adding the defoaming agent to the emulsion, and simultaneously heating and pressurizing the system so that the system reaches a first pressure, and after the system stabilizes to a second pressure, adjusting the pressurization speed so that the system reaches a third pressure, and maintaining the third pressure unchanged until a qualified emulsion is obtained.
9. The desolventizing process according to claim 8, characterized in that: The emulsion is an aqueous emulsion; Preferably, the amount of the defoaming agent added is 200ppm to 300ppm.
10. The desolventizing process according to claim 8 or 9, characterized in that: Satisfy at least one of A to E: A. The first pressure is not less than -75KPa; B. The second pressure is not less than -85KPa and less than -75KPa; C. The third pressure is not less than -96 KPa and less than -85 KPa; D. The heating temperature is 38°C to 45°C; E. Pressurize the system to reach the first pressure at a rate of 3 to 5 KPa / min.
Citation Information
Patent Citations
Polyurethane foam composite and preparation method thereof and polyurethane foam composite
CN106496504A
Polyurethane rigid foam compound for pipeline heat insulation, and preparation method of polyurethane rigid foam compound
CN107868218A
Organosilicon surfactant and application thereof in preparation of polyurethane rigid foams
CN111393655A
Nitrogen and sulfur doped porous carbon electrode material and preparation method and application thereof