Preparation method of novel heterogeneous enhanced anion exchange membrane

By plasma surface treatment of the porous support net and plated with inorganic crystals, the problems of uneven distribution and shedding of inorganic substances in traditional heterogeneous enhanced anion exchange membrane are solved, the mechanical and electrochemical properties of the membrane are improved, and the Lifespan and reduce costs.

CN118949706APending Publication Date: 2024-11-15GUANGDONG MINGYANG TECH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411134009.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The traditional heterogeneous enhanced anion exchange membrane has uneven distribution of inorganic substances in the cast film liquid and is prone to fall off, resulting in electrolyte contamination and insufficient mechanical and electrochemical performance.

Method used

By plasma surface treatment of the porous support mesh, thin inorganic crystals are plated to improve its hydrophilicity and bond strength with the support mesh, forming a more uniform casting film liquid combined with the support mesh to avoid the inorganic substances falling off.

Benefits of technology

It improves the mechanical and electrochemical properties of the anion exchange membrane, extends the service life, reduces replacement costs, and avoids electrolyte contamination.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention discloses a novel heterogeneous enhanced anion exchange membrane preparation method, which comprises: carrying out plasma surface treatment on a porous support net, sequentially soaking in a first metal salt solution and a second anion salt solution, and uniformly coating the surface of the porous support net with a membrane casting solution to carry out membrane casting. Plasma surface treatment is carried out on the porous supporting net, so that the hydrophilicity of the surface of the porous supporting net is improved, and the bonding strength of inorganic salt and a porous supporting net framework is improved; secondly, a layer of thin inorganic substance crystals is plated on a porous supporting net framework subjected to plasma surface treatment, so that the hydrophilicity of the porous supporting net framework is better improved, a membrane casting solution can be uniformly infiltrated into the supporting net, and the membrane casting solution and the supporting net can be better combined together and are more firmly combined; the hidden danger that the supporting net falls off is avoided, the mechanical performance and electrochemical performance of the anion-exchange membrane are well improved, the service life of the anion-exchange membrane is prolonged, and the cost is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of electrochemical technology, in particular to a preparation method of a novel heterogeneous enhanced anion exchange membrane. Background Art

[0002] At present, there are three main routes for hydrogen production: 1) Hydrogen production from fossil energy reforming represented by coal and natural gas; 2) Hydrogen production from industrial by-product gas represented by coke oven gas, chlor-alkali tail gas, and propane dehydrogenation; 3) Hydrogen production from water electrolysis. In addition, there are other ways to produce hydrogen, including biomass hydrogen production, solar photocatalytic water decomposition hydrogen production, and nuclear energy hydrogen production. With the growth of hydrogen demand, the depletion of fossil energy, and the deterioration of the ecological environment, green hydrogen production has attracted more and more attention, and the development path of the hydrogen energy supply system has gradually developed towards the goal of achieving a green, economic, efficient and renewable hydrogen energy supply system. With the development of science and technology, water electrolysis hydrogen production and energy storage technology, as a clean and efficient energy storage method, is gradually attracting global attention and research. Water electrolysis hydrogen production technology is mainly divided into four major technologies: alkaline aqueous solution electrolysis (ALK), proton exchange membrane electrolysis (PEM), anion exchange membrane electrolysis (AEM) and solid oxide (SOEC). Among them, anion exchange membrane electrolysis (AEM) is considered to be a hydrogen production technology with great development prospects due to its unique low cost and high efficiency advantages.

[0003] Anion exchange membrane (AEM) is a type of polymer membrane that contains alkaline active groups and has selective permeability to anions, also known as ion selective permeability membrane. Anion exchange membrane consists of three parts: a polymer main chain with fixed groups, namely a polymer matrix (base membrane), a positively charged active group (cation), and anions that can move freely on the active group. The anion exchange membrane is the key part of the anion exchange membrane fuel cell, playing a dual role of transmitting anions and blocking gases in the fuel cell. The quality of its performance directly affects the service life of the fuel cell. In addition to excellent electrochemical properties, good mechanical properties and thermal stability are also essential.

[0004] According to the structure of the membrane, it can be divided into three categories: homogeneous, semi-homogeneous and heterogeneous. Homogeneous and semi-homogeneous have excellent electrochemical properties, but their physical properties are poor, so people have turned their attention to heterogeneous anion exchange membranes.

[0005] Traditional heterogeneous enhanced anion exchange membranes are usually prepared by blending inorganic substances such as zirconium dioxide, calcium carbonate, and barium sulfate into a casting solution containing an organic solvent, and then coating the mixture on the surface of a porous reinforcement layer to form a membrane, such as CN116272397 A; or coating different amounts of inorganic substances on the membrane surface, such as CN 117046317 A, to improve the hydrophilicity of the casting solution, increase the wettability with the porous support layer, or reduce the "microgap" between the membrane electrode, thereby improving the mechanical properties of the anion exchange membrane.

[0006] However, this traditional heterogeneous enhanced anion exchange membrane has very fatal shortcomings: 1. It is well known that inorganic substances such as zirconium oxide, calcium carbonate, and barium sulfate are not soluble in organic solvents. If they are directly doped in them, the size of their particle distribution in the casting solution cannot be guaranteed, and they are unevenly dispersed in the membrane, which is easy to agglomerate, which may lead to blockage of the support mesh and ion permeation channels, thereby reducing the electrochemical performance. 2. The inorganic substances distributed in the anion exchange membrane will gradually fall off as the resin is consumed during the use of the electrolytic cell. The detached inorganic substances enter the electrolyte, causing electrolyte pollution, shortening the life of the electrolytic cell, and leading to increased replacement costs and environmental pollution. 3. The anion exchange membrane doped with inorganic substances has a rough and uneven membrane surface due to the insolubility of the inorganic substances, which affects the subsequent spraying of the membrane electrode catalyst. Therefore, as the core part of the electrolytic cell, the preparation of a new type of heterogeneous enhanced anion exchange membrane has become an important problem in today's society. Summary of the invention

[0007] The object of the present invention is to overcome at least one disadvantage of the prior art and to provide a method for preparing a novel heterogeneous enhanced anion exchange membrane.

[0008] The technical solution adopted by the present invention is: The present invention provides a method for preparing a heterogeneous enhanced anion exchange membrane, comprising the following steps: 1) Plasma surface treatment of the porous support mesh; 2) immersing the porous support mesh that has been subjected to plasma surface treatment in a first metal salt solution; 3) soaking the porous support mesh obtained by the treatment in step 2) in a second anion salt solution; 4) uniformly coating the casting solution on the surface of the porous support mesh obtained in step 3) to cast a film, thereby obtaining the heterogeneous enhanced anion exchange membrane; Wherein, the first metal salt solution is selected from at least one of calcium salt, barium salt, zirconium salt, strontium salt and cerium salt solutions; The second anion salt solution is selected from at least one of sulfate and carbonate. The sulfate is selected from at least one of sodium sulfate, magnesium sulfate and potassium sulfate, and the carbonate is selected from at least one of sodium carbonate, potassium carbonate and ammonium carbonate. By using sulfate or carbonate to generate corresponding insoluble inorganic salts, a thin layer of inorganic crystals is plated on the porous support network skeleton that has been subjected to plasma surface treatment.

[0009] In some examples, the power of the plasma surface treatment is 7-12 kw, and the treatment time is 10 s-1 min.

[0010] In some examples, the concentration of the first metal salt solution is 1-5 mol / L.

[0011] In some examples, the concentration of the second anion salt solution is 1-5 mol / L.

[0012] In some examples, the porous support network is selected from any one of polyphenylene sulfide, polyether ketone, and polypropylene.

[0013] In some examples, the porous support network has a thickness of 20 to 150 μm.

[0014] In some examples, the solid content of the casting solution is 10-33 wt %.

[0015] In some examples, the casting solution is prepared by heating and stirring an organic high molecular polymer and an organic solvent to obtain the casting solution.

[0016] In some examples, the organic high molecular polymer is selected from at least one of polyaryl-piperidine polymers, polyaryl-alkylene polymers, polybiphenyl alkyl polymers, styrene polymers, polyether polymers, polysulfone polymers, and polytetrafluoroethylene polymers.

[0017] In some examples, the mass ratio of the organic high molecular polymer to the organic solvent is 1:2 to 1:420.

[0018] In some examples, the heating temperature is 50-120°C.

[0019] The above technical features can be combined arbitrarily without contradiction.

[0020] The beneficial effects of the present invention are: The invention changes the object of improving hydrophilicity to change the traditional heterogeneous enhanced anion exchange membrane for improving the hydrophilicity of the casting solution into a novel heterogeneous enhanced anion exchange membrane for improving the hydrophilicity of the porous support network.

[0021] First, the porous support mesh is subjected to plasma surface treatment, and different components of gas are used to generate different active species in the plasma under the action of the electromagnetic field, such as using hydrogen-containing, nitrogen-containing or oxygen-containing components as plasma gas or plasma gas loaded with saturated water vapor. The high-energy particles and photons generated by the plasma interact violently with the surface of the porous support mesh in the air, such as surface cleaning, surface pollutant dissociation, surface etching, increasing the adhesion on the porous support mesh skeleton, improving the adhesion of subsequent inorganic salt crystals on the skeleton, and generating a large number of polar groups on the surface of the porous support mesh, such as -NH2, -COOH and -OH, thereby improving the hydrophilicity of the porous support mesh surface and improving the bonding strength between the inorganic salt and the porous support mesh skeleton.

[0022] Secondly, a thin layer of inorganic crystals is plated on the porous support mesh skeleton that has been treated with plasma surface, which improves its hydrophilicity and allows the casting liquid to evenly infiltrate the support mesh. Under the action of gravity, the support mesh plated with inorganic substances is firmly wrapped by the casting liquid, which wraps it in a capsule. This sandwich structure solves the problem of pollution caused by the shedding of inorganic substances in traditional heterogeneous enhanced anion exchange membranes, and also solves the problem of subsequent membrane electrode catalyst spraying caused by uneven distribution of inorganic substances clogging the mesh and poor appearance. By improving the hydrophilicity of the support mesh and improving its wettability, the casting liquid and the support mesh can be well combined and more firmly combined, avoiding the hidden danger of the support mesh shedding, greatly improving the mechanical and electrochemical properties of the anion exchange membrane, increasing its lifespan, and reducing costs. DETAILED DESCRIPTION

[0023] The following disclosure provides many different implementations or examples for implementing different solutions of the present invention. The proportions of organic high molecular polymer and organic solvent in the casting solution mentioned in the following examples and comparative examples are all proportions by mass.

[0024] The purpose of plasma surface treatment is to clean, etch and hydrophilize the porous support mesh. In the following examples, unless otherwise specified, the specific process of plasma surface treatment is as follows: cut out a 10×10 cm 2 Put the polyphenylene sulfide mesh into the normal pressure plasma cleaning cabin, set the power to 7kw~12kw, set the processing time to 10s~1min, close the cabin door, click start, and after the plasma spray gun finishes spraying the plasma flame, click stop, take out the sample, and use a dyne pen to confirm until the plasma surface treatment is completed.

[0025] Example 1 1) According to the mass fraction, 10×10 cm 2The polyphenylene sulfide mesh that has been treated with plasma surface is immersed in a 1 mol / L barium salt solution and ultrasonically treated for 30 seconds, then taken out and allowed to stand and then ultrasonically contacted with a 1 mol / L sodium sulfate solution, and a polyphenylene sulfide mesh containing barium sulfate is obtained after crystallization on its skeleton; 2) Add 1 part of poly (aryl-piperidine) polymer and 4 parts of DMF into a beaker, heat at 120°C, stir at 200 r / min, stir evenly to make it completely dissolved, filter, and vacuum degas to obtain a casting solution; 3) The casting liquid is uniformly coated on the surface of the polyphenylene sulfide mesh cloth containing barium sulfate and then placed in an oven for baking and curing to obtain a novel heterogeneous enhanced anion exchange membrane.

[0026] Example 2 1) According to the mass fraction, 10×10 cm 2 The polyphenylene sulfide mesh that has been treated with plasma surface is immersed in a 1 mol / L calcium salt solution and ultrasonically treated for 30 seconds, then taken out and allowed to stand and then ultrasonically contacted with a 2 mol / L sodium carbonate solution, and a polyphenylene sulfide mesh containing calcium carbonate is obtained after crystallization on its skeleton; 2) Add 1 part of poly (aryl-piperidine) polymer and 4 parts of DMF into a beaker, heat at 120°C, stir at 200 r / min, stir evenly to make it completely dissolved, filter, and vacuum degas to obtain a casting solution; 3) The casting liquid is uniformly coated on the surface of the polyphenylene sulfide mesh cloth containing calcium carbonate and then placed in an oven for baking and curing to obtain a novel heterogeneous enhanced anion exchange membrane.

[0027] Example 3 1) According to the mass fraction, 10×10 cm 2 The plasma surface treated polyphenylene sulfide mesh was immersed in a 1 mol / L strontium salt solution and ultrasonically treated for 30 seconds, then taken out and allowed to stand and then ultrasonically contacted with a 5 mol / L sodium sulfate solution, and a polyphenylene sulfide mesh containing strontium sulfate was obtained after crystallization on its skeleton; 2) Add 1 part of poly (aryl-piperidine) polymer and 4 parts of DMF into a beaker, heat at 120°C, stir at 200 r / min, stir evenly to make it completely dissolved, filter, and vacuum degas to obtain a casting solution; 3) The casting liquid is uniformly coated on the surface of the polyphenylene sulfide mesh cloth containing strontium sulfate and then placed in an oven for baking and curing to obtain a novel heterogeneous enhanced anion exchange membrane.

[0028] Example 4 1) According to the mass fraction, 10×10 cm 2The plasma surface treated polyetheretherketone mesh was immersed in a 1 mol / L calcium salt solution and ultrasonically treated for 30 seconds, then taken out and allowed to stand and then ultrasonically contacted with a 1 mol / L sodium carbonate solution, and polyetheretherketone mesh containing calcium carbonate was obtained after crystallization on its skeleton; 2) Add 1 part of poly (aryl-piperidine) polymer and 4 parts of DMF into a beaker, heat at 120°C, stir at 200 r / min, stir evenly to make it completely dissolved, filter, and vacuum degas to obtain a casting solution; 3) The casting liquid is uniformly coated on the surface of the polyetheretherketone mesh cloth and then placed in an oven for baking and curing to obtain a novel heterogeneous enhanced anion exchange membrane.

[0029] Example 5 1) According to the mass fraction, 10×10 cm 2 The polyphenylene sulfide mesh that has been subjected to plasma surface treatment is immersed in a 1 mol / L calcium salt solution and ultrasonically treated for 30 seconds, then taken out and allowed to stand and then ultrasonically contacted with a 1 mol / L sodium carbonate solution, and a polyphenylene sulfide mesh containing calcium carbonate is obtained after crystallization on its skeleton; 2) Add 1 part of poly(biphenyl alkyl) polymer and 4 parts of DMF into a beaker, heat at 120°C, stir at 200 r / min, stir evenly to make it completely dissolved, filter, and vacuum degas to obtain a casting solution; 3) The casting liquid is uniformly coated on the surface of the polyphenylene sulfide mesh cloth containing calcium carbonate and then placed in an oven for baking and curing to obtain a novel heterogeneous enhanced anion exchange membrane.

[0030] Example 6 1) According to the mass fraction, 10×10 cm 2 The polyphenylene sulfide mesh that has been subjected to plasma surface treatment is immersed in a 1 mol / L calcium salt solution and ultrasonically treated for 30 seconds, then taken out and allowed to stand and then ultrasonically contacted with a 1 mol / L sodium carbonate solution, and a polyphenylene sulfide mesh containing calcium carbonate is obtained after crystallization on its skeleton; 2) Add 1 part of poly(aryl-piperidine) polymer and 9 parts of DMF into a beaker, heat at 120°C, stir at 200 r / min, stir evenly to dissolve completely, filter, and vacuum degas to obtain a casting solution; 3) The casting liquid is uniformly coated on the surface of the polyphenylene sulfide mesh cloth containing calcium carbonate and then placed in an oven for baking and curing to obtain a novel heterogeneous enhanced anion exchange membrane.

[0031] Example 7 1) According to the mass fraction, 10×10 cm 2The polyphenylene sulfide mesh that has been subjected to plasma surface treatment is immersed in a 1 mol / L calcium salt solution and ultrasonically treated for 30 seconds, then taken out and allowed to stand and then ultrasonically contacted with a 1 mol / L sodium carbonate solution, and a polyphenylene sulfide mesh containing calcium carbonate is obtained after crystallization on its skeleton; 2) Add 1 part of poly (aryl-piperidine) polymer and 4 parts of DMSO into a beaker, heat at 120°C, stir at 200 r / min, stir evenly to dissolve completely, filter, and vacuum degas to obtain a casting solution; 3) The casting liquid is uniformly coated on the surface of the polyphenylene sulfide mesh cloth containing calcium carbonate and then placed in an oven for baking and curing to obtain a novel heterogeneous enhanced anion exchange membrane.

[0032] Comparative Example 1 1) According to the weight percentage, 1 part of poly (aryl-piperidine) polymer and 4 parts of DMF were added into a beaker, heated at 120°C, stirred at 200 r / min, stirred evenly to make it completely dissolved, then 10wt% of barium sulfate solid powder was added, stirred evenly, filtered, and vacuum degassed to obtain a casting solution containing barium sulfate; 2) Place the casting solution containing barium sulfate in a 10×10 cm 2 The polyphenylene sulfide mesh cloth is uniformly coated on the surface and then placed in an oven for baking and curing to obtain a heterogeneous enhanced anion exchange membrane.

[0033] Comparative Example 2 1) According to the weight percentage, 1 part of poly (aryl-piperidine) polymer and 4 parts of DMF were added into a beaker, heated at 120°C, stirred at 200 r / min, stirred evenly to make it completely dissolved, then 10wt% of calcium carbonate solid powder was added, stirred evenly, filtered, and vacuum degassed to obtain a casting solution containing calcium carbonate; 2) Place the casting solution containing calcium carbonate in a 10×10 cm 2 The polyphenylene sulfide mesh cloth is uniformly coated on the surface and then placed in an oven for baking and curing to obtain a heterogeneous enhanced anion exchange membrane.

[0034] Comparative Example 3 1) According to the weight percentage, 1 part of poly (aryl-piperidine) polymer and 4 parts of DMF were added into a beaker, heated at 120°C, stirred at 200 r / min, stirred evenly to make it completely dissolved, then 10wt% of strontium sulfate solid powder was added, stirred evenly, filtered, and vacuum degassed to obtain a casting solution containing strontium sulfate; 2) Place the casting solution containing strontium sulfate in a 10×10 cm 2 The polyphenylene sulfide mesh cloth is uniformly coated on the surface and then placed in an oven for baking and curing to obtain a heterogeneous enhanced anion exchange membrane.

[0035] Comparative Example 4 1) According to the mass fraction, 10×10 cm 2 The polyphenylene sulfide mesh cloth which has not been subjected to plasma surface treatment is immersed in a 1 mol / L barium salt solution and ultrasonically treated for 30 seconds, and then taken out and allowed to stand and then ultrasonically contacted with a 1 mol / L sodium sulfate solution, and a polyphenylene sulfide mesh cloth containing barium sulfate is obtained after crystallization on its skeleton; 2) Add 1 part of poly (aryl-piperidine) polymer and 4 parts of DMF into a beaker, heat at 120°C, stir at 200 r / min, stir evenly to make it completely dissolved, filter, and vacuum degas to obtain a casting solution; 3) The casting liquid is uniformly coated on the surface of the polyphenylene sulfide mesh cloth containing barium sulfate and then placed in an oven for baking and curing to obtain a heterogeneous enhanced anion exchange membrane.

[0036] The test method is as follows: 1) Chloride ion conductivity at 25℃ mS / cm: tested according to (GB / T 20042.3-2022); 2) Tensile strength: tested according to (GB / T 20042.3-2022); 3) Alkali loss: tested according to (JC211-77); 4) Surface roughness Ra: Tested according to (GB / T 31227-2014).

[0037] The performance test comparison of the heterogeneous enhanced anion exchange membranes prepared in different examples is shown in Table 1.

[0038] Table 1. Performance test comparison of heterogeneous enhanced anion exchange membranes prepared in different examples

[0039] It can be seen from Comparative Examples 1-3 that, compared with doping inorganic salts in the casting liquid, coating a thin layer of inorganic crystals on the porous support mesh skeleton that has been subjected to plasma surface treatment improves the hydrophilicity of the support mesh and improves its wettability, so that the casting liquid and the support mesh can be well combined together and more firmly combined, avoiding the hidden danger of the support mesh falling off, greatly improving the mechanical and electrochemical properties of the anion exchange membrane, increasing its lifespan and reducing costs.

[0040] It can be seen from Comparative Example 4 that after the plasma treatment, the hydrophilicity of the surface of the porous support network is effectively improved, and the bonding strength between the inorganic salt and the porous support network skeleton is improved.

[0041] The above is a further detailed description of the present invention, which should not be regarded as a limitation on the specific implementation of the present invention. For ordinary technicians in the technical field to which the present invention belongs, simple deduction or replacement without departing from the concept of the present invention is within the protection scope of the present invention.

Claims

1. A method for preparing a novel heterogeneous enhanced anion exchange membrane, characterized in that: The following steps are involved: 1) Plasma surface treatment of the porous support mesh; 2) immersing the porous support mesh that has been subjected to plasma surface treatment in a first metal salt solution; 3) soaking the porous support mesh obtained by the treatment in step 2) in a second anion salt solution; 4) uniformly coating the casting solution on the surface of the porous support mesh obtained in step 3) to cast a film, thereby obtaining the heterogeneous enhanced anion exchange membrane; Wherein, the first metal salt solution is selected from at least one of calcium salt, barium salt, zirconium salt, strontium salt and cerium salt solutions; The second anion salt solution is selected from at least one of sulfate and carbonate.

2. The preparation method according to claim 1, characterized in that: The concentration of the first metal salt solution is 1-5 mol / L.

3. The preparation method according to claim 1, characterized in that: The concentration of the second anion salt solution is 1-5 mol / L.

4. The preparation method according to claim 1, characterized in that: The porous support network is selected from any one of polyphenylene sulfide, polyether ketone, and polypropylene.

5. The preparation method according to claim 1, characterized in that: The thickness of the porous support mesh is 20-150 μm.

6. The preparation method according to claim 1, characterized in that: The solid content of the casting solution is 10-33 wt %.

7. The preparation method according to claim 1, characterized in that: The method for preparing the casting solution is as follows: heating and stirring an organic high molecular polymer and an organic solvent to obtain the casting solution.

8. The preparation method according to claim 7, characterized in that: The organic high molecular polymer is selected from at least one of polyaryl-piperidine polymers, polyaryl-alkylene polymers, polybiphenyl alkyl polymers, styrene polymers, polyether polymers, polysulfone polymers, and polytetrafluoroethylene polymers.

9. The preparation method according to claim 7, characterized in that: The mass ratio of the organic high molecular polymer to the organic solvent is 1:2 to 1:

420.

10. The preparation method according to claim 7, characterized in that: The heating temperature is 50-120°C.

Citation Information

Patent Citations

  • Heterogeneous anion exchange membrane and device

    CN116272397A

  • Composite anion exchange membrane and preparation method thereof

    CN117046317A