Aluminum salt adsorbent synthesis and granulation process
By adding aluminum source and lithium source to a specific molar ratio to water and undergoing hydrothermal reactions, combining polyethylene glycol and pore-generating agents, an efficient aluminum salt adsorption is prepared, and the aluminum salt adsorption in the prior art is solved. The poor versatility and high cost of the agent have achieved the effect of efficient lithium extraction in high magnesium lithium than in salt lakes.
Patent Information
- Application Number
- CN202410582578.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-11
- Publication Date
- 2024-11-15
AI Technical Summary
The existing aluminum salt adsorbents are used in high-magnesium lithium salts in salt lakes with poor versus salt lakes, low adsorption capacity, complex preparation process and high cost. Traditional methods use hazardous chemicals and high energy consumption.
In a stirred state, the aluminum source and lithium source are added to water in a specific molar ratio, polyethylene glycol is added and hydrothermal reaction is carried out to form an aluminum lithium salt intermediate, followed by filtering, washing, drying and grinding, and adding binder and The pore-generating agent is blended and an aluminum salt adsorbent is prepared by efficient wet mixing and granulation mechanism.
It achieves high adsorption activity, selectivity and cycle stability, reduces production costs, simplifies the process flow, is suitable for high magnesium-lithium ratio and low lithium concentration salt lake brine lithium extraction, and is easy to industrially produce.
Smart Images

Figure FT_1 
Figure FT_2
Abstract
Description
Technical Field
[0001] The invention relates to a synthesis and granulation process of an aluminum salt adsorbent. Background Art
[0002] As a member of the non-ferrous metal family, lithium has been a hot topic in the industry in recent years. Global lithium resources are relatively abundant. According to data from the United States Geological Survey, the global lithium resource reserves in 2020 are about 21 million tons of lithium metal equivalent. In modern industry, the lithium industry occupies an important position and is the foundation for the development of new energy and new materials industries. Lithium products are widely used in metal smelting, glass and ceramics, refrigeration and lubrication, high-energy batteries, aerospace, nuclear fusion power generation and other fields, and their strategic value is increasingly valued by countries around the world.
[0003] The main source of lithium resources in my country is salt lakes. At present, the lithium content in salt lake brine is high, the resources are abundant, and the production cost is generally lower than the cost of extracting lithium from ore. It has become the main direction for domestic and foreign companies to develop and produce lithium salts. Therefore, vigorously researching and developing salt lake lithium extraction technology is the main way to enhance the competitiveness of downstream lithium resource industries and get rid of the bottleneck of imported lithium resources.
[0004] Extracting lithium from salt lake brine has simple process and low cost. According to statistics, the lithium resource reserves of salt lake brine account for about 70% to 80% of the total lithium resources. The most common methods of extracting lithium from salt lakes in Qinghai, my country are adsorption and membrane methods. The adsorption method is particularly suitable for the separation of lithium from high-magnesium and low-lithium brines (magnesium-lithium ratio of 500:1 or higher), and is also suitable for brines with relatively low lithium content (lithium content is generally below 300 mg / L). The selectivity is good in this brine. The biggest advantage is that it has great advantages in terms of economy and environmental protection, and the process is simple, the recovery rate is high, and the selectivity is good. The adsorbent material is the core of lithium extraction by adsorption. The research focus is on how to prepare adsorbents with excellent performance. From the perspective of economy and environmental protection, compared with other methods, the salt lake lithium extraction process has great advantages, especially for extracting lithium from high magnesium-lithium ratio brines. Inorganic ion adsorbents have high selectivity for lithium. As inorganic ion exchange and adsorbents for selective lithium extraction, they mainly include aluminum salt adsorbents, ion sieve oxides, layered polyvalent metal acid salts, monoclinic antimonic acid and antimonate, amorphous hydroxides, etc. In the current lithium extraction industry, only aluminum salt adsorbents have mature industrial applications.
[0005] The use of aluminum salts as lithium ion adsorbents is developed from the aluminum salt precipitation method for extracting lithium. Aluminum salt adsorbents are produced by inserting LiCl into Al(OH)3 to generate the compound "LiCl·2Al(OH)3·nH2O". This compound has a defective disordered structure. Using fresh water to remove the Li in the component + The vacancy pair Li +It has adsorption activity. When smaller metal ions enter and occupy the octahedral holes of the Al(OH)3 layer, the anion holes here play an ion sieving effect. Due to the influence of steric hindrance, alkali metal and alkaline earth metal ions with larger radius are blocked outside, thus solving the difficulty of magnesium and lithium separation. However, in general, the application of adsorbent lithium extraction process in high magnesium-lithium ratio salt lakes currently has the following problems: 1) The adsorbent has poor versatility; 2) The actual adsorption capacity is much smaller than the theoretical adsorption capacity; 3) The adsorbent preparation and molding process have a great influence on the adsorption capacity; 4) There is a certain loss of adsorbent.
[0006] The traditional preparation method of aluminum adsorbents uses lithium hydroxide and aluminum chloride. However, due to the soaring cost of lithium salt products at this stage, the cost of lithium adsorbent products has also risen, and the cost of lithium salt accounts for more than 80% of the ton cost. If the lithium salt is not recycled during the preparation process, the production cost will be too high. Most of the existing aluminum adsorbent precursor synthesis technologies require the use of ultrasonic equipment or proprietary equipment with high stirring speeds. Most of the granulation uses extrusion granulation, which has a low one-time molding rate, and the preparation process is complicated and inefficient, and there is still a lot of room for improvement.
[0007] CN106975436A discloses a method for preparing a lithium adsorbent. The granulation binder used is a chlorine-containing high molecular polymer and liquid chlorine. The method uses a large amount of organic matter, reaching 28 to 50wt% of the powder, resulting in a significant decrease in the effective specific surface area of the lithium adsorbent after granulation and a low working adsorption capacity. In addition, liquid chlorine is a highly dangerous chemical. Once leaked, it will cause serious pollution to the environment.
[0008] CN106076243A discloses a microporous aluminum salt lithium adsorbent and a preparation method thereof, a filler and a method for enriching lithium ions. The method comprises the following steps: adding a lithium hydroxide solution to a soluble aluminum salt solution at a rate of 100 to 300 mL / h at a stirring speed of 500 to 800 rpm, wherein the ratio of the amount of lithium hydroxide to the soluble aluminum salt is 2:1 to 3:1.03 to form a precipitate embedded with soluble lithium, and then removing the soluble lithium to obtain a microporous aluminum salt lithium adsorbent. The method requires a large amount of lithium hydroxide to be added, and special stirring equipment is required to maintain a high stirring speed. The method also has a slow feeding speed, low production capacity, high production cost, and a low saturated adsorption capacity of the obtained aluminum salt lithium adsorbent.
[0009] CN109266851A, CN106390960B, etc. respectively disclose a method for preparing a magnetic lithium adsorbent, both of which are to obtain a magnetic adsorbent material by directly or indirectly combining a magnetic core with a powder adsorbent. The preparation method is simple, does not require granulation, and can quickly achieve solid-liquid separation of the adsorbent and the adsorbate, but does not have any substantial process improvement for the synthesis of the powder material precursor. At the same time, the magnetic adsorbent is difficult to recover during the adsorption process, making it difficult to achieve industrial production.
[0010] CN109759006A discloses a method for preparing a lithium adsorbent, which comprises grinding a slurry containing Al(OH)3 and LiCl, and spray drying the slurry after ultrasonic microwave heating to obtain the lithium adsorbent. However, the method has the disadvantages of strict requirements on equipment and operating conditions, high energy consumption, and high production cost. Summary of the invention
[0011] The purpose of the present invention is to overcome the defects of the prior art and provide a synthesis and granulation process of an aluminum salt adsorbent. The obtained adsorbent exhibits high adsorption activity, selectivity and good cycle stability for lithium ions, and the synthesis and granulation process is relatively simple, low in cost, stable in structure, low in dissolution rate, and easy to realize large-scale industrial production.
[0012] The adsorbent is particularly suitable for lithium extraction from brine with a high magnesium-to-lithium ratio, high sulfate type, and salt lake brine with a low lithium concentration.
[0013] In order to achieve the above invention objectives, the specific technical solutions adopted are:
[0014] A process for synthesizing and granulating an aluminum salt adsorbent comprises the following steps:
[0015] Step (1), preparation of aluminum salt adsorbent precursor:
[0016] a) under stirring (preferably at room temperature), an aluminum source and a lithium source are sequentially added into water to dissolve, the aluminum source and the lithium source are measured according to an Al / Li molar ratio of 2.5 to 4.5:1, to obtain an aluminum-lithium salt mixed aqueous solution, while maintaining stirring, adding polyethylene glycol (PEG) equivalent to 0.2 wt% to 0.5 wt% of the mass of the aluminum-lithium salt mixed aqueous solution, and stirring evenly to obtain an aluminum-lithium salt intermediate.
[0017] The amount of water added is 1.1 to 2.3 times the total mass of the aluminum source and the lithium source, and preferably the amount of water added is 1.3 to 1.5 times the total mass of the aluminum source and the lithium source. The Al / Li molar ratio is preferably 3.0 to 3.5:1. The aluminum source is a soluble inorganic aluminum salt, and the aluminum source is preferably at least one of aluminum chloride, aluminum sulfate, and aluminum nitrate. The lithium source is a soluble inorganic lithium salt, and the lithium source is preferably at least one of lithium chloride, lithium sulfate, and lithium nitrate.
[0018] b) preparing an alkali solution, wherein the molar ratio of the hydroxide contained in the alkali solution to the aluminum element contained in the aluminum source in step (a) is 1.2-2.5:1, placing the alkali solution in a reactor, adding the aluminum lithium salt intermediate prepared in step (a) to carry out a hydrothermal reaction, wherein the aluminum lithium salt intermediate addition time is 1.0-3.0h; the hydrothermal reaction temperature is 70°C-95°C, and after the addition is completed, the stirring is continued for 1.0-3.0h, and the end point pH is controlled to be 6.5-8.5 after the reaction is completed. After the hydrothermal reaction is completed, a wet material slurry of an aluminum salt adsorbent precursor is obtained.
[0019] The alkali solution is a readily soluble inorganic alkali, preferably at least one of a sodium hydroxide solution and a potassium hydroxide solution, and preferably has a mass concentration of 20 wt% to 35 wt%.
[0020] c) filtering, washing, drying and grinding the aluminum salt adsorbent precursor wet material slurry obtained in step (b) to obtain an aluminum salt adsorbent precursor product. The washing is preferably performed with water, more preferably with three-stage countercurrent washing, the amount of washing water is 1 to 3 times the mass of the aluminum salt adsorbent precursor wet material slurry, and the washing time is 0.5 to 3.0 hours. The drying temperature is 70 to 95° C., and the water content of the aluminum salt adsorbent precursor product is ≤1wt%.
[0021] Step (2), doping and blending:
[0022] The binder, porogen and organic solvent are mixed uniformly at a mass ratio of 0.1 to 0.6:0.1 to 0.5:1 at a temperature of 50°C to 100°C to obtain a blend slurry; the aluminum salt adsorbent precursor product obtained in step (1) and the binder are measured at a mass ratio of 4.0 to 9.0:1, added to the blend slurry, and continued to stir and mix to obtain a viscous doped blend.
[0023] Step (3), granulation and molding:
[0024] The viscous mixed blend obtained in step (2) is mixed and chopped into a single piece by a high-efficiency wet mixing granulator, and then dried and sieved to obtain a finished aluminum salt adsorbent.
[0025] Further, in the present application, the aluminum source is calculated based on the moles of aluminum atoms, for example, 1 mole of aluminum nitrate or aluminum chloride is used as 1 mole of aluminum source, and 1 mole of aluminum sulfate is used as 2 moles of aluminum source. The alkali solution is calculated based on the moles of hydroxide, and the lithium source is calculated based on the moles of lithium ions.
[0026] Furthermore, in step (a), the polyethylene glycol is at least one of PEG-200, PEG-400, PEG-600, PEG-800, PEG-1000, PEG-1500, PEG-2000, PEG-3000, PEG-4000, and PEG-6000. PEG can easily form strong hydrogen bonds with the surface of aluminum salt adsorbent precursor precipitation particles in aqueous solution, and its ether bonds can also easily produce affinity with the surface of aluminum salt adsorbent precursor precipitation particles, thereby forming a layer of polymer film, and the serpentine molecular bonds give the protective film a steric hindrance effect, which greatly weakens the attraction between particles, thereby effectively preventing particle growth and inhibiting the agglomeration of aluminum salt adsorbent precursor particles. In addition, the agglomerates are subsequently opened by grinding, and these aluminum salt adsorbent precursor primary particles or smaller agglomerates cannot be re-agglomerated into large agglomerates. With the increase in the specific surface area of the particles, the grains have a mechanical isolation effect, reducing the average particle size of the particles. The agglomeration energy of the aluminum salt adsorbent precursor powder obtained in this way can be minimized, laying a foundation for the preparation of aluminum salt adsorbent precursors with high adsorption performance, while overcoming the limitations of traditional dispersion processes on special equipment such as ultrasound or homogeneous dispersion.
[0027] Furthermore, the order of adding materials for the hydrothermal reaction in step (b) is that the aluminum lithium salt intermediate is added to the alkaline solution, the adding time is 1.0 to 3.0 hours, the pH of the reaction is controlled to be 6.5 to 8.5, the aluminum salt adsorbent precursor wet material is LiCl·1.8 to 3.5Al(OH)3·1.0 to 3.9H2O generated by the hydrothermal reaction, and the aluminum salt adsorbent precursor is a microporous material, preferably LiCl·2.0 to 2.3Al(OH)3·1.5 to 2.OH2O; the inventors have found through a large number of experimental studies that the use of this reaction condition can ensure that the material can be evenly dispersed in the alkaline system, affecting the hydrothermal reaction and avoiding the agglomeration of the aluminum salt adsorbent precursor. At the above set temperature, it can not only ensure the uniform dispersion of various particles in the solution, but also avoid the uncontrollable reaction due to the early progress of the hydrothermal reaction. If the temperature is too low, the reaction will not proceed normally; if the temperature is too high, the molecules in the solution will increase their kinetic energy due to the heat, which is not conducive to the formation of stable crystal nuclei. As the number of grains increases, the probability of collision between grains increases, which will cause grain stacking.
[0028] Furthermore, in step (c), the obtained aluminum salt adsorbent precursor wet material slurry is filtered, washed, dried, and ground to obtain a microporous aluminum salt adsorbent precursor product. The washing adopts three-stage countercurrent washing, and the filter cake after the aluminum salt adsorbent precursor wet material slurry is filtered and dried after three-stage countercurrent re-slurry washing. In the three-stage countercurrent re-slurry washing, the first-stage washing uses the separation mother liquor of the previous second-stage washing to prepare the slurry, the second-stage washing uses the separation mother liquor of the previous third-stage washing to prepare the slurry, and the third-stage washing uses a certain amount of fresh water to prepare the slurry. The filter cake is dried and dehydrated to obtain a microporous aluminum salt adsorbent precursor product, that is, the aluminum salt adsorbent precursor product of the present invention. The amount of washing water is 1 to 3 times the mass of the precursor wet material, and the washing time is 0.5 to 3.0 hours. The filtrate and washing water obtained by filtering the aluminum salt adsorbent precursor wet material slurry can be concentrated and removed and returned as a lithium salt aqueous solution. The drying temperature of the microporous aluminum salt adsorbent precursor wet material is 70-95° C., and the water content of the microporous aluminum salt adsorbent precursor product is ≤1wt%.
[0029] Furthermore, the organic solvent in step (2) is at least one of dimethylformamide (DMF), dimethyl sulfoxide (DMSO), ethylene carbonate (EC), sodium thiocyanate (CNNaS), dimethylacetamide (DMAc), N-methylpyrrolidone (NMP), and tetrahydrofuran (THF).
[0030] Furthermore, the binder in step (2) is at least one of ABS resin, polyacrylonitrile (PAN), polyvinyl alcohol (PVA), polyethyleneimine (PEI), polyacrylic acid (PAA), carboxymethyl cellulose (CMC), ethyl cellulose (EC), polyvinyl chloride (PVC), polyvinylidene fluoride (PVDF), phenolic resin (PF), epoxy resin (EP), and polyurethane (PU). The binder is based on the orientation of the assembly structure of heterogeneous nanomaterials, and the controlled arrangement orientation of the microstructure is used to achieve fiber improvement with excellent mechanical properties. This strategy of controlling the arrangement orientation is applied to the preparation of high-strength aluminum salt adsorbent particles, which can form hydrogen bonds on the surface of the material, giving the active particles and the current collector a strong binding force.
[0031] Furthermore, the porogen in step (2) is at least one of microcrystalline cellulose, polyvinyl pyrrolidone (PVP), polyethylene glycol (PEG), and a water-soluble surfactant. The water-soluble surfactant is at least one of sodium chloride (NaCl), potassium chloride (KCl), sodium carbonate (Na2CO3), potassium nitrate (KNO3), sodium sulfate (Na2SO4), etc. When the aluminum salt adsorbent precursor product is suspended and polymerized with an organic solvent, the porogen exists in the monomer droplets in the form of small droplets, and rapidly diffuses into pores by utilizing the solubility and hydrophilicity between the liquids. After polymerization, the polymer can be evaporated at high temperature to remove the porogen.
[0032] Furthermore, the high-efficiency wet mixing granulator in step (3) combines mixing and granulation in one. Its greatest advantage is that it has a fast granulation speed and can make the viscous mixed blend in step (2) into a soft material and shred it into granules at one time without filtering and solvent granulation.
[0033] Furthermore, the drying temperature in step (3) is 60 to 120° C., more preferably 80 to 110° C., and the particle size diameter of the sieved finished product is 0.1 to 2.5 mm, more preferably 0.5 to 1.2 mm.
[0034] The aluminum salt adsorbent of the present invention is particularly suitable for lithium extraction from brine with a high magnesium-to-lithium ratio, high sulfate type brine and low lithium concentration salt lake brine, and exhibits high adsorption activity, selectivity and good cycle stability for lithium ions and other impurity ions, and has simple synthesis and granulation processes, low cost, stable structure, low dissolution rate, and easy large-scale industrial production.
[0035] Compared with the prior art, the present invention has the following beneficial effects:
[0036] (1) By adding polyethylene glycol (PEG), the aluminum salt adsorbent precursor grains are mechanically isolated and the average particle size is reduced. In this way, the agglomeration of the aluminum salt adsorbent precursor powder obtained is minimized, while overcoming the limitation of the traditional dispersion process on special equipment such as ultrasound or homogeneous dispersion.
[0037] (2) The multi-stage countercurrent washing process of the wet material of the aluminum salt adsorbent precursor can, on the one hand, elute the soluble inorganic components in the precursor, and on the other hand, it is all made of water. At the same time, the filtrate and washing water can be concentrated and removed and returned as a lithium salt aqueous solution, which greatly reduces the production cost of the aluminum salt adsorbent.
[0038] (3) The porogen optimizes the specific surface area and pore structure of the aluminum salt adsorbent, so that the final product can provide more active sites, with a lithium adsorption capacity of 2.5-5.5 g / L, high mass transfer efficiency, and a high lithium ion elution rate. The doped binder improves the product's pressure resistance and impact resistance, and the structure is stable, with an annual loss rate of less than 2wt%.
[0039] (4) The aluminum salt adsorbent precursor synthesis and granulation process can be carried out with the help of existing conventional equipment. The preparation process is simple, the reaction, aging and granulation time are short and efficient, and the one-time molding rate of the high-efficiency wet mixing granulator product is more than 80%. It has low requirements on equipment and pipeline materials, is environmentally friendly, has low production costs, and is more suitable for large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] Figure 1 and Figure 2 This is an optical photograph of the aluminum salt adsorbent granulation product obtained in Example 1 of the present invention. DETAILED DESCRIPTION
[0041] The present invention is further described below in conjunction with specific implementation modes.
[0042] Example 1
[0043] The aluminum salt adsorbent synthesis and granulation process of this embodiment includes the following steps:
[0044] Step (1) Preparation of aluminum salt adsorbent precursor:
[0045] a) under stirring at room temperature, aluminum chloride hexahydrate and lithium chloride are sequentially added into water to dissolve, the amount of water added being equivalent to 1.38 times the total mass of the aluminum source and the lithium source, and the aluminum chloride hexahydrate and lithium chloride are in an Al / Li molar ratio of 3.18:1 to obtain an aluminum lithium salt mixed aqueous solution, while maintaining stirring, adding polyethylene glycol (PEG-200) equivalent to 0.2wt% of the mass of the aluminum lithium salt mixed aqueous solution, and stirring evenly to obtain an aluminum lithium salt intermediate.
[0046] b) preparing an alkaline sodium hydroxide solution, wherein the molar ratio of the hydroxide contained in the alkaline solution to the aluminum element contained in the aluminum source in step (a) is 1.89:1, and the mass concentration of the sodium hydroxide solution is 25wt%. The alkaline solution is placed in a reactor, and the aluminum lithium salt intermediate prepared in step (a) is added to carry out a hydrothermal reaction. The hydrothermal reaction temperature is 85° C., and the aluminum lithium salt intermediate is added for 2.0 h. After the addition is completed, the stirring is continued at the temperature for 3.0 h. After the reaction is completed, the end point pH is controlled to be 7.0. After the hydrothermal reaction is completed, a wet slurry of an aluminum salt adsorbent precursor is obtained.
[0047] c) filtering, washing with water, drying and grinding the aluminum salt adsorbent precursor wet material slurry obtained in step (b) to obtain an aluminum salt adsorbent precursor product. The washing is performed with water, three-stage countercurrent washing is performed, the amount of washing water is three times the mass of the aluminum salt adsorbent precursor wet material slurry, and the washing time is 3.0 hours. The drying temperature is 80° C., and the water content of the aluminum salt adsorbent precursor product is 0.26wt%.
[0048] Step (2) doping and blending:
[0049] ABS resin, PVP and DMF are mechanically stirred at a mass ratio of 0.42:0.1:1 at 60°C to obtain a blend slurry, and the aluminum salt adsorbent precursor product obtained in step (1) and ABS are measured at a mass ratio of 7.5:1, added to the blend slurry, and continued to stir and mix to obtain a viscous doped blend.
[0050] Step (3) granulation and molding:
[0051] The viscous mixed blend obtained in step (2) is mixed and chopped into a single piece by a high-efficiency wet mixing granulator, and then dried and sieved at 80° C. to obtain a finished aluminum salt adsorbent with a particle size of 0.3 to 1.2 mm.
[0052] Figure 1 and Figure 2 This is an optical photograph of the aluminum salt adsorbent granulation product obtained in Example 1 of the present invention.
[0053] Example 2
[0054] The aluminum salt adsorbent synthesis and granulation process of this embodiment includes the following steps:
[0055] Step (1) Preparation of aluminum salt adsorbent precursor:
[0056] a) under stirring at room temperature, aluminum sulfate as an aluminum source and lithium chloride as a lithium source are sequentially added into water to dissolve, wherein the amount of water added is equivalent to 2.0 times the total mass of the aluminum source and the lithium source, and the aluminum sulfate and the lithium chloride are in an Al / Li molar ratio of 3.5:1 to obtain an aluminum-lithium salt mixed aqueous solution, and the stirring is maintained, and polyethylene glycol (PEG-400) equivalent to 0.40 wt% of the mass of the aluminum-lithium salt mixed aqueous solution is added, and the stirring is uniformly performed to obtain an aluminum-lithium salt intermediate.
[0057] b) preparing an alkaline potassium hydroxide solution, wherein the molar ratio of the hydroxide contained in the alkaline solution to the aluminum element contained in the aluminum source in step (a) is 2.0:1, and the mass concentration of potassium hydroxide is 25wt%. The alkaline solution is placed in a reactor, and the aluminum lithium salt intermediate prepared in step (a) is added to carry out a hydrothermal reaction. The hydrothermal reaction temperature is 90° C., and the aluminum lithium salt intermediate is added for 2.0 h. After the addition is completed, the stirring is continued at the temperature for 2.0 h. After the reaction is completed, the end point pH is controlled to be 7.5. After the hydrothermal reaction is completed, a wet slurry of an aluminum salt adsorbent precursor is obtained.
[0058] c) filtering, washing with water, drying and grinding the aluminum salt adsorbent precursor wet material slurry obtained in step (b) to obtain an aluminum salt adsorbent precursor product. The washing adopts three-stage countercurrent washing, the washing water volume is twice the mass of the aluminum salt adsorbent precursor wet material slurry, and the washing time is 1.0h. The drying temperature is 90°C, and the water content of the aluminum salt adsorbent precursor product is 0.34wt%.
[0059] Step (2) doping and blending:
[0060] PAN, PEG and DMF are mechanically stirred at a mass ratio of 0.35:0.2:1 at 80°C to obtain a blend slurry. The aluminum salt adsorbent precursor product obtained in step 1 and PAN are measured at a mass ratio of 8.0:1, added to the blend slurry, and continued to stir and mix to obtain a viscous doped blend.
[0061] Step (3) granulation and molding:
[0062] The doped blend is mixed and chopped into a one-step molding by a high-efficiency wet mixing granulator, and then dried and sieved at 110° C. to obtain a finished aluminum salt adsorbent with a particle size of 0.6 to 1.5 mm.
[0063] Example 3
[0064] The aluminum salt adsorbent synthesis and granulation process of this embodiment includes the following steps:
[0065] Step (1) Preparation of aluminum salt adsorbent precursor:
[0066] a) under stirring at room temperature, aluminum sulfate as an aluminum source and lithium sulfate as a lithium source are sequentially added into water to dissolve, the amount of water added being equivalent to 1.3 times the total mass of the aluminum source and the lithium salt, and the aluminum sulfate and the lithium sulfate being measured according to an Al / Li molar ratio of 2.8:1 to obtain an aluminum-lithium salt mixed aqueous solution, while maintaining stirring, adding polyethylene glycol (PEG-4000) equivalent to 0.20 wt % of the mass of the aluminum-lithium salt mixed aqueous solution and stirring uniformly to obtain an aluminum-lithium salt intermediate.
[0067] b) preparing an alkaline sodium hydroxide solution, wherein the molar ratio of the hydroxide contained in the alkaline solution to the aluminum element contained in the aluminum source in step (a) is 2.0:1, and the mass concentration of sodium hydroxide is 35wt%. The alkaline solution is placed in a reactor, and the aluminum lithium salt intermediate prepared in step (a) is added to carry out a hydrothermal reaction. The hydrothermal reaction temperature is 80° C., and the aluminum lithium salt intermediate is added for 1.5 h. After the addition is completed, the stirring is continued at the temperature for 1.5 h. After the reaction is completed, the end point pH is controlled to be 6.5. After the hydrothermal reaction is completed, a wet slurry of an aluminum salt adsorbent precursor is obtained.
[0068] c) filtering, washing with water, drying and grinding the aluminum salt adsorbent precursor wet material slurry obtained in step (b) to obtain an aluminum salt adsorbent precursor product. The washing adopts three-stage countercurrent washing, the washing water volume is 1 times the mass of the aluminum salt adsorbent precursor wet material slurry, and the washing time is 3.0 hours. The drying temperature is 70° C., and the water content of the aluminum salt adsorbent precursor product is 0.41wt%.
[0069] Step (2) doping and blending:
[0070] PVC, NaCl and THF are mechanically stirred at a mass ratio of 0.58:0.3:1 at 95°C to obtain a blend slurry, and the aluminum salt adsorbent precursor product obtained in step 1 and PVC are measured at a mass ratio of 6.0:1, added to the blend slurry, and continued to stir and mix to obtain a viscous doped blend.
[0071] Step (3) granulation and molding:
[0072] The viscous mixed blend obtained in step (2) is mixed and chopped into a single-piece shape by a high-efficiency wet mixing granulator, and then dried and sieved at 80° C. to obtain a finished aluminum salt adsorbent with a particle size of 0.6 to 1.2 mm.
[0073] Example 4
[0074] The aluminum salt adsorbent synthesis and granulation process of this embodiment includes the following steps:
[0075] Step (1) Preparation of aluminum salt adsorbent precursor:
[0076] a) under stirring at room temperature, aluminum chloride hexahydrate as an aluminum source and lithium sulfate as a lithium source are sequentially added into water for dissolution, wherein the amount of water added is equivalent to 1.8 times the total mass of the aluminum source and the lithium source, and the aluminum chloride hexahydrate and the lithium sulfate are measured according to an Al / ㈠ molar ratio of 3.0:1 to obtain an aluminum lithium salt mixed aqueous solution, and the mixture is stirred continuously, and polyethylene glycol (PEG-600) equivalent to 0.30wt% of the mass of the aluminum lithium salt mixed aqueous solution is added and stirred uniformly to obtain an aluminum lithium salt intermediate.
[0077] b) preparing an alkaline solution and a potassium hydroxide solution, wherein the molar ratio of the hydroxide contained in the alkaline solution to the aluminum element contained in the aluminum source in step (a) is 1.9:1, and the mass concentration of the potassium hydroxide solution is 35wt%. The alkaline solution is placed in a reactor, and the aluminum lithium salt intermediate prepared in step (a) is added to carry out a hydrothermal reaction. The hydrothermal reaction temperature is 95° C., and the aluminum lithium salt intermediate is added for 1.5 h. After the addition is completed, the stirring is continued at the temperature for 3.0 h. After the reaction is completed, the end point pH is controlled to be 8.0. After the hydrothermal reaction is completed, a wet slurry of an aluminum salt adsorbent precursor is obtained.
[0078] c) filtering, washing, drying and grinding the aluminum salt adsorbent precursor wet material slurry obtained in step (b) to obtain an aluminum salt adsorbent precursor product. The washing is performed with water, a three-stage countercurrent washing is performed, the amount of washing water is twice the mass of the aluminum salt adsorbent precursor wet material slurry, and the washing time is 2.0 hours. The drying temperature is 80° C., and the water content of the aluminum salt adsorbent precursor product is 0.32wt%.
[0079] Step (2) doping and blending:
[0080] PVA, KCl and NMP are mechanically stirred at a mass ratio of 0.50:0.25:1 at 80°C to obtain a blend slurry. The aluminum salt adsorbent precursor product obtained in step 1 and PVA are measured at a mass ratio of 8.0:1, added to the blend slurry, and continued to stir and mix to obtain a viscous doped blend.
[0081] Step (3) granulation and molding:
[0082] The viscous doped blend obtained in step (2) is mixed and chopped into a single-piece shape by a high-efficiency wet mixing granulator, and then dried and sieved at 110° C. to obtain a finished aluminum salt adsorbent with a particle size of 0.6 to 1.2 mm.
[0083] Comparative Example 1
[0084] The synthesis and granulation process of the aluminum salt adsorbent in this comparative example is similar to that in Example 4, and includes the following steps:
[0085] Step (1) Preparation of aluminum salt adsorbent precursor:
[0086] a) under stirring at room temperature, aluminum chloride hexahydrate as an aluminum source and lithium sulfate as a lithium source are sequentially added into water to dissolve, the amount of water added being equivalent to 1.8 times the total mass of the aluminum source and the lithium source, and the aluminum chloride hexahydrate and the lithium sulfate being measured according to an Al / Li molar ratio of 3.0:1 to obtain an aluminum lithium salt mixed aqueous solution, and stirring is maintained without adding polyethylene glycol to obtain an aluminum lithium salt intermediate.
[0087] b) preparing an alkaline solution and a potassium hydroxide solution, wherein the molar ratio of the hydroxide contained in the alkaline solution to the aluminum element contained in the aluminum source in step (a) is 2.1:1, and the mass concentration of the potassium hydroxide solution is 35wt%. The alkaline solution is placed in a reactor, and the aluminum lithium salt intermediate prepared in step (a) is added to carry out a hydrothermal reaction. The hydrothermal reaction temperature is 95° C., and the aluminum lithium salt intermediate is added for 1.5 h. After the addition is completed, the stirring is continued at the temperature for 3.0 h. After the reaction is completed, the end point pH is controlled to be 9.5. After the hydrothermal reaction is completed, a wet slurry of an aluminum salt adsorbent precursor is obtained.
[0088] c) filtering, washing, drying and grinding the aluminum salt adsorbent precursor wet material slurry obtained in step (b) to obtain an aluminum salt adsorbent precursor product. The washing is performed with water, a three-stage countercurrent washing is performed, the amount of washing water is twice the mass of the aluminum salt adsorbent precursor wet material slurry, and the washing time is 2.0 hours. The drying temperature is 80° C., and the water content of the aluminum salt adsorbent precursor product is 0.32wt%.
[0089] Step (2) doping and blending:
[0090] PVA and NMP are mechanically stirred at a mass ratio of 0.50:1 at 80°C to obtain a blend slurry without adding a porogen. The aluminum salt adsorbent precursor product obtained in step 1 and PVA are measured at a mass ratio of 8.0:1, added to the blend slurry, and continued to stir and mix to obtain a viscous doped blend.
[0091] Step (3) granulation and molding:
[0092] The viscous mixed blend obtained in step (2) is mixed and chopped into a single-piece shape by an extrusion granulator, and then dried and sieved at 110° C. to obtain a finished aluminum salt adsorbent with a particle size of 0.4 to 1.5 mm.
[0093] The products obtained in the above embodiments were subjected to performance testing.
[0094] The aluminum salt adsorbent obtained in each embodiment was used for adsorption test on lithium-containing old brine in Lop Nur sulfate salt lake in Xinjiang, my country, wherein Li + The content is 261mg / L. + The concentration was determined using an ion chromatograph (THERMO Aquion).
[0095] Adsorption experiment: static adsorption test was adopted, 500ml of brine was measured and added to a polytetrafluoroethylene beaker, 20g of the aluminum salt adsorbent obtained in the example was taken, and the adsorption and desorption test was carried out with stirring at a speed of 150r / min, the adsorption time was 4h, and the supernatant was taken after adsorption equilibrium, the desorption conditions were 300ml of fresh water desorption, desorption temperature was 25℃, and the desorption time was 3h. Each group of adsorption and desorption tests was carried out in parallel for 20 groups, and the average value was taken as the average adsorption capacity of the aluminum salt adsorbent. The results are shown in Table 1.
[0096] Table 1
[0097] Example Granulation one-step forming rate (%) Average adsorption capacity (g / L) Average lithium desorption rate (%) Breakage rate (%) / 20 times 1 85.3 4.57 94.37 0.14 2 90.7 4.98 97.69 0.21 3 92.4 4.25 98.14 0.17 4 83.6 5.06 96.32 0.11 Comparative Example 1 78.9 2.43 90.36 0.27
[0098] In this specification, unless otherwise specified, all percentages are by mass.
[0099] In Table 1, the average adsorption capacity is the content of lithium ions adsorbed per liter of adsorbent. The breakage rate is the percentage of adsorbent particles that are broken or broken during multiple uses. During use, if the adsorbent particles cannot maintain their integrity and break or break, it will cause difficulties in use. The main manifestations are: broken resin is discharged during backwashing, and fine particles leak through the flow part into the subsequent equipment, resulting in a decrease in resin layer height, a decrease in exchange capacity, an increase in water flow resistance, contamination of resin in subsequent equipment, a decrease in system effluent water quality, and contamination of water vapor quality when entering the high-temperature system.
[0100] From the results in Table 1, it can be seen that in Comparative Example 1, no polyethylene glycol was added to obtain the aluminum lithium salt intermediate, and no porogen was added for doping and blending. The performance of the obtained aluminum salt adsorbent product is not as good as that of the embodiments.
Claims
1. A process for synthesizing and granulating an aluminum salt adsorbent, It is characterized in that The following steps are involved: Step (1), preparation of aluminum salt adsorbent precursor: a) adding an aluminum source and a lithium source to water in sequence and dissolving them under stirring to obtain an aluminum-lithium salt mixed aqueous solution, adding polyethylene glycol while stirring, and stirring to obtain an aluminum-lithium salt intermediate; b) preparing an alkali solution, placing the alkali solution into a reaction kettle, adding the aluminum lithium salt intermediate prepared in step (a) to carry out a hydrothermal reaction, and continuing to keep warm and stir after the addition is completed, and obtaining a wet material slurry of an aluminum salt adsorbent precursor after the hydrothermal reaction is completed; c) filtering, washing, drying and grinding the aluminum salt adsorbent precursor wet material slurry obtained in step (b) to obtain an aluminum salt adsorbent precursor product; Step (2), doping and blending: The binder, porogen and organic solvent are stirred evenly to obtain a blend slurry; the aluminum salt adsorbent precursor product obtained in step (1) and the binder are added to the blend slurry, and the mixture is stirred and mixed to obtain a viscous doped blend; Step (3), granulation and molding: The viscous doped blend obtained in step (2) is mixed and chopped into a single piece by a high-efficiency wet mixing granulator, and then dried and sieved to obtain a finished aluminum salt adsorbent.
2. The aluminum salt adsorbent synthesis and granulation process according to claim 1, It is characterized in that Step (1), preparation of aluminum salt adsorbent precursor: a) under stirring, sequentially adding an aluminum source and a lithium source into water to dissolve, wherein the aluminum source and the lithium source are measured according to an Al / Li molar ratio of 2.5 to 4.5:1 to obtain an aluminum-lithium salt mixed aqueous solution, and stirring is continued, and polyethylene glycol equivalent to 0.2 wt% to 0.5 wt% of the mass of the aluminum-lithium salt mixed aqueous solution is added, and stirring is performed uniformly to obtain an aluminum-lithium salt intermediate; b) preparing an alkali solution, wherein the molar ratio of the hydroxide contained in the alkali solution to the aluminum element contained in the aluminum source in step (a) is 1.2 to 2.5:1, placing the alkali solution in a reactor, and adding the aluminum lithium salt intermediate prepared in step (a) to carry out a hydrothermal reaction, wherein the aluminum lithium salt intermediate addition time is 1.0 to 3.0 hours; the hydrothermal reaction temperature is 70° C. to 95° C., and after the addition is completed, the stirring is continued at the temperature for 1.0 to 3.0 hours, and the end point pH is controlled to be 6.5 to 8.5 after the reaction is completed. After the hydrothermal reaction is completed, a wet material slurry of an aluminum salt adsorbent precursor is obtained; c) filtering, washing, drying and grinding the aluminum salt adsorbent precursor wet material slurry obtained in step (b) to obtain an aluminum salt adsorbent precursor product; Step (2), doping and blending: The binder, porogen and organic solvent are mixed uniformly at a mass ratio of 0.1 to 0.6:0.1 to 0.5:1 at a temperature of 50°C to 100°C to obtain a blend slurry; the aluminum salt adsorbent precursor product obtained in step (1) and the binder are measured at a mass ratio of 4.0 to 9.0:1, added to the blend slurry, and stirred and mixed to obtain a viscous doped blend; Step (3), granulation and molding: The viscous doped blend obtained in step (2) is mixed and chopped into a single piece by a high-efficiency wet mixing granulator, and then dried and sieved to obtain a finished aluminum salt adsorbent.
3. The synthesis and granulation process of the aluminum salt adsorbent according to claim 1 or 2, It is characterized in that In step (a), stirring is performed at room temperature; and / or The amount of water added is 1.1 to 2.3 times the total mass of the aluminum source and the lithium source; and / or Al / Li molar ratio is 3.0 to 3.5:1; and / or The aluminum source is at least one of aluminum chloride, aluminum sulfate, and aluminum nitrate; and / or The lithium source is at least one of lithium chloride, lithium sulfate and lithium nitrate.
4. The aluminum salt adsorbent synthesis and granulation process according to claim 3, It is characterized in that In step (a), the amount of water added is 1.3 to 1.5 times the total mass of the aluminum source and the lithium source.
5. The synthesis and granulation process of the aluminum salt adsorbent according to claim 1 or 2, It is characterized in that In step (a), the polyethylene glycol is at least one of PEG-200, PEG-400, PEG-600, PEG-800, PEG-1000, PEG-1500, PEG-2000, PEG-3000, PEG-4000, and PEG-6000; The order of adding materials for the hydrothermal reaction in step (b) is that the aluminum lithium salt intermediate is added to the alkali solution, the adding time is 1.0 to 3.0 hours, and the pH value after the reaction is controlled to be 6.5 to 8.5; In step (b), the alkali solution is at least one of a sodium hydroxide solution and a potassium hydroxide solution, and the mass concentration is 20wt% to 35wt%.
6. The aluminum salt adsorbent synthesis and granulation process according to claim 1 or 2, It is characterized in that In step (c), the washing is carried out with water, the amount of washing water is 1 to 3 times the mass of the wet slurry of the aluminum salt adsorbent precursor, and the washing time is 0.5 to 3.0 hours; the drying temperature is 70 to 95° C., and the water content of the aluminum salt adsorbent precursor product is ≤1wt%.
7. The synthesis and granulation process of the aluminum salt adsorbent according to claim 6, It is characterized in that In step (c), the washing adopts three-stage countercurrent washing, and the filter cake after filtering the aluminum salt adsorbent precursor wet material slurry is dried after three-stage countercurrent re-slurry washing. In the three-stage countercurrent re-slurry washing, the first-stage washing uses the separated mother liquor of the previous second-stage washing to make the slurry, the second-stage washing uses the separated mother liquor of the previous third-stage washing to make the slurry, and the third-stage washing uses a certain amount of fresh water to make the slurry. The filter cake is dried and dehydrated to obtain a microporous aluminum salt adsorbent precursor product, that is, the aluminum salt adsorbent precursor product of the present invention.
8. The aluminum salt adsorbent synthesis and granulation process according to claim 1 or 2, It is characterized in that The organic solvent in step (2) is at least one of dimethylformamide, dimethyl sulfoxide, ethylene carbonate, sodium thiocyanate, dimethylacetamide, N-methylpyrrolidone and tetrahydrofuran; The binder in step (2) is at least one of ABS resin, polyacrylonitrile, polyvinyl alcohol, polyethyleneimine, polyacrylic acid, carboxymethyl cellulose, ethyl cellulose, polyvinyl chloride, polyvinylidene fluoride, phenolic resin, epoxy resin, and polyurethane; The porogen in step (2) is at least one of microcrystalline cellulose, polyvinyl pyrrolidone, polyethylene glycol, and a water-soluble surfactant.
9. The synthesis and granulation process of the aluminum salt adsorbent according to claim 8, It is characterized in that In step (2), the water-soluble surfactant is at least one of sodium chloride, potassium chloride, sodium carbonate, potassium nitrate and sodium sulfate.
10. The aluminum salt adsorbent synthesis and granulation process according to claim 1 or 2, It is characterized in that The drying temperature in step (3) is 60-120° C., and the particle size diameter of the sieved finished product is 0.1-2.5 mm.
Citation Information
Patent Citations
Preparation method of granular lithium adsorbent
CN109225124A
Synthesis process of lithium salt adsorbent precursor
CN114618440A
Mesoporous aluminum-based lithium adsorbent as well as preparation method and application thereof
CN116272843A
Preparation method of lithium adsorbent particles
CN117718002A
Preparation method, application and device of aluminum salt lithium ion adsorbent
CN117999120A