Preparation method of aluminum-based lithium extraction adsorbent

By using hydrothermal reaction and azeotropic distillation technology of aluminum-lithium mixed solution and urea in the preparation of lithium adsorbent, the problems of uneven particle size and plate bonding in the prior art were solved, and aluminum-based lithium extract with high specific surface area and adsorption capacity were obtained. Adsorbents, suitable for large-scale production and application.

CN118949914APending Publication Date: 2024-11-15CHANGSHA DESIGN & RES INST OF CHEM IND MIN
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202410582584.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-05-11
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

In the existing lithium adsorbent preparation methods, the highly alkaline sodium hydroxide leads to fast reaction speed and uneven particle size, and the traditional drying method leads to the plate-setting of the adsorbent powder, affecting the specific surface area and adsorption capacity.

Method used

The soluble aluminum salt and lithium salt are mixed into a mixed aluminum-lithium solution, and the urea solution is stirred and hydrothermal reaction is carried out to form an aluminum-based lithium extract adsorbent gel, and is dehydrated by azeotropic distillation to obtain a uniform particle size and high specific surface area. Adsorbent.

Benefits of technology

It overcomes the problems of uneven particle size and plate bonding in traditional processes, improves the specific surface area and adsorption capacity of the adsorbent, and achieves a more efficient lithium extraction effect, which is suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118949914A_ABST
    Figure CN118949914A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of an aluminum-based lithium extraction adsorbent. The preparation method comprises the following steps: adding a dispersing agent into soluble aluminum salt and soluble lithium salt to prepare an aluminum-lithium mixed solution; uniformly mixing the aluminum-lithium mixed solution with a urea solution, and carrying out a stirring hydrothermal reaction; washing and centrifuging a gel mixture obtained by the hydrothermal reaction to obtain aluminum-based lithium extraction adsorbent gel; and dispersing the aluminum-based lithium extraction adsorbent gel into organic alcohol, carrying out azeotropic distillation, dehydrating, drying, and grinding to obtain the aluminum-based lithium extraction adsorbent. By adopting a mild and stable reaction system, the problems of strong alkalinity, high crystallization speed and large product particle size of the traditional synthesis process are solved, the particle size of the adsorbent is effectively reduced, the specific surface area is increased, and the mass transfer efficiency is improved; the adsorption capacity of the prepared aluminum-based lithium extraction adsorbent reaches 14-16 mg / g, and the aluminum-based lithium extraction adsorbent has wide popularization value; the reaction process is short, and expanded production is easy.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for preparing a lithium extraction material, and in particular to a method for preparing a lithium extraction adsorbent. Background Art

[0002] As a member of the large family of non-ferrous metals, lithium has been a hot topic in the industry in recent years. The lithium content in salt lake brine is high, the resources are abundant, and the production cost is much lower than the cost of ore extraction. It has become the main direction for domestic and foreign companies to develop and produce lithium salts. my country's salt lake brine lithium resources are mainly distributed in Qinghai Province and Tibet Autonomous Region. Among them, the reserves of salt lake brine lithium resources in Qinghai Province account for nearly 50%, and the Tibet Autonomous Region accounts for about 30%. Qinghai salt lake brine lithium resources are mainly concentrated in Chaerhan Salt Lake, Dongtaijinaier Salt Lake, Xitaijinaier Salt Lake, Yiliping Salt Lake and Dachaidan Salt Lake. Tibet's salt lake brine lithium resources are mainly concentrated in Zabuye Salt Lake, Jiezechaka Salt Lake and Longmu Co Salt Lake. The methods for extracting and separating lithium from salt lake brine mainly include precipitation method, solvent extraction method, calcination method, membrane method and adsorption method. The adsorption method has great advantages from both environmental and economic perspectives, especially the advantages of extracting lithium from low-grade lithium-containing brine or seawater. The key technology of lithium extraction by adsorption is the adsorbent, which is required to have extremely high selectivity for lithium in order to eliminate the interference of a large number of alkali metal and alkaline earth metal ions coexisting in brine. In recent years, my country's salt lake lithium extraction industry has continued to develop at a high speed, and the production line construction of lithium-containing salt lakes that are easier to extract has basically been completed. However, there are still a large number of salt lakes in my country that have not yet been developed. The chemical composition of the lithium resources in these salt lakes is complex, and the lithium ions in them are difficult to effectively separate from other elements, and there are great difficulties in resource utilization, which puts higher requirements on lithium extraction adsorbents.

[0003] CN108993376A discloses a method for preparing a lithium adsorbent, which is to fully mix an aluminum source and a lithium source, and then hydrothermally react with sodium hydroxide, and then obtain an aluminum salt lithium adsorbent after aging, washing and drying. Although the adsorbent synthesis process disclosed in CN108993376A is feasible, due to the strong alkalinity of sodium hydroxide and the fast reaction speed, the addition and mixing reactions during the reaction and crystallization process are uneven, and the local reaction is strong and the generated products are easy to agglomerate, resulting in uneven product particle size and severe wrapping; in addition, the traditional vacuum drying method will cause the adsorbent powder to compact, affecting the specific surface area of ​​the adsorbent. A combination of various factors will result in a low adsorbent capacity. Summary of the invention

[0004] The technical problem to be solved by the present invention is to overcome the above-mentioned defects of the prior art and provide a method for preparing an aluminum-based lithium extraction adsorbent with a large specific surface area and a high adsorption capacity.

[0005] The technical solution adopted by the present invention to solve the technical problem is as follows: A method for preparing an aluminum-based lithium extraction adsorbent comprises the following steps: (1) Adding a dispersant to a soluble aluminum salt and a soluble lithium salt to prepare an aluminum-lithium mixed solution; (2) the aluminum-lithium mixed solution and the urea solution are uniformly mixed and subjected to a stirring hydrothermal reaction; (3) washing and centrifuging the gel mixture obtained by the hydrothermal reaction to obtain an aluminum-based lithium extraction adsorbent gel; (4) dispersing the aluminum-based lithium extraction adsorbent gel in an organic alcohol, performing azeotropic distillation, dehydrating and drying, and then grinding to obtain an aluminum-based lithium extraction adsorbent.

[0006] The chemical formula of the obtained aluminum-based lithium extraction adsorbent can be written as: LiCl·2Al(OH)3·xH2O.

[0007] The invention adopts a mild and stable reaction system to overcome the problems of strong alkalinity, fast crystallization speed and large product particle size in the traditional synthesis process, effectively reduces the particle size of the adsorbent, increases the specific surface area and improves the mass transfer efficiency; the reaction process is short and easy to scale up production.

[0008] Preferably, in step (1), the Al / Li molar ratio in the aluminum-lithium mixed solution is 1:0.5-2.0.

[0009] By adopting the above technical solution, the product has better performance.

[0010] Preferably, in step (1), the soluble aluminum salt is one or more of aluminum chloride, aluminum sulfate, aluminum nitrate, sodium aluminate, and lithium bromide.

[0011] The adoption of the above technical solution helps to obtain a lithium extraction adsorbent with uniform particle size.

[0012] Preferably, in step (1), the soluble lithium salt is one or more of lithium chloride, lithium sulfate, lithium hydroxide and lithium nitrate.

[0013] The adoption of the above technical solution helps to obtain a lithium extraction adsorbent with uniform particle size.

[0014] Preferably, in step (1), the dispersant is one or more of sodium polyacrylate, triethylhexyl phosphate, sodium dodecyl sulfate, polyethylene glycol, fatty acid, and polyethylene glycol ester.

[0015] The adoption of the above technical solution helps to obtain a lithium extraction adsorbent with uniform particle size.

[0016] Preferably, in step (1), the amount of the dispersant used is 0.5-2% of the mass of the soluble aluminum salt.

[0017] The adoption of the above technical solution helps to obtain a lithium extraction adsorbent with uniform particle size.

[0018] Preferably, in step (1), the amount of water in the aluminum-lithium mixed solution is 1.5 to 3.0 times the sum of the mass of the soluble aluminum salt and the soluble lithium salt.

[0019] The adoption of the technical solution helps to mix the solution evenly.

[0020] Preferably, in step (2), the mass ratio of urea to water in the urea solution is 1:0.8-1.2.

[0021] The adoption of the technical solution helps to mix the solution evenly.

[0022] Preferably, in step (2), the amounts of urea solution and aluminum-lithium mixed solution used meet a urea / Al molar ratio of 6 to 15:1.

[0023] By adopting the above technical solution, the hydrothermal reaction effect is better.

[0024] Preferably, in step (2), the aluminum-lithium mixed solution and the urea solution are uniformly mixed by homogeneous dispersion and / or ultrasonic dispersion.

[0025] By adopting the above technical solution, a better mixing effect is achieved.

[0026] Preferably, in step (2), the temperature of the stirring hydrothermal reaction is 85-110°C.

[0027] By adopting the above technical solution, the hydrothermal reaction effect is better.

[0028] Preferably, in step (2), the stirring speed of the hydrothermal reaction is 400 to 800 rpm.

[0029] By adopting the above technical solution, the hydrothermal reaction effect is better.

[0030] Preferably, in step (2), the stirring time of the hydrothermal reaction is 5 to 8 hours.

[0031] By adopting the above technical solution, the hydrothermal reaction effect is better.

[0032] Preferably, in step (3), the washing temperature is 40 to 70°C.

[0033] By adopting the above technical solution, the washing effect is better.

[0034] Preferably, in step (4), the boiling point of the organic alcohol during azeotropic distillation is lower than 150°C.

[0035] By adopting the above technical solution, it is avoided that the aluminum-based lithium extraction adsorbent gel is damaged by excessively high temperature. When the selected organic alcohol has a high boiling point under normal pressure, reduced pressure distillation can be used.

[0036] Preferably, in step (4), the organic alcohol is one or more of ethanol, ethylene glycol, isopropanol, glycerol, and n-butanol.

[0037] By adopting the above technical solution, a better dehydration effect is achieved.

[0038] The temperature of the azeotropic distillation can be determined according to the boiling point of the organic alcohol used, so long as the azeotropic distillation can be achieved while the temperature is not too high.

[0039] Preferably, in step (4), the aluminum-based lithium extraction adsorbent gel is dispersed in the organic alcohol by ultrasonic dispersion.

[0040] By adopting the above technical solution, a better dispersing effect is achieved.

[0041] The present invention mainly utilizes the slow decomposition of urea to uniformly provide hydroxide, and the aluminum-lithium mixed solution and hydroxide slowly react in a mild system to generate hydroxide gel. Under uniform precipitation conditions, the "nucleation" speed of the solid product is much greater than the "growth" speed, and small-sized adsorbent particles can be obtained, and aluminum and lithium salts can achieve good uniform combination; azeotropic distillation dehydration can further solve the problem of easy agglomeration and hardening in ordinary drying, and can effectively control the particle size of the aluminum-based adsorbent precursor, ensure the looseness of the powder, and obtain lithium extraction powder with high adsorption capacity.

[0042] Beneficial effects of the present invention: (1) The present invention adopts a mild and stable reaction system to overcome the problems of strong alkalinity, fast crystallization speed and large product particle size in the traditional synthesis process, effectively reducing the particle size of the adsorbent, increasing the specific surface area and improving the mass transfer efficiency; (2) The aluminum-based lithium extraction adsorbent prepared by the present invention has an adsorption capacity of 14 to 16 mg / g, which has wide promotion value; (3) The reaction process is short and easy to scale up production. BRIEF DESCRIPTION OF THE DRAWINGS

[0043] Figure 1 This is a particle size distribution diagram of the aluminum-based lithium extraction adsorbent obtained in Example 1 of the present invention. DETAILED DESCRIPTION

[0044] The present invention is further described below in conjunction with embodiments and drawings.

[0045] The raw materials used in the embodiments of the present invention are all obtained through conventional commercial channels. Example 1

[0046] The preparation method of the aluminum-based lithium extraction adsorbent of this embodiment comprises the following steps: (1) Aluminum chloride and lithium chloride are mixed in water at an Al / Li molar ratio of 1:0.5, and polyethylene glycol is added in an amount of 1% based on the mass of the aluminum salt to obtain an aluminum-lithium mixed solution; wherein the amount of water added is 1.5 times the total mass of the aluminum salt and the lithium salt; (2) The aluminum-lithium mixed solution is mixed with a urea solution, wherein the urea / Al molar ratio is 13.5:1; the mixture is mixed in a homogenizer, and a stirring hydrothermal reaction is performed at 100° C. for 5 hours at a stirring speed of 600 rpm to obtain a gel mixture; the mass ratio of urea to water in the urea solution is 1:1; (3) The gel mixture obtained by the hydrothermal reaction was washed with deionized water at 60° C. and centrifuged three times to obtain an aluminum-based lithium extraction adsorbent gel; (4) The aluminum-based lithium-extraction adsorbent gel is ultrasonically dispersed in n-butanol, subjected to azeotropic distillation, dehydrated, dried, and then ground to obtain a high-efficiency lithium salt adsorbent.

[0047] The particle size distribution of the obtained lithium extraction adsorbent is as follows: Figure 1 As shown, it can be seen that the adsorbent D50 is around 500nm, the overall particle size is below 2μm, and the particle size distribution is uniform.

[0048] Adsorption test: 5g of high-efficiency lithium salt adsorbent was used to conduct static adsorption experiment on magnesium sulfate subtype salt lake brine containing 0.250g / L lithium. The adsorption was stopped after 1h, and the solid and liquid were separated by centrifugation. After testing and analysis, the lithium adsorption capacity was found to be 15.08mg / g. Example 2

[0049] The preparation method of the aluminum-based lithium extraction adsorbent of this embodiment comprises the following steps: (1) Aluminum chloride and lithium hydroxide are mixed in water at an Al / Li molar ratio of 1:0.5, and polyethylene glycol is added in an amount of 1.5% based on the mass of the aluminum salt to obtain an aluminum-lithium mixed solution; wherein the amount of water added is 1.5 times the total mass of the aluminum salt and the lithium salt; (2) The aluminum-lithium mixed solution is mixed with a urea solution, with a urea / Al molar ratio of 6:1; the mixture is mixed in a homogenizer, and a stirring hydrothermal reaction is performed at 110° C. for 5 hours at a stirring speed of 600 rpm to obtain a gel mixture; the mass ratio of urea to water in the urea solution is 1:1.1; (3) The gel mixture obtained by the hydrothermal reaction was washed with deionized water at 60° C. and centrifuged three times to obtain an aluminum-based lithium extraction adsorbent gel; (4) The aluminum-based lithium-extraction adsorbent gel is ultrasonically dispersed in ethanol, subjected to azeotropic distillation, dehydrated, dried, and then ground to obtain a high-efficiency lithium salt adsorbent.

[0050] Adsorption test: 5g of high-efficiency lithium salt adsorbent was used to conduct static adsorption experiment on magnesium chloride salt lake brine containing 0.261g / L lithium. The adsorption was stopped after 1h, and the solid and liquid were separated by centrifugation. After testing and analysis, the lithium adsorption capacity was found to be 14.39mg / g. Example 3

[0051] The preparation method of the aluminum-based lithium extraction adsorbent of this embodiment comprises the following steps: (1) Aluminum chloride and lithium hydroxide are mixed in water at an Al / Li molar ratio of 1:0.6, and polyethylene glycol is added in an amount of 1.5% based on the mass of the aluminum salt to obtain an aluminum-lithium mixed solution; wherein the amount of water added is 1.5 times the total mass of the aluminum salt and the lithium salt; (2) The aluminum-lithium mixed solution is mixed with a urea solution, wherein the urea / Al molar ratio is 6:1; the mixture is mixed in a homogenizer, and a stirring hydrothermal reaction is performed at 95° C. for 6 hours at a stirring speed of 500 rpm to obtain a gel mixture; the mass ratio of urea to water in the urea solution is 1:1; (3) The gel mixture obtained by the hydrothermal reaction was washed with deionized water at 50° C. and centrifuged three times to obtain an aluminum-based lithium extraction adsorbent gel; (4) The aluminum-based lithium-extraction adsorbent gel is ultrasonically dispersed in isopropanol, subjected to azeotropic distillation, dehydrated and dried, and then ground to obtain a high-efficiency lithium salt adsorbent.

[0052] Adsorption test: 5g of high-efficiency lithium salt adsorbent was used to conduct static adsorption experiment on magnesium chloride salt lake brine containing 0.261g / L lithium. The adsorption was stopped after 1h, and the solid and liquid were separated by centrifugation. After testing and analysis, the lithium adsorption capacity was found to be 14.52mg / g.

Claims

1. A method for preparing an aluminum-based lithium extraction adsorbent, characterized in that: The following steps are involved: (1) Adding a dispersant to a soluble aluminum salt and a soluble lithium salt to prepare an aluminum-lithium mixed solution; (2) the aluminum-lithium mixed solution and the urea solution are uniformly mixed and subjected to a stirring hydrothermal reaction; (3) washing and centrifuging the gel mixture obtained by the hydrothermal reaction to obtain an aluminum-based lithium extraction adsorbent gel; (4) dispersing the aluminum-based lithium extraction adsorbent gel in an organic alcohol, performing azeotropic distillation, dehydrating and drying, and then grinding to obtain an aluminum-based lithium extraction adsorbent.

2. The method for preparing an aluminum-based lithium extraction adsorbent according to claim 1, characterized in that: In step (1), the Al / Li molar ratio in the aluminum-lithium mixed solution is 1:0.5-2.

0.

3. The method for preparing an aluminum-based lithium extraction adsorbent according to claim 1 or 2, characterized in that: In step (1), the soluble aluminum salt is one or more of aluminum chloride, aluminum sulfate, aluminum nitrate, sodium aluminate, and lithium bromide; in step (1), the soluble lithium salt is one or more of lithium chloride, lithium sulfate, lithium hydroxide, and lithium nitrate; in step (1), the dispersant is one or more of sodium polyacrylate, triethylhexyl phosphoric acid, sodium dodecyl sulfate, polyethylene glycol, fatty acid, and polyethylene glycol ester.

4. The method for preparing an aluminum-based lithium extraction adsorbent according to any one of claims 1 to 3, characterized in that: In step (1), the amount of the dispersant used is 0.5 to 2% of the mass of the soluble aluminum salt; in step (1), the amount of water used in the aluminum-lithium mixed solution is 1.5 to 3.0 times the sum of the mass of the soluble aluminum salt and the soluble lithium salt.

5. The method for preparing an aluminum-based lithium extraction adsorbent according to any one of claims 1 to 4, characterized in that: In step (2), the mass ratio of urea to water in the urea solution is 1:0.8-1.2; in step (2), the amount of urea solution and aluminum-lithium mixed solution used is consistent with a urea / Al molar ratio of 6-15:

1.

6. The method for preparing an aluminum-based lithium extraction adsorbent according to any one of claims 1 to 5, characterized in that: In step (2), the aluminum-lithium mixed solution and the urea solution are evenly mixed by homogeneous dispersion and / or ultrasonic dispersion; in step (4), the aluminum-based lithium extraction adsorbent gel is dispersed in the organic alcohol by ultrasonic dispersion.

7. The method for preparing an aluminum-based lithium extraction adsorbent according to any one of claims 1 to 6, characterized in that: In step (2), the temperature of the stirring hydrothermal reaction is 85 to 110° C.; in step (2), the stirring speed of the stirring hydrothermal reaction is 400 to 800 rpm; in step (2), the time of the stirring hydrothermal reaction is 5 to 8 hours.

8. The method for preparing an aluminum-based lithium extraction adsorbent according to any one of claims 1 to 7, characterized in that: In step (3), the washing temperature is 40 to 70°C.

9. The method for preparing an aluminum-based lithium extraction adsorbent according to any one of claims 1 to 8, characterized in that: In step (4), the boiling point of the organic alcohol during azeotropic distillation is lower than 150°C.

10. The method for preparing an aluminum-based lithium extraction adsorbent according to any one of claims 1 to 9, characterized in that: In step (4), the organic alcohol is one or more of ethanol, ethylene glycol, isopropanol, glycerol, and n-butanol.

Citation Information

Patent Citations

  • Aluminum salt lithium adsorbent, and preparation method and application thereof

    CN108993376A

  • Method for synthesizing nanometer gama-Al2O3 by adopting solvent replacement / azeotropic distillation drying method and applications thereof

    CN103395809A

  • Aluminum salt adsorbent and application thereof in extraction of lithium in salt lake brine

    CN108854996A

  • Synthesis process of lithium salt adsorbent precursor

    CN114618440A

  • Preparation method of functional material for extracting lithium from aluminum salt

    CN115155510A